Groove forming method, field effect transistor preparation method and process equipment
By alternately performing deposition and etching steps, the protective film protects the first sidewall, solving the problem of excessive etching of the first sidewall during groove formation, ensuring the integrity of the gate layer and the quality of source and drain growth.
Patent Information
- Application Number
- CN202410903321.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-11
AI Technical Summary
During the formation of the groove, the first sidewalls were over-etched, resulting in the inability to wrap the gate layer of the gate structure, which easily caused defects during subsequent source and drain growth.
By alternately performing the deposition step and the first etching step, a first protective film is formed to cover the first sidewall, and after the second protective film is removed, at least part of the second sidewall is etched to ensure that the first protective film is not completely etched. , thereby protecting the first sidewall from excessive loss and ensuring that the first sidewall can effectively wrap the gate layer of the gate structure after the target groove is formed.
This effectively avoids defects in the gate layer of the gate structure during source and drain growth, ensuring the integrity of the gate layer and the smooth progress of subsequent processes.
Smart Images

Figure CN118762995A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor manufacturing technology, and in particular to a method for forming a groove, a method for preparing a field effect transistor, and a process equipment. Background Art
[0002] In integrated circuits with a process of 14nm and below, in order to solve the leakage problem caused by the short channel effect, the field effect transistor structure is transformed from a planar field effect transistor (Planar Field Effect Transistor, referred to as Planar FET) to a fin field effect transistor (Fin Field Effect Transistor, referred to as FinFET) with a three-dimensional gate structure.
[0003] In one process route, during the preparation of the source and drain, it is necessary to first etch the fin structure between two adjacent gate structures to form a target groove in the fin structure, such as a silicon groove (Si Recess); then selectively grow the source and drain in the target groove to form the source and drain on both sides of the gate structure respectively. Summary of the invention
[0004] The present application provides a method for forming a groove, a method for preparing a field effect transistor and a process equipment to solve the problem in the related art that, during the process of forming the groove, the first side wall is over-etched, resulting in the first side wall being unable to wrap the gate layer of the gate structure, which in turn causes the gate layer of the gate structure to be prone to defects during the subsequent source and drain growth.
[0005] The first aspect of the present application provides a method for forming a groove, which is applied to a film layer to be etched, wherein a plurality of fin structures and a plurality of gate structures are arranged on the film layer to be etched, the plurality of fin structures are arranged at intervals, the plurality of gate structures are arranged at intervals and straddle the plurality of fin structures, the sidewalls of the gate structures are provided with a first sidewall, the sidewalls of the fin structures are provided with a second sidewall, and the second sidewall is located between two adjacent gate structures; the method comprises: alternately performing a deposition step and a first etching step, etching at least a portion of the second sidewall to expose the fin structure between two adjacent gate structures; wherein the deposition step is used to deposit a first protective film on the top of the gate structure, and the first protective film covers the top surface of the first sidewall, and is also used to deposit a second protective film on the top of the fin structure, and the second protective film covers the top surface of the second sidewall, the thickness of the first protective film is greater than the thickness of the second protective film, and the first etching step is used to remove the second protective film, and at least partially etch the second sidewall and partially etch the first protective film; etching the fin structure between two adjacent gate structures to form a target groove.
[0006] In one embodiment, the deposition step and the first etching step are alternately performed to at least partially etch the second sidewall spacer, including: alternately and cyclically performing the deposition step and the first etching step to etch the entire second sidewall spacer to remove the second sidewall spacer.
[0007] In one embodiment, the process conditions of the deposition step further include a lower electrode power of 0 W to control the non-directionality of plasma so that the amount of deposition byproducts deposited on the top of the gate structure is greater than that deposited on the top of the fin structure.
[0008] In one embodiment, the film layer to be etched has a pattern-dense area and a pattern-sparse area, the gate structure includes a first gate structure located in the pattern-sparse area and a second gate structure located in the pattern-dense area, the first protective film includes a first sub-protective film and a second sub-protective film, the first sub-protective film is deposited on the top of the first gate structure, the second sub-protective film is deposited on the top of the second gate structure, and the thickness of the second sub-protective film is greater than the thickness of the first sub-protective film; the first etching step etches part of the first protective film, including: etching part of the first sub-protective film and part of the second sub-protective film at the same time, so that neither the first sub-protective film nor the second sub-protective film is completely consumed.
[0009] In one embodiment, etching a fin structure between two adjacent gate structures to form a target groove includes: performing a second etching step to etch the fin structure between the two adjacent gate structures to a predetermined depth to form an initial groove; the opening width of the initial groove is equal to the distance between two adjacent first side walls; performing a third etching step to isotropically etch the initial groove to form a target groove with a smooth side wall surface; the maximum opening width of the target groove is greater than the opening width of the initial groove.
[0010] In one embodiment, the gate structure includes a gate layer, a first mask layer, and a second mask layer that are stacked; in the process of forming an initial groove, the first side wall is etched to a predetermined height; the predetermined height is higher than the height of the first mask layer by a first preset value, and the first preset value is greater than or equal to the first preset value.
[0011] In one embodiment, the fin-like structure includes a fin and a gate insulation layer covering the surface of the fin, a top surface of the gate insulation layer is provided with a first opening, the first opening exposes the top surface of the fin between two adjacent gate structures, an initial groove is formed by etching the exposed top surface of the fin, and a maximum recess depth of the target groove relative to the top surface of the gate insulation layer is less than or equal to a second preset value.
[0012] In one embodiment, etching byproducts are generated during the first etching step, and the method further includes: before performing the second etching step, performing a byproduct removal step to remove the etching byproducts and the remaining first protective film.
[0013] The second aspect of the present application provides a method for preparing a field effect transistor, characterized in that it includes: using the method for forming a groove in any of the above-mentioned embodiments to form a target groove in a fin structure between two adjacent gate structures; selectively growing a source and a drain in the target groove to form a source and a drain on both sides of the gate structure, respectively.
[0014] The third aspect of the present application provides a semiconductor process equipment, including a process chamber, an air intake assembly, an upper electrode assembly, a lower electrode assembly and a controller, the controller including at least one processor and at least one memory, the memory storing a computer program, and when the computer program is executed by the processor, a method of any of the above-mentioned embodiments is implemented.
[0015] The advantages or beneficial effects of the above technical solution include at least: by alternately performing the deposition step and the first etching step, a first protective film can be first formed on the top of the gate structure, and the first protective film covers the top surface of the first side wall, and a second protective film can be formed on the top of the fin structure, and the second protective film covers the top surface of the second side wall, and the thickness of the first protective film is greater than the thickness of the second protective film; after removing the second protective film, at least part of the second side wall and part of the first protective film are etched to ensure that the first protective film is not completely etched, so that the first protective film can protect the top surface of the first side wall during the etching of the second side wall, avoiding excessive loss of the height of the first side wall, and then after the target groove is formed, it is beneficial to ensure that the first side wall can effectively wrap the gate layer of the gate structure, avoiding defects in the gate layer of the gate structure during source and drain growth. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The accompanying drawings herein are incorporated into and constitute a part of the specification, illustrate embodiments consistent with the present application, and together with the specification are used to explain the principles of the present application. In addition, these drawings and text descriptions are not intended to limit the scope of the concept of the present application in any way, but to illustrate the concept of the present application for those skilled in the art by referring to specific embodiments.
[0017] Figure 1 FIG. 1 is a schematic flow chart of a method for forming a groove in the related art.
[0018] Figure 2 Shown is a schematic diagram of the three-dimensional structure of the film layer to be etched.
[0019] FIG. 3A to FIG. 3H It is a schematic diagram of the cross-sectional structure of each step in the process of forming a groove in the related technology.
[0020] Figure 4 FIG. 1 is a schematic diagram of a process of forming a groove according to an embodiment of the present application.
[0021] FIG. 5A to FIG. 5N Shown is a schematic cross-sectional structure diagram of each step in the process of forming a groove in the present application.
[0022] FIG. 6A to FIG. 6C Shown is a schematic diagram of the cross-sectional structure of the pattern-intensive area at each step in the process of forming the grooves in the present application.
[0023] Fig. 7A Shown is a schematic diagram of the cross-sectional structure of a film layer to be etched in the present application at a viewing angle in a sparsely patterned area.
[0024] Figure 7B Shown is a schematic cross-sectional structure diagram of another viewing angle in which the film layer to be etched of the present application is located in a sparsely patterned area.
[0025] Figure 7C Shown is a schematic diagram of the cross-sectional structure of a film layer to be etched in the present application at a viewing angle in a pattern-dense area.
[0026] Figure 8 Shown is a schematic structural diagram of a semiconductor process equipment according to an embodiment of the present application. DETAILED DESCRIPTION
[0027] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present application. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.
[0028] Figure 1 FIG. 1 is a schematic flow chart of a method for forming a groove in the related art. Figure 2 Shown is a schematic diagram of the three-dimensional structure of the film layer to be etched. FIG. 3A to FIG. 3H Shown is a schematic cross-sectional structure diagram of each step in the process of forming a groove in the related art.
[0029] like Figure 1 As shown, in the related art, the method for forming a groove includes the following steps S110 to S140.
[0030] Step S110, please refer to Figure 2 , Figure 3A and Figure 3B , a film layer 10 to be etched is provided, and a plurality of fin structures 12 and a plurality of gate structures 13 are arranged on one side surface of the film layer 10 to be etched; wherein the plurality of fin structures 12 are arranged at intervals, and the plurality of gate structures 13 are arranged across the plurality of fin structures 12, and the sidewalls of the gate structures 13 are provided with first sidewalls 14, and the sidewalls of the fin structures 12 are provided with second sidewalls 15, and the second sidewalls 15 are located between two adjacent gate structures 13. Figure 3A for Figure 2Schematic diagram of the cross-sectional structure along the cutting line A1-A2, Figure 3B for Figure 2 Schematic diagram of the cross-sectional structure along the cutting line B1-B2, Figure 2 The first side wall 14 and the second side wall 15 are omitted.
[0031] Step S120, please refer to Figure 3C and Figure 3D , performing a first etching step to remove the second spacer 15 , so that the fin structure 12 between two adjacent gate structures 13 is exposed.
[0032] Step S130, please refer to Figure 3E and Figure 3F , performing a second etching step to etch the fin structure 12 between two adjacent gate structures 13 to form an initial groove 12A.
[0033] Step S140, please refer to Figure 3G and Figure 3H , perform a third etching step to isotropically etch the initial groove 12A to form a target groove 12B with a smooth sidewall surface.
[0034] The inventor discovered during the implementation of the relevant technology that: Figure 3C and Figure 3D As shown, during the etching of the second sidewall 15, the first sidewall 14 of the gate structure 13 is etched at the same time, causing a loss in the height of the first sidewall 14, and as shown in FIG. Figure 3E and Figure 3F As shown, in the process of etching the fin structure 12 between two adjacent gate structures 13, the first side wall 14 of the gate structure 13 will also be etched simultaneously, causing the height of the first side wall 14 to be lost again, which will cause excessive loss of the height of the first side wall 14, resulting in the first side wall 14 being unable to wrap the gate layer 131 of the gate structure 13, and then the gate layer 131 of the gate structure 13 is prone to defects when the source and drain grow.
[0035] In view of this, the method for forming a groove, the method for preparing a field effect transistor and the process equipment of the embodiments of the present application can effectively solve the problem existing in the related technology that during the process of forming the groove, the first side wall is over-etched, resulting in the first side wall being unable to wrap the gate layer of the gate structure, which in turn causes the gate layer of the gate structure to be prone to defects during the subsequent source and drain growth.
[0036] Please also read Figure 2 , Figure 3A and Figure 3BThe method for forming a groove in the embodiment of the present application is applicable to a film layer 10 to be etched, wherein a plurality of fin structures 12 and a plurality of gate structures 13 are arranged on one side surface of the film layer 10 to be etched, wherein the plurality of fin structures 12 are arranged at intervals, wherein the plurality of gate structures 13 are arranged at intervals and straddle the plurality of fin structures 12, wherein the sidewalls of the gate structures 13 are provided with a first sidewall 14, wherein the sidewalls of the fin structures 12 are provided with a second sidewall 15, wherein the second sidewall 15 is located between two adjacent gate structures 13. Exemplarily, the film layer 10 to be etched includes a substrate 11, a plurality of fin structures 12 and a plurality of gate structures 13 located on one side surface of the substrate 11, wherein the plurality of fin structures 12 are arranged at intervals and all extend along a first direction D1, wherein the plurality of gate structures 13 are arranged at intervals and all extend along a second direction D2, so as to straddle the plurality of fin structures 12; wherein the first direction D1 and the second direction D2 are perpendicular to each other. The method for forming a groove in the embodiment of the present application is described in detail below in conjunction with the accompanying drawings.
[0037] Figure 4 FIG. 1 is a schematic flow chart of a method for forming a groove according to an embodiment of the present application.
[0038] like Figure 4 As shown, the method for forming a groove includes the following steps S210 to S220.
[0039] Step S210, please refer to FIG. 5A to FIG. 5H , alternately performing a deposition step and a first etching step, etching at least a portion of the second sidewall 15 to expose the fin structure 12 between two adjacent gate structures 13; wherein the deposition step is used to deposit a first protective film 16 on the top of the gate structure 13, and the first protective film 16 covers the top surface of the first sidewall 14, the deposition step is also used to deposit a second protective film 17 on the top of the fin structure 12, and the second protective film 17 covers the top surface of the second sidewall 15, the thickness of the first protective film 16 is greater than the thickness of the second protective film 17, and the first etching step is used to remove the second protective film 17, and at least etch a portion of the second sidewall 15 and a portion of the first protective film 16.
[0040] Please also refer to Figure 2 , Figure 3A and Figure 3BIn the film layer 10 to be etched, the gate structure 13 is arranged across the fin structure 12. This structure causes the top height of the fin structure 12 to be lower than the top height of the gate structure 13. It is not easy for plasma to pass through the gap between two adjacent gate structures 13 and reach the top of the fin structure 12, resulting in a high distribution density of plasma at the top of the gate structure 13 and an extremely low distribution density at the top of the fin structure 12. Therefore, when performing the deposition step, the thickness of the first protective film 16 deposited on the top of the gate structure 13 can be greater than the thickness of the second protective film 17 deposited on the top of the fin structure 12, resulting in a deposition loading effect.
[0041] In step S210, Figure 5A and Figure 5B As shown, by first performing a deposition step to generate a deposition loading effect, a first protective film 16 capable of covering the top surface of the first spacer 14 can be formed on the top of the gate structure 13, and a second protective film 17 capable of covering the top surface of the second spacer 15 can be formed on the top of the fin structure 12, and the thickness of the first protective film 16 is greater than the thickness of the second protective film 17; Figure 5C and Figure 5D As shown, the first etching step is then performed to remove the second protective film 17 and to at least partially etch the second side wall 15 and partially etch the first protective film 16, so that in the process of thinning the thickness of the second side wall 15, the first protective film 16 can protect the top of the first side wall 14 and avoid excessive loss of the height of the first side wall 14.
[0042] Step S220, please refer to Figure 5K to Figure 5N , the fin structure 12 between two adjacent gate structures 13 is etched to form a target groove 12B.
[0043] According to the above scheme, by alternately performing the deposition step and the first etching step, a first protective film 16 can be first formed on the top of the gate structure 13, and the first protective film 16 covers the top surface of the first sidewall 14, and a second protective film 17 is formed on the top of the fin structure 12, and the second protective film 17 covers the top surface of the second sidewall 15, and the thickness of the first protective film 16 is greater than the thickness of the second protective film 17. After removing the second protective film 17, at least a portion of the second sidewall 15 and a portion of the first protective film 16 are etched to ensure that the first protective film 16 is not completely etched, so that the first protective film 16 can protect the top surface of the first sidewall 14 during the etching of the second sidewall 15, thereby avoiding excessive loss of the height of the first sidewall 14, and further after forming the target groove 12B, it is beneficial to ensure that the first sidewall 14 can effectively wrap the gate layer 131 of the gate structure 13, thereby avoiding defects in the gate layer 131 of the gate structure 13 during source and drain growth.
[0044] In one embodiment, the deposition step and the first etching step are alternately performed to at least partially etch the second sidewall spacer 15 , including: alternately and cyclically performing the deposition step and the first etching step to etch the entire second sidewall spacer 15 to remove the second sidewall spacer 15 .
[0045] Next, a process of performing multiple deposition steps and the first etching step in an alternating cycle is described by taking an example.
[0046] For example, Figure 5A and Figure 5B As shown, after the first deposition step is performed, a first protective film 16 is formed on the top of the gate structure 13, and a second protective film 17 is formed on the top of the fin structure 12, and the thickness of the first protective film 16 is greater than the thickness of the second protective film 17; Figure 5C and Figure 5D As shown, during the first etching step, the first protective film 16 and the second protective film 17 are etched at the same time. After the second protective film 17 is removed, the second sidewall 15 located below the second protective film 17 is etched to a certain depth h1. Since the thickness of the first protective film 16 is greater than that of the second protective film 17, the first protective film 16 will not be completely etched after the second sidewall 15 is etched to a certain depth h1. In this way, during the process of removing the second protective film 17 and etching the second sidewall 15, the first protective film 16 can protect the first sidewall 14 and avoid the loss of the height of the first sidewall 14.
[0047] Similarly, if Figures 5E to 5H As shown, by alternately performing multiple deposition steps and the first etching step, the height of the second sidewall 15 can be gradually reduced until the second sidewall 15 is removed, and the first protective film 16 is not completely etched, so that the first protective film 16 can protect the first sidewall 14 during the process of removing the first sidewall 15. Figure 5E and Fig. 5F As shown in FIG. 1 , since the first protective film 16 is not completely etched after each alternating execution of the deposition step and the first etching step, after the i-th deposition step is executed, the thickness of the first protective film 16 is greater than the thickness of the i-1-th deposition step, and after the i-th first etching step is executed, the thickness of the first protective film 16 is also greater than the thickness after the i-1-th first etching step is executed, where i is an integer greater than 1; Fig. 5F As shown, since the height of the second sidewall 15 is shortened, the second protective film 17 will cover the top of the fin structure 12 and the top surface of the second sidewall 15. Figure 5G and Figure 5H When the second sidewall 15 is completely removed, the remaining portion of the first protection film 16 can still cover the top surface of the first sidewall 14 .
[0048] It should be noted that in step S210, the number of alternating cycles of the deposition step and the first etching step can be selected according to the height of the second sidewall 15, for example, 2 to 8 times (including the endpoint value) can be selected, and this embodiment of the present application does not limit this.
[0049] The above scheme can gradually remove the second side wall 15 by alternately executing multiple deposition steps and the first etching step without causing loss in the height of the first side wall 14; and this method of alternately executing the deposition step and the first etching step can also avoid the first protective film 16 blocking between two adjacent gate structures 13, which causes the plasma to be unable to reach the top of the fin structure 12, and is more conducive to the smooth progress of the process steps.
[0050] It should be noted that if Figure 3C and Figure 3D As shown, in order to ensure that the height of the first sidewall 14 can effectively wrap the gate layer 131 of the gate structure 13, the related technology can also perform the second etching step and the third etching step in sequence without completely removing the second sidewall 15. This method will result in that after the target groove 12B is formed, the second sidewall 15 is still not completely removed. The second sidewall 15 will cause the epitaxial growth in the target groove 12B to be unable to be performed, so it is necessary to further remove the remaining second sidewall 15, such as Figure 3G and Figure 3H As shown, however, in the process of removing the remaining second sidewall 15, the target groove 12B will continue to be etched, so that the maximum recess depth h4 of the target groove 12B is greater than the size required by the process, for example, greater than Compared with the related art, the method of the embodiment of the present application can completely remove the second sidewall 15 without losing the height of the first sidewall 14, which is beneficial for the height of the first sidewall 14 and the maximum groove depth h4 of the target groove 12B to meet the process requirements at the same time.
[0051] In one embodiment, the process conditions of the deposition step include that the reaction gas includes a fluorocarbon gas.
[0052] Exemplarily, the fluorocarbon gas may be any one of fluoromethane (CH3F), difluoromethane (CH2F2), octafluorocyclobutane (C4F8) and hexafluoro-2-butyne (C4F6). Preferably, when fluoromethane is selected as the fluorocarbon gas, its flow rate may be in the range of 50 sccm to 150 sccm (including the end values).
[0053] like Figure 5A and Figure 5BAs shown, in the deposition step, the reaction gas is selected as a fluorinated gas, so that the first protective film 16 deposited on the top of the gate structure 13 and the second protective film 17 deposited on the top of the fin structure 12 are both fluorinated films. Since the fluorinated film is easily removed by oxygen (O2), Figure 5C and Figure 5D As shown, in the first etching step, the second protective film 17 can be removed and the first protective film 16 can be thinned by adding oxygen, and this method does not require additional process steps. For example, if the first protective film 16 and the second protective film 17 are both oxide films or nitride films, it will make it difficult to remove the second protective film 17 and thin the first protective film 16, and additional process steps need to be added.
[0054] In one embodiment, Figure 5A and Figure 5B As shown, the process conditions of the deposition step also include the lower electrode power being 0W to control the non-directionality of the plasma, so that the amount of the deposition byproduct deposited on the top of the gate structure 13 is greater than the amount deposited on the top of the fin structure 12. By configuring the lower electrode power to be 0W, the plasma generated by the ionization of the carbon fluorine gas can be made non-directional, so that deposition is more likely to occur on the top of the gate structure 13, and it can be ensured that the amount of the deposition byproduct deposited on the top of the gate structure 13 is greater than the amount deposited on the top of the fin structure 12, thereby controlling the thickness of the first protective film 14 to be greater than the thickness of the second protective film 15. Among them, the deposition byproduct can be a carbon fluorine film.
[0055] Furthermore, the process conditions of the deposition step may also include: the pressure range of the process chamber is 10mTorr to 100mTorr (including the end value). The thickness of the deposited fluorocarbon film is directly proportional to the flow rate of the fluorocarbon gas and inversely proportional to the pressure of the process chamber, that is, the greater the flow rate of the fluorocarbon gas and the smaller the pressure of the process chamber, the thicker the fluorocarbon film. Therefore, by controlling the flow rate of the fluorocarbon gas and the pressure of the process chamber, the thickness of the first protective film 16 and the second protective film 17 can be controlled.
[0056] In addition, in the deposition step, the reaction gas may also include argon (Ar), and the flow rate of argon is in the range of 200sccm to 500sccm (including the endpoint values). Argon can act as a transport carrier and assist in ignition. The upper electrode power can be selected from 500W to 1000W (including the endpoint values) to control the ionization of carbon fluorine gases. The temperature range of the wafer carrier can be 40°C to 70°C. The radio frequency coil of the upper electrode assembly includes an inner coil and an outer coil, and the current ratio of the outer coil current to the total current of the inner and outer coils is in the range of 0.2 to 0.7 (including the endpoint values), and the total current is the sum of the current of the inner coil and the current of the outer coil. The process time range of the deposition step can be 8s to 20s (including the endpoint values).
[0057] In one embodiment, the process conditions of the first etching step include that the reaction gas includes a carbon-fluorine gas and oxygen.
[0058] Exemplarily, the flow rate of the fluorocarbon gas is in the range of 100 sccm to 200 sccm (including the end values), and the fluorocarbon gas includes but is not limited to fluoromethane. The flow rate of oxygen is in the range of 5 sccm to 50 sccm (including the end values).
[0059] In this embodiment, if Figure 5A and Figure 5B As shown, the first protective film 16 and the second protective film 17 can both be made of fluorocarbon films, and the materials of the first sidewall 14 and the second sidewall 15 can both be made of silicon nitride (SiN). Since the fluorocarbon film has the characteristic of being easily removed by oxygen, and the thickness of the first protective film 16 is greater than that of the second protective film 17, as shown in FIG. Figure 5C and Figure 5D As shown, in the first etching step, oxygen is selected as the reaction gas to first remove the second protective film 17 and then continue to etch the second side wall 15 to thin the second side wall 15, and at the same time thin the first protective film 16 without completely etching the first protective film 16, so that the remaining first protective film 16 can protect the first side wall 14 from being etched.
[0060] In one embodiment, the process conditions of the first etching step further include at least one of the following:
[0061] The pressure range of the process chamber is 50mTorr to 100mTorr (including the end values);
[0062] The power range of the lower electrode is 50W to 200W (including the end points).
[0063] In this application, if Figure 5C and Figure 5D As shown, the fin structure 12 includes a fin 121 and a gate insulating layer 122 covering the surface of the fin 121. The material of the fin 121 can be single crystal silicon, and the material of the gate insulating layer 122 can be silicon dioxide (SiO2). By configuring the pressure of the process chamber to be between 50mTorr and 100mTorr, it can be ensured that the oxygen in the first etching step is added to the process chamber under high chamber pressure conditions, which is more conducive to improving the selectivity of the gate insulating layer 122, thereby reducing damage to the gate insulating layer 122 during the etching of the second sidewall 15. In addition, by configuring the range of the lower electrode power to be between 50W and 200W, the lower electrode power in the first etching step can be higher, so that the etching is carried out downward, and the directionality of the etching can be ensured.
[0064] Furthermore, the process conditions of the first etching step may also include: the reaction gas includes argon, and the flow range of argon is 200mTorr~500mTorr (including endpoint values); the upper electrode power range is 500W~1000W (including endpoint values); the process time range is 8s~20s (including endpoint values).
[0065] In one embodiment, please refer to Figure 2 , Figure 3A and Fig. 6A The film layer 10 to be etched has a sparse pattern area and a dense pattern area, wherein: Figure 3A is a schematic diagram of the cross-sectional structure of the film layer 10 to be etched in the sparsely patterned area, Fig. 6A Schematic diagram of the cross-sectional structure of the film layer 10 to be etched in the pattern-dense area. The gate structure 13 includes a first gate structure 13A located in the pattern-sparse area and a second gate structure 13B located in the pattern-dense area. The density of the second gate structure 13B in the pattern-dense area is higher than that of the first gate structure 13A in the pattern-sparse area. In other words, the distance between two adjacent second gate structures 13B is smaller than the distance between two adjacent first gate structures 13A.
[0066] like Figure 5A and Figure 6B As shown, the first protection film 16 includes a first sub-protection film 161 and a second sub-protection film 162, the first sub-protection film 161 is deposited on the top of the first gate structure 13A, the second sub-protection film 162 is deposited on the top of the second gate structure 13B, and the thickness of the second sub-protection film 162 is less than the thickness of the first sub-protection film 161. Since the density of the second gate structure 13B is higher than that of the first gate structure 13A, the reaction gas distributed to the top of the second gate structure 13B per unit volume is less than the reaction gas distributed to the top of the first gate structure 13A, resulting in the thickness of the formed second sub-protection film 162 being less than the thickness of the first sub-protection film 161.
[0067] like Figure 5C and Figure 6C As shown, the first etching step of etching part of the first protection film 16 includes: etching part of the first sub-protection film 161 and part of the second sub-protection film 162 at the same time, so that neither the first sub-protection film 161 nor the second sub-protection film 162 is completely consumed.
[0068] Exemplarily, the graphic dense area may be a static random access memory (SRAM) area, and the graphic sparse area may be a test key area. In the related art, in the process of forming the target groove 12B, factors such as the graphic size, sparseness and mask opening position of different areas may cause differences in the distribution of reaction byproducts. For example, the distance between two adjacent second gate structures 13B in the SRAM area is smaller, so that the number of second gate structures 13B per unit area is greater, and thus the reaction byproducts evenly distributed on the top of each second gate structure 13B are less, and the first sidewall 14 set on the sidewall of the second gate structure 13B cannot be effectively protected. This micro-load effect causes the first sidewall 14 of the second gate structure 13B in the SRAM area to lose more height, making the gate layer 131 of the second gate structure 13B in the SRAM area more prone to defects during subsequent source and drain generation.
[0069] In this embodiment, if Figure 5A and Figure 6B As shown, by first performing a deposition step, a first sub-protection film 161 is deposited on the top of the first gate structure 13A, and a second sub-protection film 162 is deposited on the top of the second gate structure 13B, and the thickness of the first sub-protection film 161 is greater than the thickness of the second sub-protection film 162; Figure 5C , Figure 5D and Figure 6C As shown, part of the first sub-protective film 161 and part of the second sub-protective film 162 are etched simultaneously during the execution of the first etching step, and the first sub-protective film 161 and the second sub-protective film 162 are not completely consumed. Then, in the process of removing the second side wall 15, it can be ensured that the second sub-protective film 162 can cover the first side wall 14 on the side wall of the second gate structure 13B, and the first sub-protective film 161 can cover the first side wall 14 on the side wall of the first gate structure 13A, thereby protecting the first side wall 14 in the pattern-dense area and the pattern-sparse area, avoiding the first side wall 14 in the pattern-dense area from being unable to be effectively protected due to uneven distribution of reaction by-products, and helping to prevent defects in the gate layer 131 of the second gate structure 13B in the pattern-dense area during subsequent source and drain generation.
[0070] In one embodiment, please refer to FIG. 5I to FIG. 5N , etching the fin structure 12 between two adjacent gate structures 13 to form a target groove 12B, including the following steps S221 to S222.
[0071] Step S221: FIG. 5I to FIG. 5L, a second etching step is performed to etch the fin structure 12 between two adjacent gate structures 13 to a predetermined depth h2, forming an initial groove 12A; the opening width W1 of the initial groove 12A is equal to the distance between two adjacent first sidewalls 14. The predetermined depth h2 is the etching depth h2 of the initial groove 12A.
[0072] For example, please refer to Fig.5I and Figure 5J The fin structure 12 includes a fin portion 121 and a gate insulating layer 122 covering a surface of the fin portion 121. Step S221 may include:
[0073] Please also read Figure 5K and Figure 5L , performing a first pre-etching step to form a first opening 122A in the gate insulating layer 122 , wherein the first opening 122A is used to expose the top surface of the fin 121 between two adjacent gate structures 13 ;
[0074] A first main etching step is performed to etch the fin 121 between two adjacent gate structures 13 to a predetermined depth h2 to form an initial groove 12A.
[0075] The reaction gas of the first pre-etching step may be carbon tetrafluoride (CF4). The process conditions of the first main etching step include: the upper electrode power range is 400W to 900W (including the end value), the lower electrode power range is 200W to 600W (including the end value), the pulse frequency of the lower electrode power is 100Hz to 200Hz (including the end value), the pulse duty ratio of the lower electrode power ranges from 20% to 60% (including the end value), the pressure range of the process chamber is 5mTorr to 30mTorr (including the end value), the etching gas includes hydrogen bromide (HBr) and oxygen, the flow rates of hydrogen bromide and oxygen are both 200sccm to 600sccm, the temperature range of the wafer carrier is 40℃ to 70℃, and the ratio of the current of the outer coil in the RF coil to the total current of the inner and outer coils ranges from 0.2 to 0.5 (including the end value). In addition, the lower electrode power signal adopts a synchronous pulse mode. Compared with the continuous pulse mode, the synchronous pulse mode of the lower electrode power signal makes the etching more uniform and stable, which is beneficial to the basically consistent etching depth of the initial groove 12A at different positions, and is more helpful to timely remove the etching by-products generated during the etching process, which can effectively alleviate the load effect.
[0076] Step S222, please refer to Figure 5M and Figure 5N , perform a third etching step to isotropically etch the initial groove 12A so that the initial groove 12A forms a target groove 12B with a smooth sidewall surface; the maximum opening width W2 of the target groove 12B is greater than the opening width W1 of the initial groove 12A.
[0077] Exemplarily, the process conditions of the third etching step include: the pressure range of the process chamber is 100mTorr to 500mTorr (including the end value), the upper electrode power range is 200W to 800W (including the end value), the etching gas includes nitrogen trifluoride (NF3) and hydrogen (H2), the flow rate range of nitrogen trifluoride and hydrogen is 20sccm to 60sccm, and the flow rate of hydrogen is greater than 1.5 times the flow rate of nitrogen trifluoride, and the auxiliary gas includes helium (He) and argon (Ar), and the flow rate of helium and argon is 200sccm to 500sccm. Among them, by selecting the pressure of the process chamber between 100mTorr and 500mTorr, the third etching step can be performed at a higher chamber pressure, which is more conducive to chemical etching, and the selectivity of the gate insulating layer 122 and the first sidewall 14 is improved, and the gate insulating layer 122 and the first sidewall 14 are etched. The upper electrode power is proportional to the etching rate. The higher the upper electrode power is, the faster the etching rate is. By selecting the upper electrode power between 200W and 800W, the etching gas can be controlled to etch the fin 121 at a suitable etching rate. The flow rate of nitrogen trifluoride is also proportional to the etching rate. The larger the flow rate of carbon trifluoride is, the faster the etching rate is. By selecting the flow rate of nitrogen trifluoride between 20sccm and 60sccm, the etching gas can be controlled to etch the fin 121 at a suitable etching rate. By selecting the flow rate of hydrogen between 20sccm and 60sccm, which is greater than 1.5 times the flow rate of nitrogen trifluoride, it is beneficial to control the smoothness and selectivity of the side wall surface of the target groove 12B, avoid more longitudinal etching of the target groove 12B, and make the etching depth h4 of the target groove 12B slightly greater than the etching depth h2 of the initial target groove 12A. Furthermore, in the third etching step, helium is used as a dilution gas for adjusting the uniformity of etching; and argon acts as a dilution gas and a cleaning gas.
[0078] The above scheme first performs the second etching step to etch the fin structure 12 between two adjacent gate structures 13 to form an initial groove 12A, and then performs the third etching step to isotropically etch the target groove 12B, so that the maximum opening width W2 of the target groove 12B is greater than the opening width W1 of the initial groove 12A. Since the opening width W1 of the initial groove 12A is greater than the distance between the two adjacent first side walls 14, it can be ensured that the maximum opening width W2 of the target groove 12B is greater than the distance between the two adjacent first side walls 14, thereby reducing the channel length between the two adjacent target grooves 12B, which helps to improve device performance and make the side wall surface of the target groove 12B smooth, which is more conducive to meeting the subsequent source and drain growth process requirements.
[0079] In one embodiment, please refer to Fig.5I The gate structure 13 includes a gate layer 131, a first mask layer 132, and a second mask layer 133 which are stacked. The gate layer 131 may be made of polysilicon, the first mask layer 132 may be made of silicon nitride, and the second mask layer 133 may be made of silicon dioxide. Preferably, the top surface of the first sidewall 14 is flush with the top surface of the second mask layer 133.
[0080] like Figure 5K and Figure 5L In the process of forming the initial groove 12A, the first sidewall 14 is etched to a predetermined height h3; the predetermined height h3 is higher than the height of the first mask layer 132 by a first preset value k1, and the first preset value k1 is greater than or equal to
[0081] Optionally, the first preset value k1 can be selected and adjusted according to actual needs. For example, the first preset value k1 can be It can also be As long as the first preset value k1 is greater than or equal to That's it.
[0082] Please also read Figure 5M , the top corner position 14A of the first sidewall 14 is very easy to be damaged. If the height of the first sidewall 14 is low, the top of the gate layer 131 is easily exposed due to the damage of the top corner position 14A of the first sidewall 14, which will cause defects in the top of the gate layer 131 during the growth of the source and drain. In this embodiment, the predetermined height h3 to which the first sidewall 14 is etched is set to be higher than the height of the first mask layer 132 by a first preset value k1, and the first preset value k1 is greater than or equal to It can be ensured that the height of the first spacer 14 can effectively wrap the top of the gate layer 131, thereby preventing defects from being generated on the top of the gate layer 131 during the growth of the source and drain.
[0083] In one embodiment, Figure 5M and Figure 5N As shown, the fin-like structure 12 includes a fin 121 and a gate insulating layer 122 covering the surface of the fin 121, and a first opening 122A is provided on the top surface of the gate insulating layer 122. The first opening 122A exposes the top surface of the fin 121 between two adjacent gate structures 13. The initial groove 12A is formed by etching the exposed top surface of the fin 121, and the maximum recess depth h4 of the target groove 12B relative to the gate insulating layer 122 is less than or equal to a second preset value.
[0084] For example, Figure 5LAs shown, the first opening 122A can be formed in the second etching step. For example, the second etching step includes a pre-etching step and a main etching step performed in sequence. The pre-etching step is used to etch the top surface of the gate insulating layer 122 between two adjacent gate structures 13 to form the first opening 122A, so that the first opening 122A can expose the top surface of the fin 121 between the two gate structures 13. Figure 5K and Figure 5L As shown, the main etching step is used to etch the top surface of the fin 121 exposed by the first opening 122A to a predetermined depth h2 to form an initial groove 12A, and the initial groove 12A is located between the two side walls of the gate insulating layer 122. Figure 5M and Figure 5N As shown, since the target groove 12B is formed by etching the initial groove 12A, the target groove 12B is also located between two sidewalls of the gate insulating layer 122 .
[0085] like Figure 3H As shown, in actual applications, during the subsequent source and drain growth process, a cubic crystal will be epitaxially grown, and the diagonal size of the crystal is approximately If the maximum recess depth h4 of the target groove 12B relative to the gate insulating layer 122 is greater than That is, the second preset value is Then the maximum depression depth h4 of the target groove 12B is likely to exceed half r of the diagonal dimension of the crystal, so that the two side walls of the gate insulating layer 122 will block the epitaxial growth of the crystal, resulting in the crystal being unable to grow. In this embodiment, by selecting the maximum depression depth h4 between the target groove 12B and the top surface of the gate insulating layer 122 to be less than or equal to The epitaxial growth of the sidewall barrier material of the gate insulating layer 122 can be avoided, which is beneficial to the normal growth of the subsequent source and drain.
[0086] In one embodiment, etching byproducts are generated during the execution of the first etching step, and the method further includes: Figure 5G and Figure 5J Before performing the second etching step, a byproduct removal step is performed to remove the etching byproducts and the remaining first protective film 16.
[0087] For example, Fig. 5FAs shown, during the first etching step, fluoromethane (CH3F) is used as the etching gas for etching the second sidewall 17. Since the material of the second sidewall 17 is silicon nitride (SiN), in addition to silicon tetrafluoride (SiF4), nitrogen trifluoride (NF3), ammonia (NH3) and nitrogen (N2) produced during the etching process, fluoromethane will also decompose into hydrocarbon (CHx) groups under ionization. The etching byproducts produced by the reaction of hydrocarbon groups with silicon nitride are CHN polymers. By adding oxygen in the byproduct removal step, the oxygen ions produced by the ionization of oxygen can react with the etching byproducts to generate gaseous substances such as carbon dioxide (CO2) and water vapor (HO2), which are finally extracted from the process chamber as waste; the oxygen ions can also remove the remaining first protective film 16. In this way, the top of the gate structure 13 and the first sidewall 14 can be completely exposed and not covered by the etching byproducts, and the surface of the fin structure 12 can be not covered by the etching byproducts.
[0088] In addition, other process conditions of the by-product removal step include: the upper electrode power range is 100W~400W (including endpoint values), the lower electrode power is 0W, the pressure of the process chamber is 5mTorr~30mTorr (including endpoint values), the oxygen flow rate range is 50sccm~300sccm (including endpoint values), the temperature of the wafer carrier is 40℃~70℃ (including endpoint values), and the ratio of the current of the outer coil of the RF coil to the sum of the currents of the inner and outer coils is in the range of 0.2~0.7 (including endpoint values).
[0089] In one embodiment, Figure 2 , Fig. 7A , Figure 7B and Figure 7C As shown, the film layer 10 to be etched further includes an interlayer dielectric layer 18 and an isolation dielectric layer 19. The interlayer dielectric layer 18 is located between the substrate 11 and the gate insulating layer 122 and between two adjacent fins 121. The isolation dielectric layer 19 covers the surface of the gate insulating layer 122 on the side away from the substrate 11 and the surface of the gate structure 13. By etching the isolation dielectric layer 19 to cover the top surface of the gate structure 13, the top surface of the gate insulating layer 122 and the portion of the plane on the side of the gate insulating layer 122 away from the interlayer dielectric layer 18, the isolation dielectric layer 19 after etching can form a first sidewall 14 on the sidewall of the gate structure 13 and a second sidewall 15 on the sidewall of the fin structure 12. It should be noted that since the materials of the gate insulating layer 122 and the interlayer dielectric layer 18 can both be silicon dioxide, the contact surface between the gate insulating layer 122 and the interlayer dielectric layer 18 is not shown in the cross-sectional structure drawing.
[0090] The embodiment of the present application further provides a method for preparing a field effect transistor, comprising the following steps S310 to S320.
[0091] Step S310, please refer to FIG. 5A to FIG. 5N , using any of the above-mentioned methods for forming a groove, a target groove 12B is formed in the fin structure 12 between two adjacent gate structures 13 .
[0092] Step S320 , selectively growing a source and a drain in the target groove 12B to form a source and a drain on both sides of the gate structure 13 , respectively.
[0093] Exemplarily, selectively growing a source and a drain in the target groove 12B includes: selectively growing silicon germanium (SiGe) epitaxially or silicon phosphide (SiP) epitaxially in the target groove 12B to form a source and a drain on both sides of the gate structure 13, respectively. The silicon germanium material is an N-type material, and the silicon phosphide material is a P-type material. The field effect transistor may be a fin field effect transistor. The type of the field effect transistor may be a P-type metal oxide semiconductor (Positive Channel Metal Oxide Semiconductor, referred to as PMOS) transistor and an N-type metal oxide semiconductor (Negative Channel Metal Oxide Semiconductor, referred to as NMOS) transistor.
[0094] The specific structure of the field effect transistor refers to the above embodiments. Since the method for preparing the field effect transistor adopts all the technical solutions of all the above embodiments, it at least has all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0095] Figure 8 Shown is a schematic structural diagram of a semiconductor process equipment according to an embodiment of the present application.
[0096] like Figure 8 As shown, the semiconductor process equipment 200 may include a process chamber 20, an inlet assembly 20A, an upper electrode assembly 20B and a lower electrode assembly 20C, a pumping assembly 20D and a controller ( Figure 8 The controller includes at least one processor and at least one memory, wherein a computer program is stored in the memory, and when the computer program is executed by the processor, the method of any one of the above embodiments is implemented.
[0097] Exemplarily, the controller can be a host computer or a slave computer. The controller can control the valve opening of the air inlet component 20A to introduce the corresponding process gas into the process chamber 20; the controller can also control the opening and closing degree of the valve of the air inlet component 20A to control the flow rate of the process gas. The controller can also control the exhaust component 20D to exhaust the interior of the process chamber 20, such as controlling the valve opening degree or the exhaust pump speed of the exhaust component 20D, to control the pressure inside the process chamber 20, discharge reaction byproducts, etc.
[0098] The upper electrode assembly 20B may include an RF coil 21, an upper RF power source 23, and an upper matcher 25. The controller is also used to control the upper RF power source 23 to provide RF power to the RF coil 21 through the upper matcher 25, so that the RF coil 21 excites the process gas inside the process chamber 20 to generate plasma P. The RF coil 21 may include an inner coil and an outer coil (attached Figure 8 not shown).
[0099] The lower electrode assembly 20C may include a wafer carrier 22, a lower RF power supply 24, and a lower matcher 26. The controller is also used to control the lower RF power supply 24 to provide RF power to the wafer carrier 22 through the lower matcher 26 to provide RF bias. The wafer carrier 22 may be, for example, an electrostatic chuck, a mechanical chuck, or a vacuum adsorption chuck.
[0100] The semiconductor process equipment 200 of the embodiment of the present application may be an inductively coupled plasma (ICP) device. The embodiment of the present application does not limit the type of the semiconductor process equipment 200.
[0101] In addition, in this application, unless otherwise clearly specified and limited, the terms "connected", "connected", "stacked" and the like should be understood in a broad sense, for example, it can be fixedly connected, detachably connected, or integrated; it can be directly connected, or indirectly connected through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0102] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, etc. made within the spirit and principles of the present application shall be included in the protection scope of the present application.
Claims
1. A method for forming a groove, characterized in that: Applied to a film layer to be etched, a plurality of fin structures and a plurality of gate structures are arranged on the film layer to be etched, the plurality of fin structures are arranged at intervals, the plurality of gate structures are arranged at intervals and straddle the plurality of fin structures, the sidewalls of the gate structures are provided with a first sidewall, the sidewalls of the fin structures are provided with a second sidewall, and the second sidewall is located between two adjacent gate structures; the method comprises: Alternately performing a deposition step and a first etching step, etching at least a portion of the second sidewall to expose the fin structure between two adjacent gate structures; wherein the deposition step is used to deposit a first protective film on the top of the gate structure, and the first protective film covers the top surface of the first sidewall, and is also used to deposit a second protective film on the top of the fin structure, and the second protective film covers the top surface of the second sidewall, the thickness of the first protective film is greater than the thickness of the second protective film, and the first etching step is used to remove the second protective film, and at least etch a portion of the second sidewall and a portion of the first protective film; The fin structure between two adjacent gate structures is etched to form a target groove.
2. The method according to claim 1, characterized in that The alternately performing the deposition step and the first etching step to at least partially etch the second sidewall includes: alternately and cyclically performing the deposition step and the first etching step to etch the entire second sidewall to remove the second sidewall.
3. The method according to claim 1, characterized in that The process conditions of the deposition step further include a lower electrode power of 0 W to control the non-directionality of plasma so that the amount of deposition byproducts deposited on the top of the gate structure is greater than that deposited on the top of the fin structure.
4. The method according to claim 1, characterized in that: The film layer to be etched has a pattern-dense area and a pattern-sparse area, the gate structure includes a first gate structure located in the pattern-sparse area and a second gate structure located in the pattern-dense area, the first protection film includes a first sub-protection film and a second sub-protection film, the first sub-protection film is deposited on the top of the first gate structure, the second sub-protection film is deposited on the top of the second gate structure, and the thickness of the second sub-protection film is less than the thickness of the first sub-protection film; The first etching step of etching a portion of the first protective film includes: etching a portion of the first sub-protective film and a portion of the second sub-protective film simultaneously, so that neither the first sub-protective film nor the second sub-protective film is completely consumed.
5. The method according to claim 1, characterized in that Etching the fin structure between two adjacent gate structures to form a target groove, comprising: Performing a second etching step to etch the fin structure between two adjacent gate structures to a predetermined depth to form an initial groove; the opening width of the initial groove is equal to the distance between two adjacent first sidewalls; A third etching step is performed to isotropically etch the initial groove, so that the initial groove forms the target groove with a smooth sidewall surface; the maximum opening width of the target groove is greater than the opening width of the initial groove.
6. The method according to claim 5, characterized in that The gate structure includes a gate layer, a first mask layer and a second mask layer which are stacked; in the process of forming the initial groove, the first sidewall is etched to a predetermined height; the predetermined height is higher than the height of the first mask layer by a first preset value.
7. The method according to claim 5, characterized in that The fin-shaped structure includes a fin and a gate insulation layer covering the surface of the fin, the top surface of the gate insulation layer is provided with a first opening, the first opening exposes the top surface of the fin between two adjacent gate structures, the initial groove is formed by etching the exposed top surface of the fin, and the maximum depression depth of the target groove relative to the top surface of the gate insulation layer is less than or equal to a second preset value.
8. The method according to claim 5, characterized in that Etching byproducts are generated during the execution of the first etching step. The method further includes: before executing the second etching step, executing a byproduct removal step to remove the etching byproducts and the remaining first protective film.
9. A method for preparing a field effect transistor, characterized in that: include: Using the method for forming a groove according to any one of claims 1 to 8, forming a target groove in the fin structure between two adjacent gate structures; A source and a drain are selectively grown in the target groove to form a source and a drain on both sides of the gate structure, respectively.
10. A semiconductor process equipment, comprising a process chamber, an air inlet assembly, an upper electrode assembly, a lower electrode assembly and a controller, characterized in that: The controller comprises at least one processor and at least one memory, wherein a computer program is stored in the memory, and when the computer program is executed by the processor, the method according to any one of claims 1 to 9 is implemented.