Method for forming semiconductor device
By forming multiple fins and dielectric fins on the substrate of the semiconductor device and adjusting the width of the gap area, the problem of gate deposition and replacement in the FinFET structure is solved, the integration density and performance are improved, and a more efficient manufacturing process.
Patent Information
- Application Number
- CN202410760052.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-06-13
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-11
AI Technical Summary
Existing semiconductor device manufacturing technology is difficult to effectively improve integration density and performance, especially when forming FinFET structures. It is difficult to optimize the gap area between fins to facilitate gate deposition and replacement.
The replacement gate structure is then formed by forming a plurality of fins and dielectric fins on a substrate and depositing silicon and oxide layers therebetween, adjusting the width of the gap region to facilitate deposition and subsequent removal of the dummy gate.
Achieving higher integration density and performance, improving FinFET efficiency and reliability, simplifying the process flow and reducing production costs.
Smart Images

Figure CN118762994A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for forming a semiconductor device. Background Art
[0002] Semiconductor devices are used in a variety of electronic applications, such as personal computers, cell phones, digital cameras, and other electronic devices. Semiconductor devices are typically manufactured by sequentially depositing insulating or dielectric layers, conductive layers, and semiconductor material layers over a semiconductor substrate and patterning the various material layers using lithography to form circuit components and elements thereon.
[0003] The semiconductor industry continues to increase the integration density of various electronic components (eg, transistors, diodes, resistors, capacitors, etc.) by continually reducing the minimum feature size, thereby allowing more components to be packed into a given area. Summary of the invention
[0004] According to one embodiment of the present disclosure, a method for forming a semiconductor device includes forming a plurality of fins above a substrate, the fins including a first semiconductor fin adjacent to an isolation region; and a dielectric fin embedded in the isolation region; depositing a silicon layer over a first surface of the first semiconductor fin, a second surface of the dielectric fin, and a third surface of the isolation region; forming an oxide layer over the silicon layer; removing a portion of the oxide layer and the silicon layer to expose the second surface of the dielectric fin; forming a dummy gate over a remaining portion of the oxide layer and between the fins; forming a first epitaxial region in the first semiconductor fin; and replacing the dummy gate with a gate structure.
[0005] According to an embodiment of the present disclosure, a method for forming a semiconductor device includes forming a plurality of first fins above a first region of a substrate, wherein the plurality of first fins include a silicon fin and a first dielectric fin; forming a plurality of second fins above a second region of the substrate, wherein the second fins include a silicon germanium fin and a second dielectric fin; forming a first isolation region and a second isolation region above the substrate, wherein the first isolation region is inserted between the silicon fin and the first dielectric fin, a first gap region is above the first insulating region and between the first fins, and a second gap region is above the second isolation region and between the second fins; A silicon layer is formed over the second fin, the second isolation region, and the second fin; an oxide layer is formed over the silicon layer, wherein the forming of the silicon layer and the forming of the oxide layer include reducing a first lateral width of the first gap region and a second lateral width of the second gap region; multiple portions of the oxide layer and the silicon layer are etched to expose the first dielectric fin and the second dielectric fin, wherein the etching of portions of the oxide layer and the silicon layer includes increasing a first lateral width of the first gap region and a second lateral width of the second gap region; a first gate structure is formed over the first fin and in the first gap region; and a second gate structure is formed over the second fin and in the second gap region.
[0006] According to one embodiment of the present disclosure, a method for forming a semiconductor device includes forming semiconductor fins and dielectric fins in an insulating material disposed above a substrate; recessing the insulating material to form an isolation region, the semiconductor fins and the dielectric fins protruding above an upper surface of the isolation region; depositing a silicon layer over a first surface of the semiconductor fin, a second surface of the dielectric fin, and an upper surface of the isolation region; depositing a dummy dielectric layer on the silicon-containing layer; removing portions of the dummy dielectric layer and the silicon layer from the second surface of the dielectric fin; and forming a dummy gate over the semiconductor fin and the dielectric fin, the dummy gate being in physical contact with the isolation region. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] The aspects of this disclosure are in the attached Figure 1 The following detailed description is best understood when read together. It should be noted that, in accordance with the standard practice in the industry, various features are not drawn to scale. In fact, the dimensions of the various features may be arbitrarily increased or reduced for clarity of discussion.
[0008] Figure 1 illustrates an example of a FinFET in a three-dimensional view according to some embodiments;
[0009] Figure 2 , Figure 3 , Figure 4 , Figure 5 , Figure 6 , Figure 7 , Figure 8 , Fig. 9 , Fig.10 , Fig.11 , Fig.12 , Fig.13 , Fig.14A , Fig. 14B , Fig.15A , Fig. 15B , Fig.16A , Fig. 16B , Fig. 16C , Fig.16D , Fig.17A , Fig. 17B , Fig. 17C , Fig.17D , Fig.18A , Fig.18B , Fig.19A , Fig.19B , Fig. 20A , Fig. 20B , Fig. 20C , Fig.21A , Fig. 21B , Fig. 21C , Fig.21D , Fig.22A , Fig. 22B , Fig.23A ,and Fig. 23Bis a cross-sectional view of an intermediate stage in fabricating a FinFET according to some embodiments.
[0010]
Explanation of symbols
[0011] 50:Substrate
[0012] 50N: n-type region
[0013] 50P: p-type region
[0014] 52: Fins
[0015] 52A: Fins
[0016] 52B: Fins
[0017] 54: Insulation material
[0018] 56:STI area
[0019] 56P:Part
[0020] 58: Channel Area
[0021] 60: dummy dielectric layer
[0022] 62: Virtual gate layer
[0023] 64: Mask layer
[0024] 72: dummy gate
[0025] 74:Mask
[0026] 80: Gate sealing spacer
[0027] 82: epitaxial source / drain region
[0028] 86: Gate spacer
[0029] 87:CESL
[0030] 88: First ILD
[0031] 89: District
[0032] 90: Groove
[0033] 92: Gate dielectric layer
[0034] 94: Gate electrode
[0035] 94A: Lining layer
[0036] 94B: Work function tuning layer
[0037] 94C: Filling material
[0038] 96: Gate mask
[0039] 108: Second ILD
[0040] 110: Gate contact
[0041] 112: Source / drain contact
[0042] 202: Mask
[0043] 210: Dielectric fins
[0044] 220: Gap Zone
[0045] 232: Silicon layer
[0046] 240: Mask layer
[0047] 244: Gate isolation region
[0048] D1~D3: Distance
[0049] D N :distance
[0050] G1: First gap
[0051] G2: Second gap
[0052] G3: The third gap
[0053] G4: The fourth gap
[0054] G5: The fifth gap
[0055] G6: Sixth Gap
[0056] G A : Gap G1, G2
[0057] G B : Gap G3, G4
[0058] G C : Gap G5, G6
[0059] W1~W3: Width
[0060] W A :Width W1, W2, W3
[0061] W N :width DETAILED DESCRIPTION
[0062] The following disclosure provides many different embodiments, or examples, for implementing the different features of the present disclosure. Specific examples of components and configurations are described below to simplify the present disclosure. Of course, these are only examples and are not intended to be restrictive. For example, in the following description, the formation of a first feature above or on a second feature may include an embodiment in which the first feature is formed in direct contact with the second feature, and may also include an embodiment in which an additional feature may be formed between the first feature and the second feature so that the first feature and the second feature may not be in direct contact. In addition, the present disclosure may repeat reference numbers and / or letters in various examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or configurations discussed.
[0063] Additionally, for ease of description, spatially relative terms, such as "below," "beneath," "lower," "above," "upper," and the like, may be used herein to describe the relationship of one element or feature illustrated in the figures to another element or feature. The spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations), and the spatially relative descriptors used herein may be similarly interpreted accordingly.
[0064] Embodiments are described in the specific context of integrated circuit dies including fin field-effect transistors (finFETs). However, various embodiments are applicable to dies including other types of transistors (e.g., nanoFETs such as nanowire FETs, nanosheet FETs, or the like, planar transistors, or the like), in place of or in combination with finFETs.
[0065] In various embodiments, a finFET is formed to include a plurality of semiconductor fins, some of which are adjacent to each other by isolation regions and dielectric fins. For example, the semiconductor fins may be separated from the dielectric fins by a gap region directly above the isolation region. A process of forming a dummy gate structure (e.g., a dummy dielectric layer and a dummy gate) above the semiconductor fins and the dielectric fins may be performed to provide sufficient space in the gap region to facilitate the deposition of the dummy gate and the subsequent removal of the dummy gate during the gate replacement process. In detail, a silicon layer is formed to cover both the semiconductor fins and the dielectric fins, and a dummy dielectric layer is formed above the silicon layer. The dummy dielectric layer and the silicon layer are then removed from the dielectric fins, wherein the silicon layer serves as a protective layer (e.g., an etch stop layer) for the dielectric fins and the isolation regions during the removal process. In this way, the gap region between the semiconductor fins and the dielectric fins is widened, thereby facilitating the deposition and subsequent removal of the dummy gate. Additionally, as discussed in more detail below, the disclosed embodiments allow for the dimensions and process parameters of various features to be adjusted to achieve additional benefits. The resulting integrated circuits including these semiconductor devices (e.g., finFETs) can have higher efficiency and improved yields while also providing better performance and reliability.
[0066] Figure 1 An example of a FinFET in a three-dimensional view according to some embodiments is illustrated. The FinFET includes a fin 52 on a substrate 50 (e.g., a semiconductor substrate). Isolation regions 56 are disposed in the substrate 50, and the fins 52 protrude above and between adjacent isolation regions 56. Although the isolation regions 56 are described / illustrated as being separated from the substrate 50, as used herein, the term "substrate" may be used to refer to only a semiconductor substrate or a semiconductor substrate including isolation regions. In addition, although the fin 52 is illustrated as a single continuous material as the substrate 50, the fin 52 and / or the substrate 50 may include a single material or multiple materials. In this context, the fin 52 refers to the portion extending between adjacent isolation regions 56.
[0067] A gate dielectric layer 92 is along the sidewalls of the fin 52 and over the top surface of the fin 52, and a gate electrode 94 is over the gate dielectric layer 92. Source / drain regions 82 are disposed on opposite sides of the fin 52 relative to the gate dielectric layer 92 and the gate electrode 94. The source / drain regions 82 may be referred to as a source or a drain, individually or collectively depending on the context. Figure 1Reference cross sections used in the subsequent figures are further illustrated. Cross section AA is along the longitudinal axis of gate electrode 94 and in a direction, for example, perpendicular to the direction of current flow between source / drain regions 82 of the FinFET. Cross section BB is perpendicular to cross section AA and along the longitudinal axis of fin 52 and in a direction, for example, of current flow between source / drain regions 82 of the FinFET. Cross section CC is parallel to cross section AA and extends through the source / drain region of the FinFET. For clarity, the subsequent figures refer to these reference cross sections.
[0068] Some embodiments discussed herein are discussed in the context of FinFETs formed using a gate-last process. In other embodiments, a gate-first process may be used. Additionally, some embodiments contemplate aspects used in planar devices such as planar FETs, nanostructure (e.g., nanosheets, nanowires, gate-all-around, or the like) field effect transistors (NSFETs), or the like.
[0069] Figures 2 to 23B is a cross-sectional view of an intermediate stage in fabricating a FinFET according to some embodiments. Figures 2 to 13 Graphics Figure 1 Reference cross section AA shown in , but for multiple fins / FinFETs. Fig.14A , Fig.15A , Fig.16A , Fig.17A , Fig.18A , Fig.19A , Fig. 20A , Fig.21A , Fig.22A ,and Fig.23A Along Figure 1 The reference cross section AA shown in FIG. Fig. 14B , Fig. 15B , Fig. 16B , Fig. 17B , Fig.18B , Fig.19B , Fig. 20B , Fig. 20C , Fig. 21B , Fig. 22B ,and Fig. 23B Along Figure 1 A similar cross section BB as shown in FIG. 1 is illustrated, but for multiple fins / FinFETs. Fig. 16C , Fig.16D , Fig. 17C , Fig.17D , Fig. 21C ,and Fig.21D Along Figure 1 , but for multiple fins / FinFETs.
[0070] exist Figure 2 A substrate 50 is provided in. The substrate 50 may be a semiconductor substrate, such as a bulk semiconductor, a semiconductor-on-insulator (SOI) substrate, or the like, which may be doped (e.g., with a p-type or n-type dopant) or undoped. The substrate 50 may be a wafer, such as a silicon wafer. In general, an SOI substrate is a layer of semiconductor material formed on an insulator layer. The insulator layer may be, for example, a buried oxide (BOX) layer, a silicon oxide layer, or the like. The insulator layer is disposed on a substrate, typically a silicon substrate or a glass substrate. Other substrates, such as multilayer substrates or gradient substrates may also be used. In some embodiments, the semiconductor material of the substrate 50 may include silicon; germanium; compound semiconductors including silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide, and / or indium antimonide; alloy semiconductors including silicon germanium, gallium arsenide phosphide, aluminum indium arsenide, aluminum gallium arsenide, gallium indium arsenide, gallium indium phosphide, and / or gallium indium arsenide phosphide; or combinations thereof.
[0071] The substrate 50 has a device region along the substrate 50, the device region including one or more n-type regions 50N and one or more p-type regions 50P. The n-type region 50N can be used to form an n-type device, such as an NMOS transistor, for example, an n-type FinFET. The p-type region 50P can be used to form a p-type device, such as a PMOS transistor, for example, a p-type FinFET. Some of the n-type regions 50N can be physically separated from the p-type regions 50P (or vice versa), and any number of device features (e.g., other active devices, doped regions, isolation structures, etc.) can be disposed between the n-type regions 50N and the p-type regions 50P. In addition, some of the n-type regions 50N can be adjacent to some of the p-type regions 50P. The illustrations are intended to represent any such configuration of the n-type regions 50N and the p-type regions 50P, if applicable.
[0072] exist Figure 3 In the embodiment, fins 52 are formed in substrate 50. Fins 52 are semiconductor strips. In some embodiments, fins 52 can be formed in substrate 50 by etching trenches in substrate 50. Etching can be any acceptable etching process, such as reactive ion etching (RIE), neutral beam etching (NBE), the like, or a combination thereof. Etching can be anisotropic. As a result, fins 52 are made of the same semiconductor material as substrate 50. As discussed in more detail below, some of fins 52 are replaced by different semiconductor materials, so that fins 52A remain in n-type region 50N, while fins 52B are formed in p-type region 50P (see Figure 6 In some embodiments, fin 52A and substrate 50 may include silicon, while fin 52B may include silicon germanium.
[0073] The fins may be patterned by any suitable method. For example, the fins 52 may be patterned by forming a mask 202 over the substrate 50 and using one or more optical lithography processes (including double patterning or multiple patterning processes). In general, double patterning or multiple patterning processes combine optical lithography with a self-aligned process, thereby allowing the generation of patterns having, for example, a smaller pitch than that obtainable using a single direct optical lithography process. For example, in one embodiment, a sacrificial layer is formed over the substrate and patterned using an optical lithography process. Spacers are formed next to the patterned sacrificial layer using a self-aligned process. The sacrificial layer is then removed, and the remaining spacers may then be used to pattern the fins. Although not specifically illustrated, in some embodiments, the mask 202 includes multiple layers, such as an oxide (e.g., silicon oxide), a nitride (e.g., silicon nitride), and a hard mask at the top. In some embodiments, the mask 202 (or other layers) may remain on the fins 52.
[0074] exist Figure 4 In the embodiment, the insulating material 54 is formed over the substrate 50 and between adjacent fins 52. The insulating material 54 may be an oxide such as silicon oxide, a nitride, the like, or a combination thereof, and may be formed by high density plasma chemical vapor deposition (HDP-CVD), flowable CVD (FCVD) (e.g., CVD-based material deposition in a remote plasma system and post-curing to convert it into another material such as an oxide), the like, or a combination thereof. Other insulating materials formed by any acceptable process may be used. In the illustrated embodiment, the insulating material 54 is silicon oxide formed by an FCVD process. Once the insulating material is formed, an annealing process may be performed. In an embodiment, the insulating material 54 is formed such that excess insulating material 54 covers the fins 52. Although the insulating material 54 is illustrated as a single layer, some embodiments may utilize multiple layers. For example, in some embodiments, a liner (not shown) may first be formed along the surface of the substrate 50 and the fins 52. Thereafter, a filler material such as the filler material discussed above may be formed over the liner.
[0075] exist Figure 5In the embodiment, a removal process is applied to the insulating material 54 to remove excess insulating material 54 above the fins 52 and the mask 202 (if present). In some embodiments, a planarization process may be used, such as chemical mechanical polish (CMP), an etch back process, a combination thereof, or the like. The planarization process exposes the fins 52 so that the top surfaces of the fins 52 and the insulating material 54 are flush after the planarization process is completed. In embodiments where the mask 202 remains on the fins 52, the planarization process may expose the mask 202 or remove the mask 202 so that the top surfaces of the mask 202 or the fins 52, respectively, are flush with the insulating material 54 after the planarization process is completed.
[0076] exist Figure 6 In the embodiment of the present invention, according to some embodiments, some of the fins 52 are converted into fins 52B, and the remaining fins 52 may be referred to as fins 52A. For example, the fins 52 include, for example, fins 52A that have been formed in the n-type region 50N and fins 52B that have been formed in the p-type region 50P. As shown in the figure, the fins 52B are formed in the insulating material 54 by replacing some of the fins 52 in the p-type region 50P. In some embodiments, the fins 52B may include a semiconductor material different from the fins 52A and the substrate 50.
[0077] In some embodiments, a removal process is performed to remove upper portions, most of, or all of some of the fins 52 (e.g., in the p-type region 50P). According to some embodiments, one or more suitable optical lithography masking (not specifically shown) and etching processes may be used to form the trenches. Next, the fins 52B are formed by forming a semiconductor material in the trenches. In some embodiments, the semiconductor material may be formed by epitaxially (e.g., heteroepitaxially) growing the semiconductor material in the trenches above the partially removed fins 52. After growing the fins 52B, a planarization process (e.g., CMP) may be performed to make the fins 52A flush with the insulating material 54 and the fins 52B, while also removing any semiconductor material that may have been formed above or on the insulating material 54. In some embodiments, the fins 52B are made of a material different from the fins 52A (e.g., silicon), such as silicon germanium (SiGe). x Ge 1-x , where x may be in the range of 0 to 1), silicon carbide, pure germanium or substantially pure germanium, III-V compound semiconductors, II-VI compound semiconductors, or the like. For example, available materials for forming III-V compound semiconductors include, but are not limited to, indium arsenide, aluminum arsenide, gallium arsenide, indium phosphide, gallium nitride, indium gallium arsenide, indium aluminum arsenide, gallium antimonide, aluminum antimonide, aluminum phosphide, gallium phosphide, and the like.
[0078] exist Figure 7In the embodiment of the present invention, dielectric fins 210 are formed in insulating material 54 between some of the fins 52. Dielectric fins 210 may also be referred to as dummy fins, dummy dielectric fins, or the like. Dielectric fins 210 may provide electrical isolation between certain components (e.g., active devices) of the integrated circuit on opposite sides of dielectric fins 210. Dielectric fins 210 may be formed using any suitable method. In some embodiments, dielectric fins 210 may include dielectric material that provides insulation between subsequently formed source / drain regions 82 (see FIG. 1 ). FIG. 16A to FIG. 16D ). The dielectric fin 210 may be formed by forming a trench in the insulating material 54, for example, using one or more photolithography masking and etching processes. One or more materials such as silicon nitride, silicon oxide, silicon carbonitride, silicon oxycarbonitride, combinations thereof, or the like may then be formed in the trench by CVD, ALD, the like, or a combination thereof. The structure may then be planarized (e.g., CMP) to make the dielectric fin 210 flush with the insulating material 54 and the fin 52.
[0079] exist Figure 8 In the embodiment of the present invention, the insulating material 54 is recessed to form a shallow trench isolation (STI) region 56. The insulating material 54 is recessed so that the upper portions of the fins 52 and the dielectric fins 210 in the n-type region 50N and the p-type region 50P protrude from between adjacent STI regions 56. In addition, the top surface of the STI region 56 may have a flat surface, a convex surface, a concave surface (such as a dish shape), or a combination thereof as shown. The top surface of the STI region 56 may be formed to be flat, convex, and / or concave by appropriate etching. An acceptable etching process may be used to recess the STI region 56, such as an etching process that is selective to the material of the insulating material 54 (for example, etching the material of the insulating material 54 at a faster rate than etching the material of the fins 52 and the dielectric fins 210). For example, oxide removal such as using dilute hydrofluoric (dHF) acid may be used.
[0080] about Figures 2 to 6The process described is only one example of how to form fins 52 (e.g., fins 52A, 52B). In some embodiments, the fins may be formed by an epitaxial growth process. For example, a dielectric layer may be formed above the top surface of substrate 50, and a groove may be etched through the dielectric layer to expose the underlying substrate 50. A homoepitaxial structure may be epitaxially grown in the groove, and the dielectric layer may be recessed so that the homoepitaxial structure protrudes from the dielectric layer to form a fin (e.g., fin 52A). In addition, in some embodiments, a heteroepitaxial structure may be used for fins 52 (e.g., fin 52B). In such embodiments, fin 52B includes a recessed material and an epitaxially grown material disposed above the recessed material. In further embodiments, a dielectric layer may be formed above the top surface of substrate 50, and a groove may be etched through the dielectric layer. Next, a heteroepitaxial structure may be epitaxially grown in the trench using a material different from the substrate 50, and the dielectric layer may be recessed so that the heteroepitaxial structure protrudes from the dielectric layer to form the fin 52B. In some embodiments of epitaxial growth of homoepitaxial or heteroepitaxial structures, the epitaxially grown material may be in-situ doped during growth, which may avoid prior and subsequent implantation, although in-situ doping and implantation doping may be used together.
[0081] Still further, it may be advantageous to epitaxially grow a different material in the n-type region 50N (eg, NMOS region) than in the p-type region 50P (eg, PMOS region). In various embodiments, the upper portion of the fin 52 (eg, fin 52B) may be made of silicon germanium (SiGe). x Ge 1-x , where x may be in the range of 0 to 1), silicon carbide, pure germanium or substantially pure germanium, III-V compound semiconductors, II-VI compound semiconductors, or the like. For example, available materials for forming III-V compound semiconductors include, but are not limited to, indium arsenide, aluminum arsenide, gallium arsenide, indium phosphide, gallium nitride, indium gallium arsenide, indium aluminum arsenide, gallium antimonide, aluminum antimonide, aluminum phosphide, gallium phosphide, and the like.
[0082] In addition, the dielectric fins 210 may be formed in additional ways not previously described. For example, in some embodiments discussed above (not specifically shown), the fins 52 may be formed prior to depositing the insulating material 54. A conformal sacrificial layer may then be deposited over the fins 52 and along the upper surface of the substrate 50, such that gaps remain in the sacrificial layer between adjacent fins 52. Dielectric material may be deposited over the sacrificial layer and in the gaps. The structure may be planarized to remove the dielectric material from the sacrificial layer, thereby forming the dielectric fins 210 from the dielectric material remaining in the gaps in the sacrificial layer. Thereafter, an etching process may be performed to remove the sacrificial layer from between the dielectric fins 210 and the fins 52. In some embodiments, some of the sacrificial layer may remain under the dielectric fins 210 and on the substrate 50. The insulating material 54 may then be deposited and recessed to form the STI regions 56, similar to as described above.
[0083] According to some embodiments, the fins 52 may have varying pitches and widths, resulting in the fins 52A being spaced apart from each other by a first distance D1, the fins 52B being spaced apart from each other by a second distance D2, and the fins 52A and 52B being spaced apart from each other by a third distance D3. Note that the distances D1, D2, and D3 (collectively referred to as the distances D N ) can be measured laterally at the closest point (eg, at the widest portion) between individual components over STI region 56. Distance D N Any of the gaps G1 and G2 (collectively referred to as G1 and G2) may be substantially the same or different from each other, and each may vary throughout the device area of the integrated circuit. In addition, the dielectric fin 210 may be spaced apart from the fin 52A by a first gap G1, and the dielectric fin 210 may be spaced apart from the fin 52B by a second gap G2. A ) may be substantially the same or different from one another, and each may vary throughout the device area of the integrated circuit.
[0084] In addition, the dielectric fin 210 between two fins 52A may be formed with a width W1, the dielectric fin 210 between two fins 52B may be formed with a width W2, and the dielectric fin 210 between fin 52A and fin 52B may be formed with a width W3. Note that the widths W1, W2, and W3 (collectively referred to as the width W A ) can be measured laterally at the closest point of the individual fins 52 (e.g., at the widest point of the dielectric fin 210). As shown, the distance D1 can be the sum of the two gaps G1 and the width W1. Similarly, the distance D3 can be the sum of the two gaps G2 and the width W2, and the distance D2 can be the sum of the gap G1, the gap G2, and the width W3. As discussed in more detail below, embodiments disclosed herein allow the distance D N and width W N to achieve advantages in the manufacture and performance of the integrated circuit device. It should be understood that the distance D Ncan represent the shortest of these distances in the integrated circuit, and these distances D N It can be in the range from 50nm to 60nm.
[0085] like Figure 8 As shown in A For measurements in the gap region 220, this becomes particularly important in various subsequent steps. For example, as discussed in more detail below, the material of the dummy gate layer is deposited over the dummy dielectric layer 60 and within the gap region 220 (see Fig.13 ). In addition, in a subsequent step, the same material is removed from above the dummy dielectric layer 60 and from within the gap region 220 (see FIG. 19A to FIG. 19B ). In some exemplary embodiments discussed herein, the exemplary distance D N The exemplary width W may be 50 nm. A Thus, the corresponding exemplary gap G A Each may be 20 nm.
[0086] In addition, Figure 8 In the embodiment of the present invention, appropriate wells (not shown) may be formed in the fin 52 and / or the substrate 50. In some embodiments, a P-well may be formed in the n-type region 50N, and an N-well may be formed in the p-type region 50P. In some embodiments, a P-well or an N-well is formed in both the n-type region 50N and the p-type region 50P.
[0087] In embodiments with different well types, photoresists and / or other masks (not shown) may be used to achieve different implantation steps for the n-type region 50N and the p-type region 50P. For example, a photoresist may be formed over the fin 52A and the STI region 56 in the n-type region 50N. The photoresist is patterned to expose the p-type region 50P of the substrate 50. The photoresist may be formed using a spin-on coating technique and may be patterned using acceptable optical lithography. Once the photoresist is patterned, n-type impurity implantation is performed in the p-type region 50P, and the photoresist may act as a mask to substantially prevent n-type impurities from being implanted in the n-type region 50N. The n-type impurity may be phosphorus, arsenic, antimony, or the like implanted in the region at a concentration equal to or less than 10 18 cm -3 , such as at about 10 16 cm -3 With about 10 18 cm -3 After implantation, the photoresist is removed, such as by an acceptable ashing process.
[0088] After implanting the p-type region 50P, a photoresist is formed over the fin 52B and STI region 56 in the p-type region 50P. The photoresist is patterned to expose the n-type region 50N of the substrate 50. The photoresist may be formed using a spin-on coating technique and may be patterned using acceptable optical lithography. Once the photoresist is patterned, a p-type impurity implant may be performed in the n-type region 50N, and the photoresist may act as a mask to substantially prevent the p-type impurity from being implanted in the p-type region 50P. The p-type impurity may be boron, boron fluoride, or the like implanted in the region at a concentration equal to or less than 10 18 cm -3 , such as at about 10 16 cm -3 With about 10 18 cm -3 After implantation, the photoresist may be removed, such as by an acceptable ashing process.
[0089] After implantation of n-type region 50N and p-type region 50P, annealing may be performed to repair implant damage and activate implanted p-type and / or n-type impurities. In some embodiments, the growth material of the epitaxial fin may be in-situ doped during growth, which may avoid implantation, although in-situ doping and implantation doping may be used together.
[0090] exist Fig. 9 In the embodiment of the present invention, a silicon layer 232 (e.g., a silicon cap or silicon cap layer) is deposited over the fin 52, the dielectric fin 210, and the STI region 56. As shown, in addition to the semiconductor material of the fin 52, the silicon layer is formed over and along the exposed surface of the dielectric fin 210 and the STI region 56. In some embodiments (not specifically shown), a section of the silicon layer 232 along the fin 52 may have a greater degree of crystallinity than a section of the silicon layer 232 along the dielectric fin 210 and the STI region 56, although both sections of the silicon layer 232 may be non-crystalline (e.g., polycrystalline or amorphous).
[0091] In some embodiments, silicon layer 232 may be formed as a non-selective deposition and growth. For example, silicon layer 232 may be deposited at a temperature of about 400° C. or less, a pressure ranging from 1 torr to 4 torr, and a duration ranging from 15 minutes to 30 minutes. Silicon layer 232 may be deposited with a thickness ranging from 0.5 nm to 1.0 nm (e.g., 0.8 nm). As discussed in more detail below (see Fig.10 ), the silicon layer 232 may have a substantially uniform thickness, or may vary across individual features (eg, fin 52A, fin 52B, dielectric fin 210, and STI region 56).
[0092] Optionally, according to various embodiments, a nitrogen soak treatment may be performed before forming the silicon layer 232. The nitrogen soak treatment may improve the subsequent formation of the silicon layer 232 by nitriding the exposed surfaces of the fins 52, the dielectric fins 210, and the STI regions 56. The precursor material may include ammonia, nitrogen, the like, or a combination thereof, and may be performed using a suitable method, such as a plasma process.
[0093] exist Fig.10 In the embodiment of the present invention, a dummy dielectric layer 60 is formed on the silicon layer 232. The dummy dielectric layer 60 may be, for example, silicon oxide, silicon nitride, a combination thereof, or the like, and may be deposited or thermally grown according to an acceptable technique. For example, the dummy dielectric layer 60 may be formed by converting a portion of the silicon layer 232 to oxide. In some embodiments, the dummy dielectric layer 60 is deposited by CVD, ALD, the like, or a suitable method.
[0094] After forming the dummy dielectric layer 60, the silicon layer 232 may have a thickness as described above, such as about 0.8 nm, and the thickness over the fin 52 may be greater than the thickness over the dielectric fin 210 and the STI region 56. Thus, the thickness of the silicon layer 232 over the fin 52 may be in the range of 0.8 nm to 1.0 nm, and in some embodiments, the thickness over the fin 52A is thicker than the thickness over the fin 52B. Additionally, the thickness of the silicon layer 232 over the dielectric fin 210 and the STI region 56 may be in the range of 0.5 nm to 0.8 nm. In some embodiments, the thickness of the silicon layer 232 may be substantially the same (e.g., 0.8 nm) over all of the features. Furthermore, dummy dielectric layer 60 may have a thickness ranging from 2.5 nm to 3.0 nm (eg, 2.8 nm), and dummy dielectric layer 60 may have a substantially uniform thickness over individual features (eg, fin 52A, fin 52B, dielectric fin 210 , and STI region 56 ).
[0095] In addition, with respect to the gap region 220, the portion of the dummy dielectric layer 60 above the dielectric fin 210 may be separated from the portion of the dummy dielectric layer 60 above the fin 52A by a third gap G3, and the portion of the dummy dielectric layer 60 above the dielectric fin 210 may be separated from the portion of the dummy dielectric layer 60 above the fin 52B by a fourth gap G4. The gaps G3 and G4 (collectively referred to as G B ) can be substantially the same or different from each other, and each gap can vary throughout the device area of the integrated circuit. As shown in the figure, the gap G B Smaller than gap G A . Refer to the above combination Figure 8 The exemplary embodiments discussed (eg, the exemplary distance D N The exemplary width W is 50 nm. AThe thickness of the silicon layer 232 may be 0.8 nm, and the thickness of the dummy dielectric layer 60 may be 2.7 nm (for example, the total thickness is 3.5 nm). B Each can be 13nm.
[0096] exist Fig.11 , a mask layer 240 is formed and patterned over the dummy dielectric layer 60, and the dummy dielectric layer 60 and the silicon layer 232 are removed from the dielectric fins 210. The mask layer 240 may be a multi-layer mask including a photoresist and a bottom anti-reflective coating (BARC), and may be formed using any suitable method. One or more etching processes may be used to remove the dummy dielectric layer 60 and the silicon layer 232. In some embodiments, the silicon layer 232 may be used as an etch stop layer to prevent undesired damage to the underlying portion of the STI region 56. As shown, a portion 56P of the STI region 56 that is proximate to (e.g., directly adjacent to) the dielectric fin 210 may be exposed after the removal process.
[0097] exist Fig.12 , the mask layer 240 is removed from the fins 52 and the STI regions 56. For example, in embodiments where the mask layer 240 comprises a photoresist, the removal of the mask layer 240 may utilize a process such as ashing, thereby increasing the temperature of the mask layer 240 until the mask layer 240 undergoes thermal decomposition and can be easily removed. However, any suitable method may be used.
[0098] In addition, regarding the gap region 220, the dielectric fin 210 may be separated from the portion of the dummy dielectric layer 60 above the fin 52A by a fifth gap G5, and the dielectric fin 210 may be separated from the portion of the dummy dielectric layer 60 above the fin 52B by a sixth gap G6. The gaps G5 and G6 (collectively referred to as G C ) can be substantially the same or different from each other, and each can vary throughout the device area of the integrated circuit. As shown in the figure, the gap G C Smaller than gap G A and is greater than the gap G B (For example, each is 13 nm). Figures 8 to 10 The exemplary embodiments discussed (eg, the exemplary distance D N The exemplary width W is 50 nm. A The total thickness of the silicon layer 232 and the dummy dielectric layer 60 is 3.5 nm), corresponding to the exemplary gap G C Each may be 16.5 nm.
[0099] exist Fig.13In the embodiment of the present invention, a dummy gate layer 62 is formed over the dummy dielectric layer 60 and in the gap region 220, and a mask layer 64 is formed over the dummy gate layer 62. The dummy gate layer 62 may be deposited over the dummy dielectric layer 60 and then planarized, such as by CMP. The mask layer 64 may be deposited over the dummy gate layer 62. The dummy gate layer 62 may be a conductive or non-conductive material and may be selected from the group consisting of amorphous silicon, polycrystalline silicon (poly-Si), polycrystalline silicon germanium (poly-SiGe), metal nitrides, metal silicides, metal oxides, and metals. The dummy gate layer 62 may be deposited by physical vapor deposition (PVD), CVD, sputtering deposition, or other techniques for depositing selected materials. The dummy gate layer 62 may be made of other materials having high etch selectivity relative to etching of isolation regions (e.g., STI regions 56 and / or dummy dielectric layer 60). The mask layer 64 may include one or more layers of, for example, silicon nitride, silicon oxynitride, or the like. In this example, a single dummy gate layer 62 and a single mask layer 64 are formed on the n-type region 50N and the p-type region 50P. It should be noted that the dummy dielectric layer 60 is shown covering only the fin 52 for illustration purposes only. In some embodiments, the dummy dielectric layer 60 may be deposited such that the dummy dielectric layer 60 covers the STI region 56, extends above the STI region and between the dummy gate layer 62 and the STI region 56.
[0100] The dummy gate layer 62 is deposited by separating the gap region 220 from the gap G B Widen to gap G C Specifically, the wider gap region 220 allows for more efficient deposition of the dummy gate layer 62 with higher yields and fewer or no voids. These results further facilitate subsequent steps, including removal of material of the dummy gate layer 62 and the dummy dielectric layer 60 (e.g., removal of FIG. 19A to FIG. 19B dummy gate in ).
[0101] In some embodiments, depending on various parameters and dimensions of the feature, the gap G C It may be necessary to be greater than or equal to the desired dimension to achieve the above benefits. For the example herein, the gap G C It may be necessary to have a distance greater than or equal to 15 nm to achieve such benefits. Thus, the dimensions or other parameters of some features may be adjusted to obtain additional benefits. For example, with respect to the exemplary embodiment (e.g., the exemplary distance D N is 50 nm, the total thickness of the silicon layer 232 and the dummy dielectric layer 60 is 3.5 nm, and the gap G C Each is at least 15 nm), the width W of the dielectric fin 210 AAs discussed in more detail below, some of the dielectric fins 210 help provide electrical isolation between adjacent gate electrodes (see FIG. 21A to FIG. 21D ). Thus, the larger width W A The dielectric fins 210 provide improved insulation between those adjacent gate electrodes while also reducing any deleterious effects that may occur from the conductive material of the gate electrodes diffusing into the dielectric fins 210 .
[0102] FIG. 14A to FIG. 23B Various additional steps in fabricating an embodiment device are illustrated. FIG. 14A to FIG. 23B Features in either the n-type region 50N or the p-type region 50P are shown. For example, FIG. 14A to FIG. 23B The structure shown in FIG. 5 is applicable to both the n-type region 50N and the p-type region 50P. The differences, if any, in the structures of the n-type region 50N and the p-type region 50P are described in the text accompanying each figure.
[0103] exist Fig.14A and Fig. 14B In the embodiment, the mask layer 64 (see Fig.13 ) is patterned to form a mask 74. The pattern of the mask 74 can then be transferred to the dummy gate layer 62. In some embodiments (not specifically shown), the pattern of the mask 74 can also be transferred to the dummy dielectric layer 60 (and the underlying silicon layer 232) by an acceptable etching technique to form a dummy gate 72. The dummy gate 72 covers the individual channel regions 58 of the fins 52. The pattern of the mask 74 can be used to physically separate each of the dummy gates 72 from the adjacent dummy gates. The dummy gates 72 can also have a length direction that is substantially perpendicular to the length direction of the individual epitaxial fins 52.
[0104] In some embodiments, the gate sealing spacer 80 may be formed on the exposed surface of the dummy gate 72, the mask 74, and / or the fin 52. Thermal oxidation or anisotropic etching after deposition may form the gate sealing spacer 80. The gate sealing spacer 80 may be formed of silicon oxide, silicon nitride, silicon oxynitride, or the like.
[0105] After forming the gate seal spacer 80, an implantation (not explicitly shown) for lightly doped source / drain (LDD) regions may be performed. In embodiments with different device types, similar to the above Figure 8, a mask, such as a photoresist, may be formed over the n-type region 50N while exposing the p-type region 50P, and an impurity of an appropriate type (e.g., p-type) may be implanted into the exposed fins 52 in the p-type region 50P. The mask may then be removed. Subsequently, a mask, such as a photoresist, may be formed over the p-type region 50P while exposing the n-type region 50N, and an impurity of an appropriate type (e.g., n-type) may be implanted into the exposed fins 52 in the n-type region 50N. The mask may then be removed. The n-type impurity may be any of the n-type impurities discussed previously, and the p-type impurity may be any of the p-type impurities discussed previously. The lightly doped source / drain region may have a thickness of about 10 15 cm -3 to about 10 19 cm -3 Annealing can be used to repair implant damage and activate implanted impurities.
[0106] exist Fig.15A and Fig. 15B , a gate spacer 86 is formed on the gate sealing spacer 80 along the sidewalls of the dummy gate 72 and the mask 74. The gate spacer 86 can be formed by conformally depositing an insulating material and then anisotropically etching the insulating material. The insulating material of the gate spacer 86 can be silicon oxide, silicon nitride, silicon oxynitride, silicon carbonitride, a combination thereof, or the like.
[0107] It should be noted that the above disclosure generally describes processes for forming spacers and LDD regions. Other processes and sequences may be used. For example, fewer or additional spacers may be utilized, a different sequence of steps may be utilized (e.g., gate sealing spacer 80 may not be etched prior to forming gate spacer 86, thereby producing an "L-shaped" gate sealing spacer), spacers may be formed and removed, and / or the like. Furthermore, different structures and steps may be used to form n-type and p-type devices. For example, an LDD region for an n-type device may be formed prior to forming gate sealing spacer 80, while an LDD region for a p-type device may be formed after forming gate sealing spacer 80.
[0108] exist FIG. 16A to FIG. 16D In the embodiment of the present invention, epitaxial source / drain regions 82 are formed in the fins 52. The epitaxial source / drain regions 82 are formed in the fins 52 so that each dummy gate 72 is disposed between respective adjacent pairs of epitaxial source / drain regions 82. In some embodiments, the epitaxial source / drain regions 82 may extend into the fins 52 or may penetrate the fins 52. In some embodiments, gate spacers 86 are used to separate the epitaxial source / drain regions 82 from the dummy gates 72 by an appropriate lateral distance so that the epitaxial source regions 82 do not short-circuit a subsequently formed gate of the resulting FinFET. The material of the epitaxial source / drain regions 82 may be selected to apply stress in respective channel regions 58, thereby improving performance.
[0109] The epitaxial source / drain region 82 in the n-type region 50N can be formed by masking the p-type region 50P and etching the source / drain region of the fin 52 in the n-type region 50N to form a groove in the fin 52. Then, the epitaxial source / drain region 82 in the n-type region 50N is epitaxially grown in the groove. The epitaxial source / drain region 82 may include any acceptable material, such as a material suitable for n-type FinFETs. For example, if the fin 52 is silicon, the epitaxial source / drain region 82 in the n-type region 50N may include a material that applies tensile stress in the channel region 58, such as silicon, silicon carbide, phosphorus-doped silicon carbide, silicon phosphide, or the like. The epitaxial source / drain region 82 in the n-type region 50N may have a surface that protrudes from the individual surfaces of the fin 52 and may have a small facet.
[0110] The epitaxial source / drain region 82 in the p-type region 50P can be formed by masking the n-type region 50N and etching the source / drain region of the fin 52 in the p-type region 50P to form a groove in the fin 52. Then, the epitaxial source / drain region 82 in the p-type region 50P is epitaxially grown in the groove. The epitaxial source / drain region 82 may include any acceptable material, such as a material suitable for a p-type FinFET. For example, if the fin 52 is silicon, the epitaxial source / drain region 82 in the p-type region 50P may include a material that applies compressive stress in the channel region 58, such as silicon germanium, boron-doped silicon germanium, germanium, germanium tin, or the like. The epitaxial source / drain region 82 in the p-type region 50P may have a surface protruding from the individual surface of the fin 52 and may have a small facet.
[0111] The epitaxial source / drain regions 82 and / or the fins 52 may be implanted with dopants to form source / source regions, similar to the process for forming lightly doped source / drain regions discussed previously, followed by annealing. The source / drain regions may have a surface area of about 10 19 cm -3 With about 10 21 cm -3 The n-type and / or p-type impurities used for the source / drain regions may be any of the impurities discussed previously. In some embodiments, the epitaxial source / drain regions 82 may be doped in situ during growth.
[0112] As a result of the epitaxial process used to form epitaxial source / drain regions 82 in n-type region 50N and p-type region 50P, the upper surface of the epitaxial source / drain region has facets that extend laterally outward beyond the sidewalls of fin 52. In some embodiments, these facets result in the merging of adjacent source / drain regions 82 of the same FinFET, such as Fig. 16C In other embodiments, after the epitaxial process is completed, adjacent source / drain regions 82 remain separated, such as Fig.16D As shown in Fig. 16C and Fig.16D In the embodiment shown in , gate spacer 86 is formed to cover a portion of the sidewalls of fin 52 that extends over STI region 56, thereby blocking epitaxial growth. In some other embodiments, the spacer etch used to form gate spacer 86 can be adjusted to remove spacer material, thereby allowing the epitaxial growth region to extend to the surface of STI region 56. Note that Fig. 16C and Fig.16D The fin 52 shown in FIG. 5 may be applicable to either fin 52A or fin 52B.
[0113] exist FIG. 17A to FIG. 17D in FIG. 16A to FIG. 16D A first interlayer dielectric (ILD) 88 is deposited over the structure shown in FIG. The first ILD 88 may be formed of a dielectric material and may be deposited by any suitable method, such as CVD, plasma-enhanced CVD (PECVD), or FCVD. The dielectric material may include phosphosilicate glass (PSG), borosilicate glass (BSG), borophosphosilicate glass, undoped silica glass, or the like. Other insulating materials formed by any acceptable process may be used. In some embodiments, a contact etch stop layer (CESL) 87 is disposed between the first ILD 88 and the epitaxial source / drain regions 82, the mask 74, and the gate spacer 86. The CESL 87 may include a dielectric material, such as silicon nitride, silicon oxide, silicon oxynitride, or the like, which has a lower etch rate than the material overlying the first ILD 88.
[0114] exist Fig.18A and Fig.18B In the process, a planarization process such as CMP may be performed to make the top surface of the first ILD 88 flush with the top surface of the dummy gate 72 or the mask 74. The planarization process may also remove the mask 74 on the dummy gate 72, and the portions of the gate sealing spacer 80 and the gate spacer 86 along the sidewalls of the mask 74. After the planarization process, the top surfaces of the dummy gate 72, the gate sealing spacer 80, the gate spacer 86, and the first ILD 88 are flush. Therefore, the top surface of the dummy gate 72 is exposed through the first ILD 88. In some embodiments, the mask 74 may remain, in which case the planarization process makes the top surface of the first ILD 88 flush with the top surface of the mask 74.
[0115] exist Fig.19A and Fig.19BIn the etching step, the dummy gate 72 and the mask 74 (if present) are removed to form the recess 90. Portions of the dummy dielectric layer 60 and the silicon layer 232 (if present) in the recess 90 may also be removed (e.g., including in the gap region 220). In some embodiments, only the dummy gate 72 is removed, and the dummy dielectric layer 60 remains and is exposed by the recess 90. In some embodiments, the dummy dielectric layer 60 is removed from the recess 90 in the first region of the die (e.g., the core logic region) and remains in the recess 90 in the second region of the die (e.g., the input / output region). In some embodiments, the dummy gate 72 is removed by an anisotropic dry etching process. For example, the etching process may include a dry etching process using a reactive gas to selectively etch the dummy gate 72 with little or no etching of the first ILD 88 or the gate spacer 86. Each recess 90 exposes and / or covers the channel region 58 of a respective fin 52. Each channel region 58 is disposed between adjacent pairs of epitaxial source / drain regions 82. During removal, the dummy dielectric layer 60 and the silicon layer 232 may serve as an etch stop layer when etching the dummy gate 72. After removing the dummy gate 72, the dummy dielectric layer 60 and the silicon layer 232 may be selectively removed. In some embodiments (not specifically shown), the portion 56P of the STI region 56 that is proximate to (e.g., directly adjacent to) the dielectric fin 210 (e.g., the portion that is exposed after removing the silicon layer 232 and the dummy dielectric layer 60 from the dielectric fin 210) may be exposed to the dummy gate 72 due to the presence of a dummy gate electrode 72 in the STI region 56. FIG. 19A to FIG. 19B The dummy dielectric layer 60 in question is partially etched and becomes recessed during removal.
[0116] By separating the gap region 220 from the gap G B Widen to gap G C The previous step improves the removal of the dummy gate 72 and the dummy dielectric layer 60 (see Fig.12 In detail, the widened gap region 220 allows for more efficient removal of the dummy gate 72 with a higher yield because the etchant can more easily reach all corners of the gap region 220. In addition, in the dummy gate layer 62 (see Fig.13 ) during the deposition of the dummy gate 72 and the dummy dielectric layer 60, while reducing the risk of damaging other features, such as through over-etching. A In the embodiment of the present invention, these benefits and the benefits discussed previously can still be achieved. In addition, additional benefits include any damage to the dielectric fins 210 caused during this removal process will reduce the impact on the electrical isolation capabilities of these wider dielectric fins 210.
[0117] exist FIG. 20A to FIG. 20C In the process, a gate dielectric layer 92 and a gate electrode 94 are formed for replacing the gate. Fig. 20C Graphics Fig. 20B Detailed view of region 89 of fin 52. Gate dielectric layer 92 is deposited in recess 90, such as on the top surface and sidewalls of fin 52 and on the sidewalls of gate seal spacer 80 / gate spacer 86. Gate dielectric layer 92 may also be formed on the top surface of first ILD 88. In some embodiments, gate dielectric layer 92 includes one or more dielectric layers, such as one or more layers of silicon oxide, silicon nitride, metal oxide, metal silicate, or the like. For example, in some embodiments, gate dielectric layer 92 includes an interfacial layer of silicon oxide formed by thermal oxidation or chemical oxidation and an overlying high-k dielectric material, such as a metal oxide or silicate of hafnium, aluminum, zirconium, lanthanum, manganese, barium, titanium, lead, and combinations thereof. Gate dielectric layer 92 may include a dielectric layer having a k value greater than about 7.0. Methods of forming gate dielectric layer 92 may include molecular-beam deposition (MBD), ALD, PECVD, and the like. In embodiments where portions of dummy dielectric layer 60 remain in recesses 90, gate dielectric layer 92 includes the material (e.g., SiO2) of dummy dielectric layer 60. Additionally, in embodiments where portions 56P of STI regions 56 proximate to (e.g., directly adjacent to) dielectric fins 210 are partially etched during removal of dummy dielectric layer 60, gate dielectric layer 92 may further be formed in those corresponding recesses.
[0118] The gate electrode 94 is deposited over the gate dielectric layer 92 and fills the remaining portion of the recess 90. The gate electrode 94 may include a metal-containing material such as titanium nitride, titanium oxide, tantalum nitride, tantalum carbide, cobalt, ruthenium, aluminum, tungsten, combinations thereof, or multiple layers thereof. For example, although Fig. 20B A single-layer gate electrode 94 is shown in FIG. 1 , but the gate electrode 94 may include any number of liner layers 94A, any number of work function tuning layers 94B, and a filling material 94C, such as Fig. 20C . After filling the recess 90, a planarization process such as CMP may be performed to remove excess portions of the gate dielectric layer 92 and the gate electrode 94 material that are above the top surface of the ILD 88. The material of the gate electrode 94 and the remaining portion of the gate dielectric layer 92 thus form a replacement gate for the resulting FinFET. The gate electrode 94 and the gate dielectric layer 92 may be collectively referred to as a "gate stack". The gate and the gate stack may extend along the sidewalls of the channel region 58 of the fin 52.
[0119] The formation of the gate dielectric layer 92 in the n-type region 50N and the p-type region 50P may occur simultaneously, such that the gate dielectric layer 92 in each region is formed of the same material, and the formation of the gate electrode 94 may occur simultaneously, such that the gate electrode 94 in each region is formed of the same material. In some embodiments, the gate dielectric layer 92 in each region may be formed by different processes, such that the gate dielectric layer 92 may be a different material, and / or the gate electrode 94 in each region may be formed by different processes, such that the gate electrode 94 may be a different material. When different processes are used, various masking steps may be used to mask and expose the appropriate regions.
[0120] exist FIG. 21A to FIG. 21D In the embodiment of the present invention, a gate mask 96 is formed over the gate stack (including the gate dielectric layer 92 and the corresponding gate electrode 94), and the gate mask 96 may be disposed between the opposing portions of the gate spacers 86. In addition, a gate isolation region 244 is formed through the gate electrode 94 and reaches some of the dielectric fins 210. In some embodiments, forming the gate mask 96 includes recessing the gate stack so that a groove is formed directly over the gate stack and between the opposing portions of the gate spacers 86. The gate mask 96 including one or more layers of a dielectric material (such as silicon nitride, silicon oxynitride, or the like) is filled in the groove, followed by a planarization process to remove excess portions of the dielectric material extending over the first ILD 88. The gate mask 96 is optional and may be omitted in some embodiments. In such embodiments, the gate stack may remain flush with the top surface of the first ILD 88.
[0121] After forming the gate mask 96, one or more etching processes are performed to form openings and expose the dielectric fins 210. The etching process may include forming an etching mask (such as a photoresist or a three-layer etching mask, not specifically shown), patterning the etching mask, and etching the gate mask 96, ILD 88, CESL 87, gate electrode 94, and gate dielectric layer 92 to form openings.
[0122] A dielectric material is deposited in the opening to form a structure of the gate isolation region 244. According to some embodiments, the dielectric material is formed of a homogenous dielectric material such as silicon nitride, silicon oxide, or the like. In some embodiments, the dielectric material includes a plurality of dielectric layers. For example, the dielectric material may include a dielectric liner formed of a first dielectric material, and a second dielectric material above the dielectric liner. The second dielectric material is different from the first dielectric material. For example, the first dielectric material may include silicon oxide, and the second dielectric material may include silicon nitride. Alternatively, the first dielectric material may include silicon nitride, and the second dielectric material may include silicon oxide.
[0123] After the dielectric material is deposited, a planarization process is performed to level the top surface of the dielectric material. In some embodiments (not specifically shown), after the planarization process, a portion of the dielectric material may remain, overlapping the gate mask 96, to act as a hard mask layer. According to an alternative embodiment, the planarization process is performed until the top surface of the gate mask 96 or the gate electrode 94 is exposed. The portion of the dielectric material in the opening forms a gate isolation region 244, which may also be referred to as a cut metal gate (CMG) region. The gate isolation region 244 works in conjunction with the dielectric fin 210 to electrically isolate the gate electrode 94 on the opposite side.
[0124] exist Fig.22A and Fig. 22B In the embodiment, the second ILD 108 is deposited over the first ILD 88. In some embodiments, the second ILD 108 is a flowable film formed by a flowable CVD method. In some embodiments, the second ILD 108 is formed of a dielectric material such as phosphosilicate glass (PSG), borosilicate glass (BSG), borophosphosilicate glass (BPSG), undoped silicate glass (USG), or the like, and can be deposited by any suitable method such as CVD and PECVD. The gate contact 110 ( Fig.23A and Fig. 23B ) penetrates the second ILD 108 and the gate mask 96 (if present) to contact the top surface of the recessed gate electrode 94.
[0125] exist Fig.23A and Fig. 23BIn some embodiments, a gate contact 110 and a source / drain contact 112 are formed through the second ILD 108 and the first ILD 88. An opening for the source / drain contact 112 is formed through the first ILD 88 and the second ILD 108, and an opening for the gate contact 110 is formed through the second ILD 108 and the gate mask 96 (if present). Acceptable optical lithography and etching techniques may be used to form the opening. A liner (not shown) such as a diffusion barrier layer, an adhesion layer, or the like and a conductive material are formed in the opening. The liner may include titanium, titanium nitride, tantalum, tantalum nitride, or the like. The conductive material may be copper, a copper alloy, silver, gold, tungsten, cobalt, aluminum, nickel, or the like. A planarization process such as CMP may be performed to remove excess material from the surface of the ILD 108. The remaining liner and conductive material form the source / drain contact 112 and the gate contact 110 in the opening. An annealing process may be performed to form silicide at the interface between the epitaxial source / drain region 82 and the source / drain contact 112. The source / drain contact 112 is physically and electrically coupled to the epitaxial source / drain region 82, while the gate contact 110 is physically and electrically coupled to the gate electrode 106. The source / drain contact 112 and the gate contact 110 may be formed in different processes, or may be formed in the same process. Although shown as being formed in the same cross section, it should be understood that each of the source / drain contact 112 and the gate contact 110 may be formed in different cross sections, which may avoid shorting of the contacts.
[0126] It should be understood that the embodiments disclosed herein are applicable to fin 52A (e.g., comprising silicon), fin 52B (e.g., comprising silicon germanium), and their corresponding dielectric fins 210. Furthermore, dimensions associated with fin 52A and corresponding dielectric fin 210 may be similar to (e.g., substantially the same as) or different from dimensions associated with fin 52B and corresponding dielectric fin 210. Furthermore, dimensions associated with fin 52A and fin 52B separated from each other by corresponding dielectric fin 210 may be similar to fins 52A, 52B on opposite sides. For example, the gap region 220 with fin 52A may be different from the gap region 220 with fin 52B, as applicable and consistent with the above discussion.
[0127] Several advantages can be achieved. For example, the disclosed embodiments facilitate increasing the gap G between the fin 52 and the dielectric fin 210. A, in order to improve various steps, including depositing the dummy gate layer 62 and removing the dummy gate 72 and the dummy dielectric layer 60. In addition, the disclosed embodiments allow the dimensions of various features to be adjusted, such as widening some or all of the dielectric fins 210 to improve isolation between adjacent gate electrodes 94. In addition, the disclosed embodiments allow various process parameters to be adjusted, such as reducing the duration of depositing the dummy gate layer 62 or removing the dummy gate 72 and the dummy dielectric layer 60.
[0128] The disclosed FinFET embodiments may also be applied to nanostructure devices, such as nanostructure (e.g., nanosheets, nanowires, gate-all-around, or the like) field effect transistors (NSFETs). In NSFET embodiments, the fins are replaced by nanostructures formed by patterning a stack of alternating layers of channel layers and sacrificial layers. The dummy gate stack and source / drain regions are formed in a manner similar to the above-described embodiments. After removing the dummy gate stack, the sacrificial layer in the channel region may be partially or completely removed. A replacement gate structure is formed in a manner similar to the above-described embodiments, the replacement gate structure may partially or completely fill the opening left by removing the sacrificial layer, and the replacement gate structure may partially or completely surround the channel layer in the channel region of the NSFET device. An ILD and contacts to the replacement gate structure and source / drain regions may be formed in a manner similar to the above-described embodiments. The nanostructure device may be formed as disclosed in U.S. Pat. No. 9,647,071, which is incorporated herein by reference in its entirety.
[0129] In an embodiment, a method includes: forming a plurality of fins over a substrate, the plurality of fins including: a first semiconductor fin adjacent to an isolation region; and a dielectric fin embedded in the isolation region; depositing a silicon layer over a first surface of the first semiconductor fin, a second surface of the dielectric fin, and a third surface of the isolation region; forming an oxide layer over the silicon layer; removing a portion of the oxide layer and the silicon layer to expose the second surface of the dielectric fin; forming a dummy gate over a remaining portion of the oxide layer and between a plurality of fins; forming a first epitaxial region in the first semiconductor fin; and replacing the dummy gate with a gate structure. In another embodiment, the plurality of fins includes a second semiconductor fin adjacent to the isolation region, and wherein the dielectric fin is inserted between the first semiconductor fin and the second semiconductor fin. In another embodiment, the first semiconductor fin and the second semiconductor fin include different materials. In another embodiment, the thickness of the silicon layer over the first semiconductor fin is different from the thickness of the silicon layer over the second semiconductor fin. In another embodiment, replacing the dummy gate with a gate structure includes: removing the dummy gate; removing the remaining portion of the oxide layer; forming a gate dielectric over the first semiconductor fin; and forming a gate electrode over the gate dielectric. In another embodiment, removing portions of the oxide layer and the silicon layer to expose the dielectric fins includes exposing portions of the isolation regions proximate to the dielectric fins, and wherein removing remaining portions of the oxide layer includes removing portions of the isolation regions proximate to the dielectric fins.
[0130] In an embodiment, a method includes: forming a first fin over a first region of a substrate, the first fin comprising a silicon fin and a first dielectric fin; forming a second fin over a second region of the substrate, the second fin comprising a silicon germanium fin and a second dielectric fin; forming a first isolation region and a second isolation region over the substrate, the first isolation region being inserted between the silicon fin and the first dielectric fin, a first gap region being over the first isolation region and between the first fins, the second isolation region being inserted between the silicon germanium fin and the second dielectric fin, the second gap region being over the second isolation region and between the second fins; forming a first fin over the first fin, the first isolation region, and a second isolation region over the second fin; , forming a silicon layer over the first fin, the second fin, and the second isolation region; forming an oxide layer over the silicon layer, wherein forming the silicon layer and forming the oxide layer include reducing the first lateral width of the first gap region and the second lateral width of the second gap region; etching portions of the oxide layer and the silicon layer to expose the first dielectric fin and the second dielectric fin, wherein etching portions of the oxide layer and the silicon layer include increasing the first lateral width of the first gap region and the second lateral width of the second gap region; forming a first gate structure over the first fin and in the first gap region; and forming a second gate structure over the second fin and in the first gap region. In another embodiment, forming the silicon layer is performed at a temperature less than or equal to 450°C. In another embodiment, the first portion of the silicon layer over the silicon fin has a first crystallinity, wherein the second portion of the silicon layer over the first dielectric fin has a second crystallinity, and wherein the first crystallinity is greater than the second crystallinity. In another embodiment, the silicon layer has a first thickness along the silicon fin, a second thickness along the silicon germanium fin, and a third thickness along the first dielectric fin, and wherein the third thickness is less than the first thickness and the second thickness. In another embodiment, the first thickness is greater than the second thickness. In another embodiment, the method further includes, before forming the silicon layer, nitriding the exposed surfaces of the silicon fin, the first dielectric fin, the silicon germanium fin, and the second dielectric fin. In another embodiment, the method further includes: removing the first gate structure and the second gate structure; forming a first replacement gate structure over the first fin; and forming a second replacement gate structure over the second fin. In another embodiment, the method further includes: etching an opening in the first gate structure to expose the first dielectric fin; and forming a gate isolation region in the opening.
[0131] In an embodiment, a method includes: forming a semiconductor fin and a dielectric fin in an insulating material disposed above a substrate; recessing the insulating material to form an isolation region, the semiconductor fin and the dielectric fin protruding above an upper surface of the isolation region; depositing a silicon layer above a first surface of the semiconductor fin, a second surface of the dielectric fin, and an upper surface of the isolation region; depositing a dummy dielectric layer above the silicon layer; removing portions of the dummy dielectric layer and the silicon layer from the second surface of the dielectric fin; and forming a dummy gate above the semiconductor fin and the dielectric fin, the dummy gate being in physical contact with the isolation region. In another embodiment, after depositing the dummy dielectric layer, a first gap remains above the isolation region and between sidewalls of the dummy dielectric layer, wherein the first gap is less than a desired dimension, wherein after removing portions of the dummy dielectric layer and the silicon layer, a second gap remains above the isolation region and between the remaining sidewalls of the dummy dielectric layer and the dielectric fin, and wherein the second gap is greater than the desired dimension. In another embodiment, a first segment of the silicon layer along the first surface of the semiconductor fin has a different crystallinity than a second segment of the silicon layer along the second surface of the dielectric fin and the upper surface of the isolation region. In another embodiment, the first segment has a greater crystallinity than the second segment. In another embodiment, the method further includes: removing the dummy gate; and removing the dummy dielectric layer, wherein removing the dummy dielectric layer includes etching a portion of the isolation region proximate to the dielectric fin. In another embodiment, the method further includes, before depositing the silicon layer, performing a nitrogen soak process to nitride the first surface of the semiconductor fin, the second surface of the dielectric fin, and the upper surface of the isolation region.
[0132] The foregoing summarizes the features of several embodiments so that those skilled in the art can better understand the aspects of the present disclosure. Those skilled in the art will appreciate that they can readily use the present disclosure as a basis for designing or modifying other processes and structures for implementing the same purposes and / or achieving the same advantages of the embodiments introduced herein. Those skilled in the art will also recognize that such equivalent constructions do not depart from the spirit and scope of the present disclosure, and such equivalent constructions may be variously modified, substituted, and replaced herein without departing from the spirit and scope of the present disclosure.
Claims
1. A method for forming a semiconductor device, characterized in that: The following steps are involved: A plurality of fins are formed on a substrate, wherein the plurality of fins include: a first semiconductor fin adjacent to an isolation region; and a dielectric fin embedded in the isolation region; Depositing a silicon layer over a first surface of the first semiconductor fin, a second surface of the dielectric fin, and a third surface of the isolation region; forming an oxide layer over the silicon layer; removing a portion of the oxide layer and the silicon layer to expose the second surface of the dielectric fin; forming a dummy gate over a remaining portion of the oxide layer and between the plurality of fins; forming a first epitaxial region in the first semiconductor fin; and The dummy gate is replaced with a gate structure.
2. The method for forming a semiconductor device according to claim 1, wherein: Replacing the dummy gate with the gate structure comprises the following steps: removing the dummy gate; removing the remaining portion of the oxide layer; forming a gate dielectric over the first semiconductor fin; and A gate electrode is formed over the gate dielectric.
3. The method for forming a semiconductor device according to claim 2, wherein: The step of removing the portion of the oxide layer and the silicon layer to expose the dielectric fin includes the following steps: exposing a portion of the isolation region adjacent to the dielectric fin, and wherein the step of removing the remaining portion of the oxide layer includes the following steps: removing the portion of the isolation region adjacent to the dielectric fin.
4. A method for forming a semiconductor device, characterized in that: The following steps are involved: Forming a plurality of first fins above a first region of a substrate, the plurality of first fins comprising a silicon fin and a first dielectric fin; forming a plurality of second fins above a second region of the substrate, the plurality of second fins comprising a silicon germanium fin and a second dielectric fin; A first isolation region and a second isolation region are formed above the substrate, wherein the first isolation region is inserted between the silicon fin and the first dielectric fin, a first gap region is above the first insulating region and between the plurality of first fins, and a second gap region is above the second isolation region and between the plurality of second fins; forming a silicon layer over the plurality of first fins, the first isolation region, the plurality of second fins, and the second isolation region; forming an oxide layer over the silicon layer, wherein forming the silicon layer and forming the oxide layer include reducing a first lateral width of the first gap region and a second lateral width of the second gap region; Etching portions of the oxide layer and the silicon layer to expose the first dielectric fin and the second dielectric fin, wherein etching the portions of the oxide layer and the silicon layer includes increasing the first lateral width of the first gap region and the second lateral width of the second gap region; forming a first gate structure above the first fin and in the first gap region; and A second gate structure is formed above the second fin and in the second gap region.
5. The method for forming a semiconductor device according to claim 4, wherein: The silicon layer has a first thickness along the silicon fin, a second thickness along the silicon germanium fin, and a third thickness along the first dielectric fin, wherein the third thickness is less than the first thickness and the second thickness.
6. The method for forming a semiconductor device according to claim 4, wherein: Further comprising the following steps: removing the first gate structure and the second gate structure; forming a first replacement gate structure over the plurality of first fins; and A second replacement gate structure is formed above the plurality of second fins.
7. The method for forming a semiconductor device according to claim 6, wherein: Further comprising the following steps: etching an opening in the first gate structure to expose the first dielectric fin; and A gate isolation region is formed in the opening.
8. A method for forming a semiconductor device, characterized in that: The following steps are involved: forming a semiconductor fin and a dielectric fin in an insulating material disposed above a substrate; Recessing the insulating material to form an isolation region, the semiconductor fin and the dielectric fin protruding above an upper surface of the isolation region; depositing a silicon layer over a first surface of the semiconductor fin, a second surface of the dielectric fin, and the upper surface of the isolation region; Depositing a dummy dielectric layer on the silicon-containing layer; removing portions of the dummy dielectric layer and the silicon layer from the second surface of the dielectric fin; and A dummy gate is formed above the semiconductor fin and the dielectric fin, and the dummy gate is in physical contact with the isolation region.
9. The method for forming a semiconductor device according to claim 8, wherein: After depositing the dummy dielectric layer, a first gap remains over the isolation region and between multiple sidewalls of the dummy dielectric layer, wherein the first gap is less than a desired dimension, and after removing the multiple portions of the dummy dielectric layer and the silicon layer, a second gap remains over the isolation region and between a remaining sidewall of the dummy dielectric layer and the dielectric fin, and wherein the second gap is greater than the desired dimension.
10. The method for forming a semiconductor device according to claim 8, wherein: The method further comprises the following steps: performing a nitrogen soaking process before depositing the silicon layer to nitride the first surface of the semiconductor fin, the second surface of the dielectric fin, and the upper surface of the isolation region.
Citation Information
Patent Citations
FINFET structures and methods of forming the same
US9647071B2