Porous carbon material as well as preparation method and application thereof

Porous carbon materials are directly prepared through the coordination reaction of gallic acid and magnesium salt in ball milling equipment, which solves the problem of tedious impregnation process, achieves efficient and low-cost preparation of porous carbon materials, and improves the energy storage density of supercapacitor electrodes.

CN118762938AInactive Publication Date: 2024-10-11LIANYUNGANG TECHN COLLEGE
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410781763.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing porous carbon material preparation methods require a cumbersome impregnation process, which affects material performance and production efficiency.

Method used

Gallic acid and magnesium salt are used to carry out coordination reaction in ball milling equipment, and after carbonization and dilute acid removal of magnesium components, porous carbon materials are directly produced, avoiding the impregnation step.

Benefits of technology

It achieves a simplified preparation process, reduces costs, and improves the performance of porous carbon materials, especially the energy storage density in supercapacitor electrodes, which is higher than commercial activated carbon electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118762938A_ABST
    Figure CN118762938A_ABST
Patent Text Reader

Abstract

The invention discloses a porous carbon material and a preparation method and application thereof, and belongs to the technical field of porous carbon materials.The preparation method comprises the steps that gallic acid and magnesium salt are weighed and placed in ball milling equipment; carrying out ball-milling mixing, and carrying out coordination reaction on gallic acid and magnesium salt in the ball-milling process; after the obtained complex is separated and taken out, carbonization treatment is carried out, and carbide is obtained; and removing the magnesium component in the carbide by using dilute acid, filtering, washing and drying to obtain the porous carbon material. The method does not need to use an organic solvent, does not need dipping treatment, has the advantages of simple steps, easiness in operation and low cost, and is easy for large-scale application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention mainly relates to the technical field of porous carbon materials, and specifically relates to a porous carbon material and a preparation method and application thereof. Background Art

[0002] As a new type of capacitor, electrochemical capacitors have the advantages of high energy density, high power density, long cycle life, no pollution to the environment, and wide operating temperature range compared to traditional capacitors. They are regarded as the most promising new green energy in this century. In the development of electrochemical capacitors, carbon materials play a very key role as electrode materials. Compared with other materials, carbon materials are low in price, rich in sources, and have sophisticated production processes. They are the most promising type of materials for large-scale commercial production and application.

[0003] The common methods for preparing porous carbon materials include template method and activation method. The former is to form pores through a rigid template with a specific morphology, and the latter is mainly to form pores through an activator such as ZnCl2, H3PO4, KOH. The template method usually requires the pre-preparation of a template with a specific morphology, and then the precursor is loaded onto the template for carbonization and the template is removed to obtain a porous carbon material. The activation method usually involves pre-carbonizing the precursor for preparing the carbon material, then loading the activator onto the pre-carbonized substrate, and then performing high-temperature carbonization, and using acid washing to remove the activator to obtain a porous carbon material.

[0004] It is not difficult to find that both the template method and the activation method require a tedious impregnation process. The effective contact degree between the precursor and the template or the precursor and the activator after impregnation has a great influence on the structure and surface area of ​​the obtained material, and thus has a great influence on the performance of the obtained carbon material. Therefore, it is necessary to study a method for preparing porous carbon materials that does not require impregnation treatment. Summary of the invention

[0005] The technical solution of the present invention aims at the technical problem that the existing technical solutions are too single, and provides a solution that is significantly different from the existing technologies. It mainly provides a porous carbon material and its preparation method and application, which do not require impregnation treatment, so as to solve the technical problem of the complicated preparation process of the existing porous carbon material raised in the above background technology.

[0006] The technical solution adopted by the present invention to solve the above technical problems is:

[0007] A method for preparing a porous carbon material comprises the following steps:

[0008] S1. Weigh gallic acid and magnesium salt and place them in a ball mill;

[0009] S2, ball milling and mixing, during which gallic acid and magnesium salt undergo coordination reaction;

[0010] S3, separating and taking out the obtained complex, and then carbonizing it to obtain a carbide;

[0011] S4. Use dilute acid to remove the magnesium component in the carbide, and then filter, wash and dry it to obtain a porous carbon material.

[0012] Specifically, in step S1, the magnesium salt is at least one of magnesium acetate tetrahydrate, magnesium nitrate hexahydrate, and magnesium chloride hexahydrate.

[0013] Preferably, in step S1, the mass ratio of gallic acid to magnesium salt is 1:1 to 1:2.

[0014] Specifically, in step S2, the ball milling speed is 500 to 1200 revolutions per minute, and the ball milling time is 2 to 6 hours.

[0015] Furthermore, in step S2, the ball milling mixing is performed by intermittent ball milling, with a stop every 20 minutes.

[0016] Preferably, in step S3, the carbonization temperature is 700-900°C.

[0017] Preferably, in step S4, the concentration of the dilute acid is 0.2 mol / L to 1.0 mol / L, and the ratio of the dilute acid to the carbide is 10 mL: 1 g.

[0018] Specifically, in step S4, the magnesium component in the carbide is removed by using dilute acid. Specifically, the carbide is placed in a container, and then the dilute acid is added, and the mixture is stirred thoroughly. During the stirring process, the pH value of the system is detected.

[0019] The present invention provides a porous carbon material, and the porous carbon material is prepared by the above-mentioned preparation method.

[0020] The present invention also provides an application of the porous carbon material, wherein the porous carbon material is used to prepare electrodes of supercapacitors.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The present invention uses gallic acid and magnesium salt as raw materials, and is subjected to ball milling. During the ball milling process, magnesium ions can be partially dissolved in the crystal water of magnesium acetate to form free magnesium ions, which can be complexed with gallic acid. After the complex reaction occurs, volatile acetic acid is generated. As acetic acid volatilizes, the complex reaction is initiated until the reaction ends. The feasibility of preparing gallic acid and magnesium acetate complex by ball milling has been verified by experiments. The present invention does not need to use an organic solvent or perform an impregnation treatment to successfully prepare a porous carbon material.

[0023] (2) The present invention firstly performs ball milling on the raw material, and then performs carbonization treatment after ball milling to obtain carbide, and then uses dilute acid to remove the magnesium component in the carbide, and finally obtains the porous carbon material after filtering, washing and drying. The present invention has simple steps, is easy to operate, has low cost, and is easy to apply on a large scale.

[0024] (3) It was found through experiments that the porous carbon material prepared by the present invention is used as a supercapacitor electrode, and the energy density of the capacitor energy storage is as high as 18.7Wh / kg, which is higher than the energy density of commercial activated carbon electrodes (usually <10Wh / kg). Therefore, the porous carbon material prepared by the preparation method of the present invention has great advantages in making capacitor electrodes.

[0025] The present invention will be explained in detail below with reference to the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a scanning electron microscope image of a sample synthesized by ball milling in Example 1 of the present invention;

[0027] Figure 2 This is a transmission electron microscope image of a sample synthesized by ball milling in Example 1 of the present invention;

[0028] Figure 3 is an X-ray diffraction pattern of a complex of gallic acid and magnesium acetate prepared by ball milling and aqueous solution assembly in a specific embodiment;

[0029] Figure 4 The infrared spectra of the gallic acid and magnesium acetate complex prepared by ball milling and aqueous solution assembly and gallic acid in a specific embodiment;

[0030] Figure 5 This is a diagram showing the cyclic voltammetry analysis results of a sample prepared by ball milling in a specific implementation manner;

[0031] Figure 6 Capacitance diagram of samples prepared by ball milling at different carbonization temperatures as supercapacitor electrodes. DETAILED DESCRIPTION

[0032] To facilitate understanding of the present invention, the present invention will be described more comprehensively below with reference to the relevant drawings. Several embodiments of the present invention are given in the drawings, but the present invention can be implemented in different forms and is not limited to the embodiments described in the text. On the contrary, these embodiments are provided to make the content disclosed in the present invention more thorough and comprehensive.

[0033] Embodiment 1: A method for preparing a porous carbon material, comprising the following steps:

[0034] 1. Weigh 1.0 mol of gallic acid (solid powder state) and 1.0 mol of magnesium acetate tetrahydrate (solid powder state) and place them in a ball mill;

[0035] 2. Ball milling technology is used for ball milling mixing. The ball milling speed is 800 revolutions per minute. The ball milling time is 4 hours. The ball milling is performed in an intermittent manner, that is, it stops every 20 minutes. The cumulative ball milling time is 4 hours. During the ball milling process, gallic acid and magnesium acetate tetrahydrate undergo coordination reaction. The coordination reaction is carried out according to the following reaction equation:

[0036] Once the reaction equilibrium is initiated, the volatilization of acetic acid can drive the reaction;

[0037] 3. After ball milling, the obtained complex is separated (the product after ball milling will stick to the ball mill jar and the ball mill, just scrape it off) and carbonized at a carbonization temperature of 700°C;

[0038] 4. After carbonization, the magnesium component is removed by dilute acid, and the final sample is obtained after filtering, washing and drying, which is the porous carbon material; the concentration of the dilute acid is 0.2 mol / L, and the dilute acid can react with the magnesium component to generate soluble magnesium ions, thereby facilitating its removal. The specific operation is as follows:

[0039] Place the sample in a container, then add dilute acid (1 g sample corresponds to 10 mL of dilute acid), stir for 30 minutes, and test the pH value to find it is acidic (pH value is about 2.0); continue stirring for 12 hours, and continue to measure the pH of the system (pH value <5); then filter, wash, and dry.

[0040] The microstructure of the sample synthesized by the ball milling method was observed by electron microscope, and the following Figure 1 The scanning electron micrographs shown and Figure 2 Transmission electron micrograph shown.

[0041] pass Figure 1 and Figure 2 It can be seen that the sample material synthesized by the above ball milling method has a porous structure.

[0042] Embodiment 2: This embodiment differs from Embodiment 1 in that:

[0043] In this embodiment, the amount of gallic acid used is 1.0 mol, the magnesium salt is magnesium nitrate hexahydrate, and the amount of magnesium nitrate hexahydrate used is 1.2 mol;

[0044] In this embodiment, the ball milling speed is 500 revolutions per minute, and the ball milling time is 2 hours.

[0045] In this embodiment, the carbonization temperature is 800°C.

[0046] In this embodiment, the concentration of the dilute acid is 0.5 mol / L.

[0047] The rest is the same as the first embodiment.

[0048] Embodiment 3: This embodiment differs from Embodiment 1 in that:

[0049] In this embodiment, the amount of gallic acid used is 1.0 mol, the magnesium salt is magnesium chloride hexahydrate, and the amount of magnesium chloride hexahydrate used is 2.0 mol;

[0050] In this embodiment, the ball milling speed is 1200 revolutions per minute, and the ball milling time is 6 hours.

[0051] In this embodiment, the carbonization temperature is 900°C.

[0052] In this embodiment, the concentration of the dilute acid is 1.0 mol / L.

[0053] The rest is the same as the first embodiment.

[0054] The feasibility of preparing porous carbon materials by ball milling is verified by experiments below:

[0055] (1) Gallic acid and magnesium acetate complexes were prepared by ball milling and aqueous solution method, respectively.

[0056] (2) X-ray diffraction analysis was performed on the gallic acid and magnesium acetate complexes prepared by two different methods, and the following results were obtained: Figure 3 X-ray diffraction pattern shown.

[0057] Depend on Figure 3 It can be seen that the spectra of the samples obtained by the two methods are basically the same, indicating that the ball milling method can achieve the complexation of gallic acid and magnesium acetate, proving the feasibility of the scheme.

[0058] (3) Infrared spectroscopy analysis was performed on the gallic acid and magnesium acetate complexes prepared by two different methods and gallic acid, respectively, to obtain the following: Figure 4 Infrared spectrum shown.

[0059] Depend on Figure 4 It can be seen that the C curve shows that the infrared spectrum of pure gallic acid is between 3500 and 3400 cm -1 The two absorption peaks are attributed to the infrared absorption peaks of phenolic hydroxyl and carboxyl groups respectively; Curves A and B show the infrared spectra of the complex prepared by aqueous solution and the complex prepared by ball milling, respectively. Obviously, the infrared absorption peaks at 3500 and 3400 cm -1 The two absorption peaks disappeared, indicating that both aqueous solution complexation and ball milling complexation achieved the coordination of gallic acid and magnesium ions, which also proved the feasibility of this route.

[0060] The following is to verify the performance of the supercapacitor electrode made from the porous carbon material prepared by the ball milling method of the present invention:

[0061] (1) The porous carbon material sample prepared in Example 1 was tested by cyclic voltammetry. The results are as follows: Figure 5 shown.

[0062] Depend on Figure 5 It can be seen that the cyclic voltammetry curves of the porous carbon material prepared by the ball milling method used as supercapacitor electrodes at different scanning rates all show irregular rectangular shapes, indicating that the capacity of the material used as a supercapacitor electrode mainly comes from the contribution of the electrochemical double layer. The irregular rectangle indicates that there is also a Faraday capacitance contribution, indicating that the carbon material prepared by the ball milling method contains a large number of electroactive groups.

[0063] (2) Comparative analysis of the capacities of the samples prepared by ball milling as supercapacitor electrodes in Example 1, Example 2 and Example 3. The results are as follows: Figure 6 shown.

[0064] Depend on Figure 6 It can be seen that the carbon material prepared by ball milling using gallic acid and magnesium acetate tetrahydrate as precursors was used as a supercapacitor electrode to obtain the maximum storage capacity, up to 298F / g. At a high current density of 20A / g, the capacity was still as high as 176F / g, showing high rate performance.

[0065] Using the formula E = 1 / 7.2 CV 2 (C is the capacity, V is the supercapacitor voltage), through Figure 6 The energy density of supercapacitors can be calculated, and the energy density for supercapacitor energy storage is as high as 18.7Wh / kg, which is higher than the energy density of commercial activated carbon electrodes (usually <10Wh / kg).

[0066] The above is an exemplary description of the present invention in combination with the accompanying drawings. It is obvious that the specific implementation of the present invention is not limited to the above-mentioned method. As long as such non-substantial improvements are made by adopting the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.

Claims

1. A method for preparing a porous carbon material, characterized in that: The steps include: S1. Weigh gallic acid and magnesium salt and place them in a ball mill; S2, ball milling and mixing, during which gallic acid and magnesium salt undergo coordination reaction; S3, separating and taking out the obtained complex, and then carbonizing it to obtain a carbide; S4. Use dilute acid to remove the magnesium component in the carbide, and then filter, wash and dry it to obtain a porous carbon material.

2. The method for preparing a porous carbon material according to claim 1, characterized in that: In step S1, the magnesium salt is at least one of magnesium acetate tetrahydrate, magnesium nitrate hexahydrate, and magnesium chloride hexahydrate.

3. The method for preparing a porous carbon material according to claim 1, characterized in that: In step S1, the mass ratio of gallic acid to magnesium salt is 1:1 to 1:

2.

4. The method for preparing a porous carbon material according to claim 1, characterized in that: In step S2, the ball milling speed is 500 to 1200 revolutions per minute, and the ball milling time is 2 to 6 hours.

5. The method for preparing a porous carbon material according to claim 4, characterized in that: In step S2, the ball milling mixing is performed by intermittent ball milling, with a stop every 20 minutes.

6. The method for preparing a porous carbon material according to claim 1, characterized in that: In step S3, the carbonization temperature is 700-900°C.

7. The method for preparing a porous carbon material according to claim 1, characterized in that: In step S4, the concentration of the dilute acid is 0.2 mol / L to 1.0 mol / L, and the ratio of the dilute acid to the carbide is 10 mL: 1 g.

8. The method for preparing a porous carbon material according to claim 7, characterized in that: In step S4, the magnesium component in the carbide is removed by using dilute acid. Specifically, the carbide is placed in a container, and then the dilute acid is added, and the mixture is stirred thoroughly. During the stirring process, the pH value of the system is detected.

9. A porous carbon material, characterized in that: The porous carbon material is prepared by the preparation method according to any one of claims 1 to 8.

10. The use of the porous carbon material according to claim 9, characterized in that: The porous carbon material is used for making electrodes of supercapacitors.

Citation Information

Cited By

  • Porous carbon material with nanosheet shell-coated porous skeleton structure, preparation method and electrode of porous carbon material

    CN119774609A