Preparation method of modified SmFeN powder and modified SmFeN powder

Modified SmFeN powder was prepared through hydrogen reduction diffusion method and jet mill crushing, combined with ball milling technology, which solved the problem of Ca residue, improved the density and magnetic properties of the powder, simplified the process and reduced energy consumption.

CN118762920APending Publication Date: 2024-10-11HENGDIAN GRP DMEGC MAGNETICS CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411093277.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

There is Ca residue in the existing SmFeN powder preparation method, which affects its intrinsic coercive force. The process is complex, energy consumption is high, and the product structure is complex.

Method used

The samarium iron alloy is prepared by hydrogen reduction and diffusion method, and is crushed by jet mill in an ammonia atmosphere. Then the coating agent and dispersant are mixed with SmFeN powder for ball milling to obtain modified SmFeN powder to avoid the participation and residue of Ca element.

Benefits of technology

The preparation of SmFeN powder without Ca residue is achieved, the density and magnetic properties of the powder are improved, the process complexity and energy consumption are reduced, and the safety and performance stability of the production process are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004987165690000101
    Figure BDA0004987165690000101
Patent Text Reader

Abstract

The invention discloses a preparation method of modified SmFeN powder and the modified SmFeN powder, belongs to the technical field of permanent magnet materials, and overcomes the defects that Ca residues exist in SmFeN prepared in the prior art, and the intrinsic coercive force of the SmFeN is influenced. The preparation method of the modified SmFeN powder provided by the invention comprises the following steps: step 1, taking Sm2O3 and Fe as raw materials, and reacting in an H2 atmosphere to prepare a samarium-iron alloy; the preparation method comprises the following steps of 1, preparing a samarium-iron alloy, 2, preparing SmFeN powder by adopting the prepared samarium-iron alloy, and 3, mixing a coating agent, a dispersing agent and the SmFeN powder, and carrying out ball milling to prepare the modified SmFeN powder. According to the method disclosed by the invention, Ca element is not introduced, and adverse effects on the intrinsic coercive force of SmFeN are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of permanent magnetic materials, and particularly relates to a preparation method of modified SmFeN powder and the modified SmFeN powder. Background Art

[0002] Permanent magnetic materials are one of the core functional raw materials for household appliances, automotive motors, computers, etc. Rare earth permanent magnets are widely used in many fields such as automobiles, wind power, electronics, aviation, etc., and with the rapid development of green industries, the global demand for rare earth permanent magnetic materials has increased rapidly. SmFeN has the huge advantages of high saturation magnetic polarization intensity, high Curie temperature (nearly 160℃ higher than NdFeB), high magnetic anisotropy field, and low cost, and is superior to NdFeB in oxidation resistance and corrosion resistance. Since its advent, SmFeN permanent magnetic materials have been valued by people for their excellent magnetic properties and good temperature stability. It is a permanent magnet material that may surpass NdFeB in performance. SmFeN is the most valuable permanent magnetic material for research after NdFeB due to its high Curie temperature, good temperature and chemical properties, and low price. In terms of physical and chemical properties, SmFeN has higher corrosion resistance, oxidation resistance, high temperature resistance and other characteristics than NdFeB. It has important application value and broad market prospects in various extreme environmental conditions, especially in the automotive industry, consumer electronics, aerospace and other fields. In terms of price, samarium and iron raw materials are abundant and cheap, and have a good raw material cost advantage compared to neodymium iron boron.

[0003] Among the methods for preparing SmFeN, the rapid quenching method, powder metallurgy method, and hydrogen crushing method are complex, have long cycles, high energy consumption, and are difficult to produce industrially. The powder material structure obtained by the high-energy ball milling method is disordered, and the powder contains many impurities in addition to the SmFeN phase.

[0004] The conventional reduction diffusion method for preparing SmFeN uses metal Ca or calcium compounds such as CaH2, CaCl2, etc. to mix with cheap metal oxides or metal chloride raw materials and metal raw materials such as Fe. Under high-temperature Ar or N2 atmosphere, the strong reducing property of metal Ca or CaH2 is used to cause a redox reaction with the metal oxide to generate the required SmFeN powder. Compared with the high-energy ball milling method, the reduction diffusion method obtains relatively less SmFeN impurities, but due to the production process, the products obtained are all in block form and contain Ca element compounds and residual Ca, which affects the intrinsic coercivity of SmFeN. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present invention is to overcome the defect that the SmFeN prepared in the prior art has Ca residue, which affects the intrinsic coercivity of SmFeN, thereby providing a preparation method of modified SmFeN powder and modified SmFeN powder.

[0006] To this end, the present invention provides the following technical solutions.

[0007] In a first aspect, the present invention provides a method for preparing a modified SmFeN powder, comprising:

[0008] Step 1, using Sm2O3 and Fe as raw materials, reacting in a H2 atmosphere to prepare a samarium-iron alloy;

[0009] Step 2, preparing SmFeN powder using the prepared samarium-iron alloy;

[0010] Step 3: Mix the coating agent, dispersant and SmFeN powder and perform ball milling to obtain modified SmFeN powder.

[0011] Furthermore, in step 1, the reaction gas pressure is 5-10 kPa, the reaction temperature is 400-600° C., and the reaction time is 15-18 h.

[0012] Furthermore, step 1 satisfies at least one of the following conditions:

[0013] (1) The molar ratio of Sm element to Fe element in the Sm2O3 and Fe is (2-2.4):17;

[0014] (2) The Sm2O3 is in powder form, and optionally, the particle size of the Sm2O3 powder is 0.1 to 0.5 μm;

[0015] (3) Fe is in powder form, and the particle size of the iron powder is optionally 20 to 50 μm.

[0016] Furthermore, the step 2 comprises: crushing the samarium iron alloy by jet milling in an ammonia atmosphere to obtain SmFeN powder.

[0017] Furthermore, in step 2, the rotation speed of the air jet mill is 30 to 300 r / min, preferably 80 to 200 r / min.

[0018] Furthermore, step 2 satisfies at least one of the following conditions:

[0019] (1) The purity of the ammonia is above 99.9%;

[0020] (2) The particle size of the obtained SmFeN powder is 10 to 200 μm.

[0021] Furthermore, step 3 satisfies at least one of the following conditions:

[0022] (1) The mass of the dispersant is 0.05% to 1.5% of the mass of the SmFeN powder, preferably 0.1% to 1%;

[0023] (2) The mass of the coating agent is 0.3% to 7% of the mass of the SmFeN powder, preferably 0.5% to 5%.

[0024] Furthermore, step 3 satisfies at least one of the following conditions:

[0025] (1) The mass of the dispersant is 0.05% to 1.5% of the mass of the SmFeN powder, preferably 0.1% to 1%;

[0026] (2) The mass of the coating agent is 0.3% to 7% of the mass of the SmFeN powder, preferably 0.5% to 5%;

[0027] (3) The frequency of the ball milling is 0.5 to 5 Hz, preferably 1 to 3 Hz;

[0028] (4) The ball milling time is 2 to 40 hours, preferably 5 to 30 hours;

[0029] (5) The ball-to-material ratio in ball milling is 30,000:(100-5,000), preferably 30,000:(1,000-2,000).

[0030] Ball-to-material ratio = the mass ratio of the grinding body (such as zirconium balls) to the SmFeN powder in the ball mill.

[0031] Furthermore, step 3 satisfies at least one of the following conditions:

[0032] (1) The dispersant includes one or more of WAX2100 synthetic wax and sodium oleate;

[0033] (2) The coating agent comprises phosphate and / or pyrophosphate;

[0034] Optionally, the phosphate includes one or more of zinc dihydrogen phosphate and potassium dihydrogen phosphate;

[0035] Optionally, the pyrophosphate comprises sodium pyrophosphate;

[0036] (3) The medium of the ball milling is aqueous ammonia;

[0037] (4) Use zirconium balls for ball milling.

[0038] In a second aspect, the present invention provides a modified SmFeN powder prepared according to the preparation method of the modified SmFeN powder.

[0039] The coating agent used in the present invention has good solubility in water and is easily hydrolyzed into orthophosphate in water. Ferrous ions and samarium ions remain in the SmFeN powder, and phosphate ions can react with ferrous ions in water to form positively charged colloids. The colloid particles are deposited toward the cathode to form a film and are tightly bound to the metal surface.

[0040] As a dispersant, WAX2100 synthetic wax can disperse the colloid formed by phosphate, ferrous ions, calcium ions (trace impurities in the raw iron powder) and SmFeN powder in water without precipitation. At the same time, WAX2100 synthetic wax is easily soluble in water, but insoluble in organic solvents such as ethanol and acetone. Due to the electrostatic repulsion, the carboxyl groups on its molecular chain stretch the twisted polymer chain, which promotes the exposure of the adsorptive functional groups on the surface. Since these active points are adsorbed on the colloidal particles and the metal powder, a bridge is formed between the colloidal particles and the metal powder, thereby accelerating the coating of the colloidal particles, killing two birds with one stone.

[0041] Ammonia water is used as the ball milling medium. The coating agent used in the present invention, such as potassium dihydrogen phosphate, has an ionization constant greater than the hydrolysis constant, and the concentration of hydrogen ions in water environment is greater than the concentration of hydroxide ions. It is weakly acidic when dissolved in water, and the reaction of phosphate ions with ferrous ions and samarium ions is best carried out in a neutral or alkaline environment. Using ammonia water as the ball milling medium can avoid the presence of hydrogen ions affecting the formation of colloidal particles, and ultimately affecting the formation of the coating film.

[0042] The technical solution of the present invention has the following advantages:

[0043] 1. The preparation method of the modified SmFeN powder provided by the present invention comprises: step 1, using Sm2O3 and Fe as raw materials, reacting in a H2 atmosphere to obtain a samarium-iron alloy; step 2, using the obtained samarium-iron alloy to prepare SmFeN powder; step 3, mixing a coating agent, a dispersant and the SmFeN powder and ball milling them to obtain a modified SmFeN powder.

[0044] The invention uses a hydrogen reduction diffusion method to prepare a samarium-iron alloy, using Sm2O3 and Fe as raw materials, utilizing the strong reducing property of H2, and reducing the pure samarium and pure iron to form a samarium-iron alloy through adsorption and diffusion at the reduction temperature, that is, the reduced Sm is adsorbed on the surface of the surrounding Fe powder particles in the form of gas, and then diffuses into the inside of the iron particles, and finally forms a uniform and stable samarium-iron alloy. The method of the invention does not introduce the Ca element, and will not have an adverse effect on the remanence and intrinsic coercivity of SmFeN.

[0045] During the ball milling process, the dispersant inhibits the agglomeration of the samarium iron alloy powder. While the ball mill is crushing, the SmFeN powder is coated to form a dense protective film to reduce the activity of the powder, and then it is dried, that is, a dense protective film is formed before the drying process, which can not only ensure the performance of the material, but also ensure the safety of the production process.

[0046] 2. Step 2 of the present invention includes: crushing the samarium iron alloy by jet milling in an ammonia or nitrogen atmosphere to obtain SmFeN powder. The present invention performs nitriding while crushing. The crushed samarium iron alloy powder is more active and easier to nitridize. Nitrogen atoms are more likely to combine with the samarium iron alloy, and the nitriding effect is better.

[0047] 3. The speed of the jet mill is 80-200 r / min. The SmFeN powder before coating is relatively active. If the powder obtained by the jet mill is fine, the powder is very easy to oxidize. The invention controls the speed of the jet mill at a lower speed to avoid the SmFeN powder being too fine. DETAILED DESCRIPTION

[0048] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0049] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0050] A method for preparing modified SmFeN powder comprises the following steps:

[0051] (1) Preparation of samarium iron alloy by hydrogen reduction diffusion method:

[0052] Samarium oxide powder and iron powder are mixed, vacuumed and filled with hydrogen to 5-10 kPa, heated to 400-600°C, and reacted for 15-18 hours to obtain a samarium-iron alloy.

[0053] (2) Preparation of SmFeN powder:

[0054] The samarium iron alloy obtained in (1) is preliminarily crushed in a jet mill at room temperature to obtain SmFeN powder with a particle size of 10 to 200 μm. The jet mill rotates at 80 to 200 r / min and the jet mill medium is ammonia gas with a purity of 99.9%.

[0055] (3) Coating the SmFeN powder to obtain modified SmFeN powder:

[0056] The SmFeN powder obtained in (2) is poured into a ball mill equipped with zirconium balls, and an appropriate amount of ammonia water (mass concentration 25%) is poured in so that the ammonia water level is 5 cm higher than the zirconium balls. Then, a dispersant and a coating agent are added, and the ball milling is performed at a frequency of 1 to 3 Hz for 5 to 30 hours. The dispersant is 0.1% to 1% of the mass of the SmFeN powder, and the coating agent is 0.5% to 5% of the mass of the SmFeN powder.

[0057] For example, ng (100≤n≤5000, more preferably 1000≤n≤2000) is poured into a ball mill equipped with 30KG zirconium balls. An appropriate amount of ammonia water is poured in so that the ammonia water level is 5 cm higher than the zirconium balls, and then WAX2100 synthetic wax and zinc dihydrogen phosphate are added.

[0058] (4) The slurry after ball milling in (3) was separated into solid and liquid, and the solid product was dried in a vacuum drying oven at a temperature of 75° C. for 3 h.

[0059] The dried powder is stored under nitrogen atmosphere at normal temperature and pressure for future use.

[0060] Example 1

[0061] This embodiment provides a method for preparing modified SmFeN powder, comprising the following steps:

[0062] (1) Preparation of samarium iron alloy by hydrogen reduction diffusion method:

[0063] 1.39 kg of samarium oxide powder with a particle size of 0.5 μm and 3.8 kg of metallic iron powder with a particle size of 37 μm were weighed and mixed. After evacuation, hydrogen was filled in to 8 kPa, the temperature was raised to 500°C, and the reaction was carried out for 16 hours to obtain a bulk samarium-iron alloy.

[0064] (2) Preparation of SmFeN powder:

[0065] The samarium iron alloy obtained in step (1) is preliminarily crushed in a jet mill at a speed of 150 r / min and the jet mill medium is ammonia gas with a purity of 99.9%, to obtain SmFeN powder with an average particle size of 25 μm.

[0066] (3) Coating SmFeN powder:

[0067] 1.5 kg of the SmFeN powder obtained in step (2) was poured into a ball mill equipped with 30 kg of zirconium balls, and an appropriate amount of ammonia water (25%) was added so that the ammonia water level was 5 cm above the zirconium balls. Then, 7.5 g of WAX2100 synthetic wax and 45 g of zinc dihydrogen phosphate were added, with the WAX2100 synthetic wax accounting for 0.5% of the mass of the SmFeN powder and the zinc dihydrogen phosphate accounting for 3% of the mass of the SmFeN powder. The mixture was ball milled at a frequency of 2 Hz for 20 hours.

[0068] (4) The slurry after ball milling in step (3) was separated into solid and liquid, and the solid product was dried in a vacuum drying oven at a temperature of 75° C. for 3 h.

[0069] The dried powder is stored under nitrogen atmosphere at normal temperature and pressure for future use.

[0070] Example 2

[0071] This embodiment provides a method for preparing modified SmFeN powder, which is basically the same as that of Embodiment 1, except that 800 g of SmFeN powder is poured into a ball mill for ball milling after air flow milling, WAX2100 synthetic wax is 0.5% of the mass of the SmFeN powder, and zinc dihydrogen phosphate is 3% of the mass of the SmFeN powder.

[0072] Example 3

[0073] This embodiment provides a method for preparing modified SmFeN powder, which is basically the same as that of Embodiment 1, except that 3000 g of SmFeN powder is poured into a ball mill for ball milling after air flow milling, WAX2100 synthetic wax is 0.5% of the mass of the SmFeN powder, and zinc dihydrogen phosphate is 3% of the mass of the SmFeN powder.

[0074] Example 4

[0075] This embodiment provides a method for preparing modified SmFeN powder, which is basically the same as that of Embodiment 1, except that the speed of the jet mill is set to 50 r / min.

[0076] Example 5

[0077] This embodiment provides a method for preparing modified SmFeN powder, which is basically the same as that of Embodiment 1, except that the speed of the jet mill is set to 300 r / min.

[0078] Example 6

[0079] This embodiment provides a method for preparing modified SmFeN powder, which is basically the same as that of Embodiment 1, except that 5 g of zinc dihydrogen phosphate is added during ball milling.

[0080] Example 7

[0081] This embodiment provides a method for preparing modified SmFeN powder, which is basically the same as that of Embodiment 1, except that 100 g of zinc dihydrogen phosphate is added during ball milling.

[0082] Example 8

[0083] This embodiment provides a method for preparing modified SmFeN powder, which is basically the same as that of Embodiment 1, except that 1 g of WAX2100 synthetic wax is added during ball milling.

[0084] Example 9

[0085] This embodiment provides a method for preparing modified SmFeN powder, which is basically the same as that of Embodiment 1, except that 20 g of WAX2100 synthetic wax is added during ball milling.

[0086] Example 10

[0087] This embodiment provides a method for preparing modified SmFeN powder, which is basically the same as that of Embodiment 1, except that 7.5 g of potassium dihydrogen phosphate is added during ball milling.

[0088] Embodiment 11

[0089] This embodiment provides a method for preparing modified SmFeN powder, which is basically the same as that of Embodiment 1, except that 7.5 g of sodium pyrophosphate is added during ball milling.

[0090] Example 12

[0091] This embodiment provides a method for preparing modified SmFeN powder, which is basically the same as that of Embodiment 1, except that 2.5 g of zinc dihydrogen phosphate, 2.5 g of potassium dihydrogen phosphate, and 2.5 g of sodium pyrophosphate are added during ball milling.

[0092] Example 13

[0093] This embodiment provides a method for preparing modified SmFeN powder, which is basically the same as that of Embodiment 1, except that the ball milling frequency is 0.5 Hz.

[0094] Embodiment 14

[0095] This embodiment provides a method for preparing modified SmFeN powder, which is basically the same as that of Embodiment 1, except that the ball milling frequency is 5 Hz.

[0096] Embodiment 15

[0097] This embodiment provides a method for preparing modified SmFeN powder, which is basically the same as that of Embodiment 1, except that the ball milling time is 2 h.

[0098] Example 16

[0099] This embodiment provides a method for preparing modified SmFeN powder, which is basically the same as that of Embodiment 1, except that the ball milling time is 40 h.

[0100] Embodiment 17

[0101] This embodiment provides a method for preparing modified SmFeN powder, comprising the following steps:

[0102] (1) Preparation of samarium iron alloy by hydrogen reduction diffusion method:

[0103] 1.39 kg of samarium oxide powder with a particle size of 0.1 μm and 3.8 kg of metallic iron powder with a particle size of 37 μm were mixed, evacuated and filled with 8 kPa of hydrogen, heated to 400°C, reacted for 15 hours, and obtained a bulk samarium-iron alloy.

[0104] (2) Preparation of SmFeN powder:

[0105] The samarium iron alloy obtained in step (1) is preliminarily crushed in a jet mill, the speed of the jet mill is 80 r / min, and the medium of the jet mill is ammonia gas with a purity of 99.9%.

[0106] (3) Coating SmFeN powder:

[0107] 1 kg of SmFeN powder obtained in step (2) was poured into a ball mill equipped with 30 kg of zirconium balls, and an appropriate amount of ammonia water (25%) was added so that the ammonia water level was 5 cm higher than the zirconium balls. Then 1 g of WAX2100 synthetic wax and 5 g of zinc dihydrogen phosphate were added, with the WAX2100 synthetic wax accounting for 0.1% of the mass of the SmFeN powder and the zinc dihydrogen phosphate accounting for 0.5% of the mass of the SmFeN powder. The mixture was ball milled at a frequency of 1 Hz for 5 hours.

[0108] (4) The slurry after ball milling in step (3) was separated into solid and liquid, and the solid product was dried in a vacuum drying oven at a temperature of 75° C. for 3 h.

[0109] The dried powder is stored under nitrogen atmosphere at normal temperature and pressure for future use.

[0110] Embodiment 18

[0111] This embodiment provides a method for preparing modified SmFeN powder, comprising the following steps:

[0112] (1) Preparation of samarium iron alloy by hydrogen reduction diffusion method:

[0113] 1.66 kg of samarium oxide powder with a particle size of 0.5 μm and 3.8 kg of metal iron powder with a particle size of 37 μm were mixed, evacuated and filled with 8 kPa of hydrogen, heated to 600°C, reacted for 18 hours, and obtained a bulk samarium-iron alloy.

[0114] (2) Preparation of SmFeN powder:

[0115] The samarium iron alloy obtained in step (1) is preliminarily crushed in a jet mill, the speed of the jet mill is 200 r / min, and the medium of the jet mill is ammonia gas with a purity of 99.9%.

[0116] (3) Coating SmFeN powder:

[0117] 2 kg of SmFeN powder prepared in step (2) was poured into a ball mill equipped with 30 kg of zirconium balls, and an appropriate amount of ammonia water (25%) was added so that the ammonia water level was 5 cm higher than the zirconium balls. Then 20 g of WAX2100 synthetic wax and 100 g of zinc dihydrogen phosphate were added, with the WAX2100 synthetic wax accounting for 1% of the mass of the SmFeN powder and the zinc dihydrogen phosphate accounting for 5% of the mass of the SmFeN powder. The mixture was ball milled at a frequency of 3 Hz for 30 hours.

[0118] (4) The slurry after ball milling in step (3) was separated into solid and liquid, and the solid product was dried in a vacuum drying oven at a temperature of 75° C. for 3 h.

[0119] The dried powder is stored under nitrogen atmosphere at normal temperature and pressure for future use.

[0120] Comparative Example 1

[0121] This comparative example provides a method for preparing SmFeN powder, which is basically the same as Example 1, except that no coating agent is added during ball milling.

[0122] Comparative Example 2

[0123] This comparative example is basically the same as Example 1, except that step (1) comprises: weighing 1.39 kg of samarium oxide powder with a particle size of 0.5 μm, 3.8 kg of metal iron powder with a particle size of 37 μm and 479 g of metal calcium with an average particle size of 200 μm, mixing, evacuating and then filling with argon to 5 kPa, heating to 500°C, reacting for 16 hours, and obtaining a bulk samarium-iron alloy.

[0124] Comparative Example 3

[0125] This comparative example provides a method for preparing modified SmFeN powder, which is basically the same as Example 1, except that no dispersant is added during ball milling.

[0126] Test example

[0127] The performance of the modified SmFeN powder after drying of each embodiment and comparative example was tested: the powder D50 was measured using a laser particle size distribution instrument, gas analysis was performed using an ONH-2000 oxygen, nitrogen and hydrogen analyzer to obtain the content of N and O elements in the powder, the thickness of the surface coated phosphating film was tested using a SEM scanning electron microscope, the content of the metal element (calcium in the present invention) in the powder was obtained by fluorescence testing, and the intrinsic coercive force was obtained using a NIM-2000 tester.

[0128] The oxygen content characterizes the degree of oxidation, the nitrogen content characterizes the nitriding effect of the modified SmFeN powder itself, D50 characterizes the particle size of the modified SmFeN powder, the SEM electron microscope can obtain the average thickness of the coating film, and the intrinsic coercive force characterizes the magnetic properties of the modified SmFeN powder.

[0129] The test results are shown in Table 1.

[0130] Table 1 Performance parameters of modified SmFeN powder

[0131]

[0132] From Table 1, we can draw the following conclusions:

[0133] (1) The SmFeN powder obtained by the method provided in Example 1 of the present invention has an oxygen content of 0.88%, a nitrogen content of 3.36%, a powder particle size D50 of 1.32 μm, an average thickness of the coating film of 0.26 μm, a low degree of powder oxidation, no explosion occurs during the preparation process, and an intrinsic coercive force of the SmFeN powder of 16.73 KOe. This shows that the preparation method of the present invention ensures the activity and magnetism of the product, while the coating of zinc dihydrogen phosphate effectively improves the safety.

[0134] (2) By comparing Example 1 with Examples 2-3, it can be seen that when the mass of the zirconium ball is constant, the mass of the SmFeN powder added during ball milling will greatly affect the powder particle size. The particle size of the SmFeN powder has a greater impact on the magnetic properties. The larger the powder particle size, the lower the magnetic properties. The smaller the powder particle size, the higher the magnetic properties. However, a small powder particle size will cause the powder to be easily oxidized, which will reduce the magnetic properties.

[0135] (3) By comparing Example 1 with Examples 4-5, it can be seen that when the mass of the zirconium ball and the mass of the powder during ball milling are constant, the rotation speed of the air flow mill will affect the initial particle size of the powder before ball milling and thus affect the magnetic properties. In addition, the rotation speed will affect the nitridation efficiency of the samarium iron alloy during ammonia air flow milling and affect the nitrogen content of the final SmFeN powder.

[0136] (4) By comparing Example 1 with Examples 6-7, it can be seen that the amount of coating agent added during ball milling affects the particle size of the SmFeN powder. When the coating agent content is too low, the average thickness of the coating film is lower than the normal level, making the powder easily oxidized and resulting in reduced performance. When the coating agent content is too high, the particle size of the SmFeN powder becomes larger, thereby reducing the magnetic properties.

[0137] (5) By comparing Example 1 with Examples 8-9, it can be seen that the amount of dispersant added during ball milling will also affect the particle size of the SmFeN powder. Excessive dispersant will cause the particle size of the SmFeN powder to become larger, thereby reducing the performance. The dispersant promotes the coating of the coating agent. Insufficient dispersant will result in poor coating effect of the SmFeN powder, which is easy to oxidize and leads to reduced performance.

[0138] (6) By comparing Example 1 with Examples 13-14, it can be seen that when the air mill speed, steel ball mass, powder mass and added additives are constant, the ball milling frequency will also affect the powder particle size, ultimately leading to reduced powder performance.

[0139] (7) By comparing Example 1 with Examples 15-16, it can be seen that when the air mill speed, ball milling frequency, steel ball mass, powder mass and added additives are constant, the ball milling time will also affect the powder particle size, ultimately leading to reduced powder performance.

[0140] (8) From the comparison between Example 1 and Comparative Example 1, it can be seen that the uncoated SmFeN powder is very easy to oxidize and has very poor magnetic properties. Coating the SmFeN powder can reduce its activity, reduce oxidation, and improve the magnetic properties.

[0141] (9) From the comparison between Example 1 and Comparative Example 3, it can be seen that WAX2100 synthetic wax promotes the coating of zinc dihydrogen phosphate, and can better coat sodium polymetaphosphate on the surface of SmFeN powder, reduce its activity, reduce oxidation, and improve magnetic properties.

[0142] (10) Comparison between Example 1 and Comparative Example 2 shows that the samarium iron nitrogen powder obtained by calcium reduction is difficult to be finely ground by ball milling due to the presence of calcium oxide, and calcium hydroxide (generated when ammonia water is added during ball milling) as a soft magnetic phase will greatly affect the intrinsic coercivity of the powder.

[0143] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A method for preparing modified SmFeN powder, characterized in that: include: Step 1, using Sm2O3 and Fe as raw materials, reacting in a H2 atmosphere to prepare a samarium-iron alloy; Step 2, preparing SmFeN powder using the prepared samarium-iron alloy; Step 3: Mix the coating agent, dispersant and SmFeN powder and perform ball milling to obtain modified SmFeN powder.

2. The method for preparing modified SmFeN powder according to claim 1, characterized in that: In the step 1, the reaction gas pressure is 5-10 kPa, the reaction temperature is 400-600° C., and the reaction time is 15-18 h.

3. The method for preparing the modified SmFeN powder according to claim 1 or 2, characterized in that: The step 1 satisfies at least one of the following conditions: (1) The molar ratio of Sm element to Fe element in the Sm2O3 and Fe is (2-2.4):17; (2) The Sm2O3 is in powder form, and optionally, the particle size of the Sm2O3 powder is 0.1 to 0.5 μm; (3) Fe is in powder form, and the particle size of the iron powder is optionally 20 to 50 μm.

4. The method for preparing the modified SmFeN powder according to claim 1 or 2, characterized in that: The step 2 comprises: crushing the samarium iron alloy by jet milling in an ammonia atmosphere to obtain SmFeN powder.

5. The method for preparing modified SmFeN powder according to claim 4, characterized in that: In step 2, the rotation speed of the jet mill is 30 to 300 r / min, preferably 80 to 200 r / min.

6. The method for preparing modified SmFeN powder according to claim 4, characterized in that: The step 2 satisfies at least one of the following conditions: (1) The purity of the ammonia is above 99.9%; (2) The particle size of the obtained SmFeN powder is 10 to 200 μm.

7. The method for preparing modified SmFeN powder according to claim 1, characterized in that: The step 3 satisfies at least one of the following conditions: (1) The mass of the dispersant is 0.05% to 1.5% of the mass of the SmFeN powder, preferably 0.1% to 1%; (2) The mass of the coating agent is 0.3% to 7% of the mass of the SmFeN powder, preferably 0.5% to 5%.

8. The method for preparing modified SmFeN powder according to claim 1 or 7, characterized in that: The step 3 satisfies at least one of the following conditions: (1) The mass of the dispersant is 0.05% to 1.5% of the mass of the SmFeN powder, preferably 0.1% to 1%; (2) The mass of the coating agent is 0.3% to 7% of the mass of the SmFeN powder, preferably 0.5% to 5%; (3) The frequency of the ball milling is 0.5 to 5 Hz, preferably 1 to 3 Hz; (4) The ball milling time is 2 to 40 hours, preferably 5 to 30 hours; (5) The ball-to-material ratio in ball milling is 30,000:(100-5,000), preferably 30,000:(1,000-2,000).

9. The method for preparing modified SmFeN powder according to claim 1 or 7, characterized in that: The step 3 satisfies at least one of the following conditions: (1) The dispersant includes one or more of WAX2100 synthetic wax and sodium oleate; (2) The coating agent comprises phosphate and / or pyrophosphate; Optionally, the phosphate includes one or more of zinc dihydrogen phosphate and potassium dihydrogen phosphate; Optionally, the pyrophosphate comprises sodium pyrophosphate; (3) The medium of the ball milling is aqueous ammonia; (4) Use zirconium balls for ball milling.

10. A modified SmFeN powder obtained according to the method for preparing modified SmFeN powder according to any one of claims 1 to 9.

Citation Information

Cited By