Method for reducing SiO2 / 4H-SiC interface state density and application
Through low-temperature plasma treatment and high-temperature rapid annealing technology, the SiO2/4H-SiC interface state density is reduced, the problem of high interface state density in SiC MOSFET devices is solved, and the oxide layer breakdown field strength and gate withstand voltage performance of the device are improved. , enhanced reliability.
Patent Information
- Application Number
- CN202410868048.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-11
AI Technical Summary
The high density of states at the SiO2/4H-SiC interface limits the channel mobility and gate reliability of SiC MOSFET devices, and the existing annealing process is not ideal.
Low-temperature plasma treatment is used to use N2O plasma atmosphere to diffuse N and O elements to the SiO2/4H-SiC interface, and combined with high-temperature rapid annealing technology, O reacts with interface C to release CO, N passivates the dangling bonds, and P reduces the effective negative charge , reduce the interface state density.
Significantly reduces the SiO2/4H-SiC interface state density, improves the interface quality, increases the oxide layer breakdown field strength of SiC MOSFET devices, enhances the gate withstand voltage performance, reduces leakage current, and improves device reliability.
Smart Images

Figure CN118762993A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor manufacturing technology, and in particular to a method for reducing SiO2 / 4H-SiC interface state density and its application. Background Art
[0002] The third-generation semiconductor silicon carbide (SiC) has outstanding advantages such as wide bandgap, high saturation drift velocity, high thermal conductivity, and high critical breakdown electric field. SiC devices have the characteristics of high current density, high frequency, and low resistance. They can greatly reduce the size and weight of power electronic systems, achieve high temperature resistance, high frequency resistance, and low loss, and their application prospects are very broad.
[0003] However, in metal oxide semiconductor field effect transistors (MOSFETs), the density of SiO2 / SiC interface states is about two orders of magnitude higher than that of Si / SiO2 interface states in traditional silicon-based devices, which makes the channel mobility of SiC MOSFETs lower and limits the device characteristics of SiC MOSFETs. Therefore, the quality of the gate oxide structure directly affects the channel mobility and gate reliability.
[0004] At present, the annealing process after oxidation to form the SiO2 / SiC interface structure is an effective way to reduce the interface state density and optimize the interface characteristics of MOSFET. After the SiC gate oxide process adopts thermal oxidation growth, due to the defects in the interface state quality, a secondary annealing treatment is usually performed in an atmosphere containing nitrogen (N) atoms to improve the internal atomic structure of the gate oxide and reduce the performance defects caused by the dangling bonds of C atoms.
[0005] However, the interface state density obtained by the above processing method is still not ideal, and there is a large well space. Summary of the invention
[0006] In view of the deficiencies in the prior art, the object of the present invention is to provide a method and application for reducing the SiO2 / 4H-SiC interface state density.
[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0008] In a first aspect, the present invention provides a method for reducing the SiO2 / 4H-SiC interface state density, comprising:
[0009] Providing a SiO2 / 4H-SiC interface structure, wherein the SiO2 layer is formed by surface oxidation of the 4H-SiC layer;
[0010] Performing a low-temperature plasma treatment on the SiO2 / 4H-SiC interface structure, wherein the plasma atmosphere used in the low-temperature plasma treatment contains N2O, and the low-temperature plasma treatment causes N and O elements to diffuse to the interface between the SiO2 layer and the 4H-SiC layer;
[0011] Then, the SiO2 / 4H-SiC interface structure is subjected to high temperature rapid annealing treatment to obtain a SiO2 / 4H-SiC interface structure with low interface state density.
[0012] Furthermore, the plasma atmosphere also contains PH3 / Ar mixed gas.
[0013] Furthermore, the volume fraction of PH3 in the PH3 / Ar mixed gas is 5%-20%.
[0014] In a second aspect, the present invention further provides a specific application of the above processing method, such as a method for preparing a SiC MOSFET, comprising:
[0015] The 4H-SiC layer is subjected to surface oxidation treatment to form a SiO2 layer;
[0016] The above-mentioned treatment method is used to treat the formed SiO2 / 4H-SiC interface structure to reduce the interface state density of the SiO2 / 4H-SiC interface structure.
[0017] Based on the above technical solution, compared with the prior art, the beneficial effects of the present invention at least include:
[0018] The treatment method provided by the present invention adopts plasma low-temperature treatment technology to diffuse N and O plasma to the interface of the oxide layer, and then undergoes rapid high-temperature rapid annealing (RTP) technology, so that O can react with C on the interface and release in the form of CO, thereby reducing the density of C clusters, and at the same time, N plays a certain role in passivating dangling bonds, which is beneficial to improving the interface quality. P can reduce the effective negative charge of the interface, which has a promoting effect on reducing the trapped charge in the oxide layer near the interface.
[0019] The present invention can reduce the effective negative charge at the SiO2 / 4H-SiC interface, reduce the interface state density, improve the SiO2 / SiC interface quality, and further increase the oxide layer breakdown field strength of the prepared SiC MOSFET device, improve the voltage resistance of the gate, reduce the gate leakage current, and improve the device reliability.
[0020] The above description is only an overview of the technical solution of the present invention. In order to enable those skilled in the art to more clearly understand the technical means of the present application and implement them according to the contents of the specification, the following is a description of the preferred embodiments of the present invention in conjunction with detailed drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a flowchart of a processing method provided by a typical implementation case of the present invention. DETAILED DESCRIPTION
[0022] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The main purpose is to reduce the effective negative charge on the interface, reduce the interface state density, improve the quality of the SiO2 / SiC interface, and then increase the breakdown field strength of the oxide layer, improve the voltage resistance of the gate, and improve the reliability of the device. The technical solution, its implementation process and principle will be further explained below.
[0023] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0024] See also Figure 1 As shown, an embodiment of the present invention provides a method for reducing the SiO2 / 4H-SiC interface state density, which includes the following steps:
[0025] Providing a SiO2 / 4H-SiC interface structure, wherein the SiO2 layer is formed by surface oxidation of the 4H-SiC layer;
[0026] Performing a low-temperature plasma treatment on the SiO2 / 4H-SiC interface structure, wherein the plasma atmosphere used in the low-temperature plasma treatment comprises N2O, and the low-temperature plasma treatment causes N, O and P elements to diffuse to the interface between the SiO2 layer and the 4H-SiC layer;
[0027] Then, the SiO2 / 4H-SiC interface structure is subjected to high temperature rapid annealing treatment to obtain a SiO2 / 4H-SiC interface structure with low interface state density.
[0028] The key technical means of the present invention is to use plasma containing N2O for treatment, so that the N and O plasma therein diffuse to the oxide layer interface, and cooperate with high-temperature rapid annealing (RTP) technology, O can react with C on the interface to release in the form of CO, thereby reducing the density of C clusters, and at the same time N plays a certain role in passivating dangling bonds, which is beneficial to improving the interface quality, and P can reduce the effective negative charge of the interface, which promotes the reduction of trapped charges in the oxide layer near the interface, thereby significantly reducing the interface state density of the SiO2 / 4H-SiC interface structure.
[0029] Some prior art technologies propose to anneal the SiO2 / 4H-SiC interface structure to reduce its interface state density; other prior art technologies propose to perform plasma treatment (such as ammonia plasma) on the SiO2 / 4H-SiC interface structure to reduce its interface state density. However, the key technical means of the present invention is not a simple combination of the above two prior art technologies, and the principle used is also different from the above prior art technologies.
[0030] Specifically, the low-temperature plasma treatment of the present invention is not directly (or only) for reducing the interface state density, but its main purpose is to penetrate specific elements into the interface. These penetrated N, O and P elements can react at the interface only after subsequent high-temperature rapid annealing treatment, thereby removing C clusters and passivating dangling bonds, thereby significantly reducing the interface state density.
[0031] It is clear that the present invention not only involves the combination of plasma treatment and annealing treatment, but also in the present invention, the selection of plasma atmosphere and the order of plasma treatment and annealing treatment are also very critical. The lack of any one of the characteristics cannot achieve the above purpose, which is not involved in the above-mentioned prior art.
[0032] In addition, in some embodiments, the plasma atmosphere further comprises a PH3 / Ar mixed gas. Among them, Ar is used as a carrier gas for PH3. When PH3 is not introduced in some basic technical solutions, Ar may not be required as a carrier gas. In the technical solution of the present invention, adding PH3 has a better effect. This is because, after the synergistic treatment of the plasma formed by PH3, P can reduce the effective negative charge of the interface, which promotes the reduction of the trapped charge in the near-interface oxide layer. As for the specific ratio of each component, in some embodiments, the volume flow ratio of 10% PH3 / Ar mixed gas to N2O in the plasma atmosphere can preferably be set to (0.5-2): (5-10), but is not limited thereto.
[0033] The SiO2 / 4H-SiC interface structure targeted by the treatment method provided by the present invention may be a prepared inventory product, or may be a device directly prepared before the treatment method of the present invention. As for how to form the SiO2 / 4H-SiC interface structure, in some embodiments, the preparation method of the SiO2 / 4H-SiC interface structure may include the following process:
[0034] Performing oxidation treatment on the surface of the 4H-SiC layer to form the SiO2 layer;
[0035] The combination of the 4H-SiC layer and the SiO2 layer is subjected to in-situ annealing treatment to obtain the SiO2 / 4H-SiC interface structure.
[0036] In some specific embodiments, the oxidation treatment is dry oxidation in an oxygen-containing atmosphere at a temperature of 1000-1450°C for 30-360 min; the in-situ annealing treatment is carried out in a protective atmosphere at a temperature substantially similar to that during oxidation, for example, 1150-1400°C for 30-120 min.
[0037] Furthermore, in some embodiments, before the oxidation treatment, the surface of the 4H-SiC layer is subjected to an RCA cleaning treatment.
[0038] As for some specific treatment conditions, in some embodiments, the temperature of low-temperature plasma treatment is 150-500° C., and the treatment time is 1-60 min.
[0039] In some embodiments, the high temperature rapid annealing treatment is performed at a temperature of 900-1200° C. and a treatment time of 1-10 min.
[0040] In some embodiments, the annealing atmosphere of the high temperature rapid annealing treatment is N2 or a vacuum environment.
[0041] As some typical application examples of the above technical solution, a complete preparation process for forming a SiO2 / 4H-SiC interface structure with low interface state density may include the following steps:
[0042] S1: Provide 4H-SiC epitaxial wafer (or semi-finished device), perform RCA cleaning, and then spin dry;
[0043] S2: oxidizing the 4H-SiC epitaxial wafer with dry oxygen at high temperature to form SiO2, and then performing in-situ annealing;
[0044] S3: Plasma low temperature treatment;
[0045] S4: Perform high temperature rapid annealing (RTP) treatment.
[0046] In step S2, the high temperature dry oxygen oxidation is performed at a temperature of 1200-1450° C. for 30-360 min; in step S2, the in-situ annealing time is 30-120 min; in step S3, the gas used for plasma low temperature treatment includes PH3, Ar, and N2O; in step S3, the temperature range of plasma low temperature treatment is 150-500° C. for 1-60 min; in step S4, the temperature range of high temperature rapid annealing (RTP) treatment is 900-1200° C. for 1-10 min.
[0047] Finally, based on the above technical solution, in some embodiments, after treatment, the interface state density of the SiO2 / 4H-SiC interface structure is 1.5-2.0×10 12 eV-1·cm -2 (~0.2eV), the oxide layer defect charge density is 8.0-9.0×10 11 cm -2 .
[0048] A second aspect of an embodiment of the present invention further provides a specific application of the above processing method, such as a method for preparing a SiC MOSFET, which comprises the following steps:
[0049] The 4H-SiC layer is subjected to surface oxidation treatment to form a SiO2 layer;
[0050] The formed SiO2 / 4H-SiC interface structure is treated by the treatment method provided in any of the above-mentioned embodiments to reduce the interface state density of the SiO2 / 4H-SiC interface structure.
[0051] The technical solution of the present invention is further described in detail below through several embodiments and in conjunction with the accompanying drawings. However, the selected embodiments are only used to illustrate the present invention, and do not limit the scope of the present invention.
[0052] Example 1
[0053] S1: Provide SiC substrate, grow SiC epitaxial layer, form 4H-SiC epitaxial wafer, perform RCA cleaning, and then spin dry;
[0054] The RCA cleaning uses the following cleaning method:
[0055] ① Use H2SO4:H2O2=7:3 ratio solution to clean for 15 minutes, and rinse with deionized water;
[0056] ② Use a solution of NH4OH:H2O2:H2O=1:1:6 (70-80℃) to clean for 2 minutes, and then rinse with deionized water;
[0057] ③ Use a solution of HCl:H2O2:H2O=1:1:6 (70-80℃) to clean for 2 minutes, and then rinse with deionized water;
[0058] ④ Use HF:H20=1:50 solution or BOE (1:20) solution or BOE (1:7) solution to clean for 2 minutes, rinse with deionized water and dry.
[0059] S2: Dry-oxidize the 4H-SiC epitaxial wafer at high temperature to form a SiO2 layer, and then perform in-situ annealing; specifically, place the 4H-SiC epitaxial wafer in a high-temperature oxidation furnace for dry-oxidation to form a SiO2 layer, and then perform in-situ annealing in a N2 atmosphere, the oxidation temperature is 1200°C, and the oxidation time is 6 hours; the in-situ annealing gas atmosphere is N2, and the time is 1 hour.
[0060] S3: Plasma low temperature treatment is performed; the gas used in the plasma low temperature treatment technology is a 10% PH3 / Ar mixed gas, and the volume flow ratio of N2O is 1:10. The temperature of the plasma low temperature treatment technology is 350°C and the treatment time is 30 minutes.
[0061] S4: Perform high temperature rapid annealing (RTP) treatment, the temperature of the high temperature rapid annealing (RTP) technology is 1000° C., the processing time is 3 minutes, and the annealing gas atmosphere is N2.
[0062] The obtained SiO2 / 4H-SiC interface state density is 1.8×10 12 eV -1 cm -2 (N0.2eV), the oxide layer defect charge density is 9.0×10 11 cm -2 .
[0063] Comparative Example 1
[0064] This comparative example is substantially the same as Example 1, except that:
[0065] The processes of steps S3 and S4 are omitted.
[0066] The result is:
[0067] The obtained SiO2 / 4H-SiC interface state density is 6.8×10 12 eV -1 cm -2 (~0.2eV).
[0068] Comparative Example 2
[0069] This comparative example is substantially the same as Example 1, except that:
[0070] In step S3, H2 and N2 gas atmospheres are used.
[0071] The obtained SiO2 / 4H-SiC interface state density is 5.6×10 12 eV -1 cm -2 (~0.2eV).
[0072] Example 2
[0073] This embodiment is substantially the same as Embodiment 1, and the main difference is that:
[0074] In step S3, the PH3 / Ar mixed gas is not introduced, but replaced by additional N2O gas with an equal volume flow rate.
[0075] The obtained SiO2 / 4H-SiC interface state density is 1.85×10 12 eV -1 cm -2 (~0.2eV), the oxide layer defect charge density is 1.8×10 12 cm -2 .
[0076] Example 3
[0077] This embodiment is substantially the same as Embodiment 1, and the main difference is that:
[0078] S3: Plasma low temperature treatment is performed; the volume flow ratio of the gas 20% PH3 / Ar mixed gas and N2O used in the plasma low temperature treatment technology is 0.5:10, the temperature of the plasma low temperature treatment technology is 150°C, and the treatment time is 60 minutes.
[0079] S4: performing a high temperature rapid annealing (RTP) process, wherein the temperature of the high temperature rapid annealing (RTP) technology is 900° C. and the processing time is 10 minutes.
[0080] Example 4
[0081] This embodiment is substantially the same as Embodiment 1, and the main difference is that:
[0082] S3: Perform plasma low temperature treatment; the plasma low temperature treatment technology uses a 5% PH3 / Ar mixed gas and N2O with a volume flow ratio of 2:5, a temperature of 500°C, and a treatment time of 1 minute.
[0083] S4: performing a high temperature rapid annealing (RTP) process, wherein the temperature of the high temperature rapid annealing (RTP) technology is 1200° C. and the processing time is 1 minute.
[0084] The above-mentioned embodiments 3-4 can obtain interface state densities substantially similar to those of embodiment 1, and will not be described in detail here.
[0085] Based on the above embodiments and comparative examples, it can be clearly seen that the treatment method provided by the present invention, by adopting plasma low-temperature treatment technology, diffuses N and O plasma to the interface of the oxide layer, and then undergoes rapid high-temperature rapid annealing (RTP) technology, O can react with C on the interface to be released in the form of CO, thereby reducing the density of C clusters. At the same time, N plays a certain role in passivating dangling bonds, which is beneficial to improving the interface quality.
[0086] The present invention can reduce the effective negative charge at the SiO2 / 4H-SiC interface, reduce the interface state density, improve the SiO2 / SiC interface quality, and further increase the oxide layer breakdown field strength of the prepared SiC MOSFET device, improve the voltage resistance of the gate, reduce the gate leakage current, and improve the device reliability.
[0087] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for reducing the state density of SiO2 / 4H-SiC interface, characterized in that: include: Providing a SiO2 / 4H-SiC interface structure, wherein the SiO2 layer is formed by surface oxidation of the 4H-SiC layer; Performing a low-temperature plasma treatment on the SiO2 / 4H-SiC interface structure, wherein the plasma atmosphere used in the low-temperature plasma treatment contains N2O, and the low-temperature plasma treatment causes N and O elements to diffuse to the interface between the SiO2 layer and the 4H-SiC layer; Then, the SiO2 / 4H-SiC interface structure is subjected to high temperature rapid annealing treatment to obtain a SiO2 / 4H-SiC interface structure with low interface state density.
2. The processing method according to claim 1, characterized in that: The plasma atmosphere further comprises a PH3 / Ar mixed gas; The volume fraction of PH3 in the PH3 / Ar mixed gas is 5%-20%.
3. The processing method according to claim 2, characterized in that: The volume flow ratio of the PH3 / Ar mixed gas to N2O in the plasma atmosphere is (0.5-2):(5-10).
4. The processing method according to claim 1, characterized in that: The preparation method of the SiO2 / 4H-SiC interface structure comprises: Performing oxidation treatment on the surface of the 4H-SiC layer to form the SiO2 layer; The combination of the 4H-SiC layer and the SiO2 layer is subjected to in-situ annealing treatment to obtain the SiO2 / 4H-SiC interface structure.
5. The processing method according to claim 4, characterized in that: The oxidation treatment is dry oxidation in an oxygen-containing atmosphere at a temperature of 1000-1450° C. for 30-360 minutes; The in-situ annealing treatment is carried out in a protective atmosphere for 30-120 minutes.
6. The processing method according to claim 4, characterized in that: Before the oxidation treatment, the surface of the 4H-SiC layer is subjected to RCA cleaning treatment.
7. The processing method according to claim 1, characterized in that: The temperature of low temperature plasma treatment is 150-500°C, and the treatment time is 1-60min.
8. The processing method according to claim 1, characterized in that: The temperature of the high temperature rapid annealing treatment is 900-1200°C and the treatment time is 1-10min; And / or, the annealing atmosphere of the high temperature rapid annealing treatment is N2 or a vacuum environment.
9. The processing method according to claim 1, characterized in that: After treatment, the interface state density of the SiO2 / 4H-SiC interface structure is 1.5-2.0×10 12 eV- 1 cm- 2 (0.2eV), the oxide layer defect charge density is 8.0-9.0×10 11 cm- 2 .
10. A method for preparing a SiC MOSFET, characterized in that: include: The 4H-SiC layer is subjected to surface oxidation treatment to form a SiO2 layer; The formed SiO2 / 4H-SiC interface structure is treated by the treatment method described in any one of claims 1 to 9 to reduce the interface state density of the SiO2 / 4H-SiC interface structure.
Citation Information
Cited By
Production process for improving reliability of gate oxide layer of silicon carbide MOSFET device
CN121398099A