Composite positive electrode active material, preparation method, composite positive electrode and battery

By adopting double-layer coating technology on manganese-based cathode materials, using conductive polymers and halide solid electrolytes, the problem of capacity fading of manganese-based materials at high temperatures is solved, the cycle stability and rate performance of the battery are improved, and the battery life is extended. Battery life.

CN118763206APending Publication Date: 2024-10-11清陶(乌海)能源科技有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411105224.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The charge and discharge capacity of manganese-based cathode materials decreases in high-temperature environments, mainly due to the Jahn-Teller effect caused by Mn3+ and the boundary side reaction between the electrode material and the electrolyte, which causes the dissolution of manganese element, destroys the SEI film of the negative electrode, and affects the battery cycle performance.

Method used

Using double-layer coating technology, conductive polymers such as polypyridine or polyaniline are used as the first coating layer, and halide solid electrolytes such as Li2ZrCl6 are used as the second coating layer. They are first wet-coated and then dry-coated to form The composite cathode active material enhances the blocking effect on manganese ions and improves the transmission of lithium ions.

Benefits of technology

It effectively blocks the contact between the electrolyte and the positive active material, improves the cycle stability and rate performance of the battery, reduces the deposition of manganese ions on the negative electrode side, extends the battery life and maintains a high 2C discharge capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004990556710000121
    Figure BDA0004990556710000121
  • Figure BDA0004990556710000131
    Figure BDA0004990556710000131
Patent Text Reader

Abstract

The invention provides a composite positive electrode active material, a preparation method, a composite positive electrode and a battery, and relates to the technical field of lithium ion batteries. The composite positive electrode active material comprises a positive electrode active material, a first coating layer and a second coating layer; the surfaces of particles of the positive electrode active material are sequentially coated with the first coating layer and the second coating layer; the positive electrode active material is selected from at least one of lithium manganate, a lithium-rich manganese-based positive electrode material and nickel cobalt lithium manganate; the first coating layer comprises a first coating material, and the first coating material comprises a conductive polymer; and the second coating layer comprises a second coating material, and the second coating material comprises halide solid electrolyte. Dual coating of the polymer and the halide solid electrolyte is realized by adopting a coating mode of firstly carrying out wet coating and then carrying out dry coating. The battery prepared from the composite positive electrode active material is long in service life and high in 2C discharge capacity retention rate, and generation and deposition of divalent manganese ions can be effectively inhibited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a composite positive electrode active material, a preparation method, a composite positive electrode and a battery. Background Art

[0002] As electronic information products become increasingly lighter, thinner and miniaturized, and the demand for batteries for power systems such as new energy vehicles continues to expand, the commonly used positive electrode materials for lithium-ion batteries today include lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, and nickel-cobalt-manganese ternary materials. Among them, lithium cobalt oxide has a higher cost, poor thermal stability, and lower safety. The energy density of lithium iron phosphate is relatively small. Manganese-based positive electrode materials such as lithium manganese oxide, nickel-cobalt-manganese ternary materials, and lithium-rich manganese-based positive electrode materials have significant advantages such as low cost, abundant resources, non-toxicity, and high energy density. However, under high temperature conditions, the charge and discharge capacity of manganese-based positive electrode materials decreases rapidly, becoming the main disadvantage restricting its development. Related studies have shown that the main reason for the capacity decay of manganese-based materials is Mn 3+ The resulting Jahn-Teller effect and the dissolution of manganese caused by the boundary side reaction between the electrode material and the electrolyte. HF in the electrolyte will cause the trivalent manganese ions in the positive electrode active material to undergo a disproportionation reaction to generate divalent manganese ions and tetravalent manganese ions. The divalent manganese ions migrate to the negative electrode with the electrolyte and deposit at the negative electrode, continuously destroying the SEI film on the negative electrode side. The regeneration of the SEI film requires lithium ions, resulting in a decrease in the cycle performance of the battery. In the prior art, the electrolyte and the manganese-based positive electrode active material are isolated by coating. The coating causes the electrolyte to be unable to infiltrate the positive electrode well, thereby affecting the transmission of lithium ions and the rate performance of the battery. Moreover, the single-layer coating has limited effect on preventing the dissolution of divalent manganese ions.

[0003] Therefore, a composite positive electrode active material and a composite positive electrode are urgently needed to solve the problems existing in the prior art. Summary of the invention

[0004] In view of the above problems, the present invention provides a composite positive electrode active material, including a positive electrode active material and a first coating layer and a second coating layer. By selecting a conductive polymer as the first coating layer material, selecting a halide solid electrolyte as the second coating layer material, and optimizing the preparation process, the cycle stability of the battery is improved without affecting the battery rate performance, and the deposition of manganese ions on the negative electrode side can be effectively reduced.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] In a first aspect, the present invention provides a composite positive electrode active material, comprising a positive electrode active material, a first coating layer and a second coating layer;

[0007] The surface of the particles of the positive electrode active material is sequentially coated with the first coating layer and the second coating layer;

[0008] The positive electrode active material is selected from at least one of lithium manganese oxide, lithium-rich manganese-based positive electrode materials, and nickel-cobalt lithium manganese oxide;

[0009] The first coating layer includes a first coating material, and the first coating material includes a conductive polymer;

[0010] The second coating layer includes a second coating material, and the second coating material includes a halide solid electrolyte.

[0011] In some embodiments, the conductive polymer is selected from at least one of polypyridine and polyaniline.

[0012] In some embodiments, the general formula of the halide solid electrolyte is Li x MCl y , where 1≤x≤4, 4≤y≤8; M is a metal element.

[0013] In some embodiments, M is selected from at least one of V, Cr, Mn, Zn, Cd, Fe, Pb, In, Y, Al, Sc, La, Lu, Ga, Zr, Hf, and Mg.

[0014] In some of the embodiments, the mass ratio of the conductive polymer monomer to the positive electrode active material is (1-10): (90-99).

[0015] In some embodiments, the positive electrode active material is coated with the first coating layer to form a first positive electrode active material; the mass ratio of the first positive electrode active material to the second coating layer is (95-99):(1-5).

[0016] In a second aspect, the present invention provides a method for preparing a composite positive electrode active material, comprising the following steps:

[0017] S1: The positive electrode active material is mixed with water, the pH is adjusted to a first pH value, and a monomer of a conductive polymer is added to obtain a solution A; the oxidant is mixed with water, and the pH is adjusted to a second pH value to obtain a solution B; at a temperature of -5-5°C, solution A and solution B are mixed and reacted to obtain a first positive electrode active material;

[0018] S2: The first positive electrode active material prepared in S1 is mixed with the second coating material to form a second coating layer to obtain a composite positive electrode active material.

[0019] In some embodiments, the first pH value is 2-4.

[0020] In some embodiments, the second pH value is 2-4.

[0021] In some embodiments, the reaction time in step S1 is 2-4 hours.

[0022] In some embodiments, in step S1, an acidic medium is used to adjust the pH, and the acidic medium is selected from at least one of hydrochloric acid and sulfuric acid.

[0023] In some preferred embodiments, the acidic medium is hydrochloric acid.

[0024] In some embodiments, the concentration of the acidic medium is 0.8-1.5 mol / L; preferably, the concentration of the acidic medium is 0.9-1.2 mol / L.

[0025] In some embodiments, in step S1, the oxidant is selected from at least one of ammonium persulfate, hydrogen peroxide, sodium vanadate, and potassium dichromate.

[0026] In some embodiments, the mixing method in step S2 is ball milling, the ball milling speed is 150-350 rpm, and the ball milling time is 1-10 h.

[0027] In a third aspect, the present invention provides a composite positive electrode, comprising the composite positive electrode active material as described in the first aspect or the composite positive electrode active material prepared by the preparation method as described in the second aspect.

[0028] In some embodiments, in the composite positive electrode, the mass proportion of the composite positive electrode active material is 78%-99%.

[0029] In a fourth aspect, the present invention provides a battery comprising a composite positive electrode prepared from the composite positive electrode active material described above, an electrolyte and a negative electrode.

[0030] In some embodiments, the method for preparing the composite positive electrode comprises the following steps:

[0031] The composite positive electrode active material is rolled to obtain a composite positive electrode film, and the composite positive electrode film is combined with a collective flow roller to obtain a composite positive electrode.

[0032] In some embodiments, the rolling pressure is 550-650 kPa, the rolling time is 3-10 min, and the rolling temperature is 55-65°C.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. The coating layer formed on the surface of the positive electrode active material can effectively block the contact between the electrolyte and the positive electrode active material, effectively prevent the occurrence of side reactions between the positive electrode and the electrolyte, and effectively improve the cycle performance of the battery.

[0035] Compared with single-layer coating, double-layer coating has better barrier effect.

[0036] 2. The coating material is polypyridine and polyaniline, which can improve the conductivity of the positive electrode material, thereby reducing the internal resistance of the battery. At the same time, it can effectively improve the transmission of lithium ions in the coating layer, and the coating has less impact on the rate performance of the battery; polypyridine and polyaniline can be combined with Mn 2+ Complexation occurs, enhancing the first coating layer's resistance to Mn 2+ The blocking effect;

[0037] 4. Halide solid electrolytes have high room temperature conductivity (≥1×10 -3 S / cm), the selection of halide solid electrolyte can improve the cycle stability of the material without sacrificing the discharge capacity and rate performance of the material;

[0038] 5. The present invention also provides a method for preparing a composite positive electrode active material, which adopts a coating method of first wet coating and then dry coating to achieve double coating of polymer and halide solid electrolyte. The battery prepared with the prepared composite positive electrode active material has a long life and a high 2C discharge capacity retention rate. DETAILED DESCRIPTION

[0039] References to embodiments of the present application will now be provided in detail, one or more examples of which are described below. Each example is provided as an explanation rather than a limitation of the present application. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present application without departing from the scope or spirit of the present application. For example, a feature described or described as part of one embodiment may be used in another embodiment to produce a further embodiment.

[0040] Therefore, it is intended that the present application covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features and aspects of the present application are disclosed in or are apparent from the following detailed description. It will be appreciated by those of ordinary skill in the art that this discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the present application.

[0041] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0042] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0043] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0044] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0045] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, it is mentioned that the method may also include step (c), which means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0046] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0047] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0048] Manganese-based positive electrode active materials have attracted widespread attention due to their low price and high capacity. Based on the existing battery system, the electrolyte infiltrates the positive electrode and the negative electrode to realize the transmission of lithium ions inside the battery and realize the normal operation of the battery. However, in the battery with a manganese-based positive electrode, the HF in the electrolyte will cause the trivalent manganese ions in the positive electrode active material to undergo a disproportionation reaction to generate divalent manganese ions and tetravalent manganese ions. The divalent manganese ions migrate to the negative electrode with the electrolyte and deposit at the negative electrode, continuously destroying the SEI film on the negative electrode side. The SEI film needs lithium ions to regenerate, resulting in a decrease in the cycle performance of the battery. In the prior art, the electrolyte and the manganese-based positive electrode active material are isolated by coating. The coating causes the electrolyte to be unable to well infiltrate the positive electrode, thereby affecting the transmission of lithium ions and the rate performance of the battery. Moreover, the single-layer coating has limited isolation effect on the electrolyte, and the simple coating has limited effect on preventing the dissolution of divalent manganese ions.

[0049] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0050] In a first aspect, the present invention provides a composite positive electrode active material, comprising a positive electrode active material, a first coating layer and a second coating layer;

[0051] The first coating layer is disposed between the positive electrode active material and the second coating layer;

[0052] The positive electrode active material is selected from at least one of lithium manganese oxide, lithium-rich manganese-based positive electrode materials, and nickel-cobalt lithium manganese oxide;

[0053] The first coating layer includes a first coating material, and the first coating material includes a conductive polymer;

[0054] The second coating layer includes a second coating material; the second coating material includes a halide solid electrolyte.

[0055] In some of the embodiments, the conductive polymer is selected from at least one of polypyridine and polyaniline; further in some of the embodiments, the conductive polymer is selected from polypyridine or polyaniline.

[0056] The study found that polypyridine and polyaniline not only have good electronic conductivity, but also have groups that can adsorb manganese ions, reducing the dissolution of manganese caused by the Jahn-Teller effect caused by manganese ions, thereby improving the problem of capacity attenuation of manganese-based materials.

[0057] In some embodiments, the general formula of the halide solid electrolyte can be Li x MCl y ,

[0058] Among them, 1≤x≤4, 4≤y≤8; M is a metal element.

[0059] In some embodiments, M is selected from at least one of V, Cr, Mn, Zn, Cd, Fe, Pb, In, Y, Al, Sc, La, Lu, Ga, Zr, Hf, Mg, and Ni; further, M is selected from at least one of Zn, In, Zr, Cd, and Mg.

[0060] In some specific embodiments, x can be 1, 2, 3, or 4;

[0061] In some specific embodiments, y may be 4, 6, or 8;

[0062] In some specific embodiments, the halide solid electrolyte can be LiAlCl4, LiGaCl4, LiInI4, Li2ZnCl4, Li2NiF4, Li2MgCl4, Li2VCl4, Li2ZrCl6, Li2HfCl6, Li3YCl6, Li3InCl6, Li3InBr6, Li3ScCl6, Li6FeCl8, or Li6MnBr8.

[0063] In some preferred embodiments, the halide solid electrolyte is selected from at least one of Li2ZrCl6, Li3InCl6, Li3YCl6, Li3ScCl6, and Li2HfCl6;

[0064] In some of the embodiments, the mass ratio of the monomer of the conductive polymer to the positive electrode active material is (1-10):(90-99); illustratively, it can be 1:99, 2:98, 3:97, 4:96, 5:95, 6:94, 7:93, 8:92, 9:91, or 10:90.

[0065] In some embodiments, the positive electrode active material is coated with a first coating layer to form a first positive electrode active material;

[0066] In some embodiments, the mass ratio of the first positive electrode active material to the second coating layer is (95-99):(1-5), and illustratively, it can be 95:5, 96:4, 97:3, 96:2, 98:2, 95:1, or 99:1.

[0067] In a second aspect, the present invention provides a method for preparing the composite positive electrode active material as described in the first aspect, comprising the following steps:

[0068] S1: The positive electrode active material is mixed with water, the pH is adjusted to a first pH value, and a monomer of a conductive polymer is added to obtain a solution A; the oxidant is mixed with water, the pH is adjusted to a second pH value, and a solution B is obtained; at a temperature of -5-5°C, solution A and solution B are mixed and reacted to obtain a first positive electrode active material;

[0069] S2: The first positive electrode active material prepared in step S1 is mixed with the second coating material to form a second coating layer to obtain a composite positive electrode active material.

[0070] In some of the embodiments, during the preparation of solution A described in S1, the acidic medium used to adjust the pH is selected from at least one of hydrochloric acid and sulfuric acid; further in some of the embodiments, the acidic medium is hydrochloric acid.

[0071] In some of the embodiments, the concentration of the acidic medium is 0.8-1.5 mol / L; further in some of the embodiments, the concentration of the acidic medium is 0.9-1.2 mol / L; and even more in some of the embodiments, the concentration of the acidic medium is 1 mol / L.

[0072] In some of the embodiments, during the preparation of solution B described in S1, the acidic medium used to adjust the pH is selected from at least one of hydrochloric acid and sulfuric acid; further in some of the embodiments, the acidic medium is hydrochloric acid.

[0073] In some of the embodiments, the concentration of the acidic medium is 0.8-1.5 mol / L; further in some of the embodiments, the concentration of the acidic medium is 0.9-1.2 mol / L; and even more in some of the embodiments, the concentration of the acidic medium is 1 mol / L.

[0074] In some embodiments, in step S1, the oxidant is selected from at least one of ammonium persulfate, hydrogen peroxide, sodium vanadate, and potassium dichromate;

[0075] In some of the embodiments, the specific operation of mixing in step S1 is: transferring solution A and solution B to an ice water bath, adding solution B dropwise to solution A under stirring, and continuing the reaction for 2-3 hours after the addition is completed, so that the first coating material takes the positive electrode active material as the matrix, undergoes an oxidative polymerization reaction to generate a polymer and uniformly coats it to form a first positive electrode active material.

[0076] In some embodiments, the mixing method in step S2 is mechanical mixing, preferably ball milling, the ball milling speed is 150-350 rpm, and the ball milling time is 1-10 h.

[0077] In some of the embodiments, during the ball milling process, the mass ratio of the ball milling beads to the mixed material is 1:(15-60).

[0078] A wet coating method is adopted to make the first coating layer uniformly coated on the surface of the positive electrode active material particles. Since the halide solid electrolyte reacts with most solvents, a coating method of first wet coating and then dry coating is adopted to achieve double coating of the polymer and the halide solid electrolyte. Compared with other inorganic solid electrolytes, the halide solid electrolyte is softer and easier to machine, which is conducive to forming a uniform coating on the surface of the first positive electrode active material. The halide solid electrolyte has good deformation ability, which is conducive to improving the contact interface with the first coating layer.

[0079] In a third aspect, the present invention provides a composite positive electrode, comprising the composite positive electrode active material as described in the first aspect.

[0080] In some of the embodiments, in the composite positive electrode, the mass proportion of the composite positive electrode active material is 78%-99%.

[0081] In some preferred embodiments, in the composite positive electrode, the mass percentage of the composite positive electrode active material is 90-99 wt %.

[0082] In some embodiments, the composite positive electrode further includes a binder, which can bind the active material and the conductive agent together.

[0083] In some of the embodiments, in the composite positive electrode, the binder accounts for 1%-10% by mass.

[0084] In some of these embodiments, the binder includes a fiberizable binder.

[0085] It can be understood that the fiberizable binder refers to a binder that can be transformed from a granular state to a fibrous state under the action of high shear force.

[0086] In some of the embodiments, the fiberizable binder is selected from at least one of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyethylene (PE), and polypropylene (PP).

[0087] In some preferred embodiments, the fiberizable binder is selected from at least one of polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF);

[0088] In some of the embodiments, in order to further enhance the bonding effect on the positive electrode system, the composite positive electrode further includes a second binder.

[0089] In some of the embodiments, the second binder is selected from at least one of polyvinylidene fluoride, polyvinyl alcohol (PVA), carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose (CMC), polyvinyl pyrrolidone (HPC), polyethylene (PE), polypropylene (PP), ethylene-propylene-diene monomer, styrene-butadiene rubber (SBR), and fluororubber (FKM).

[0090] In some of the embodiments, the composite positive electrode further includes a conductive agent, which plays a role in collecting microcurrents between active materials and between active materials and current collectors.

[0091] In some embodiments, in the composite positive electrode, the conductive agent accounts for 1-10% by weight.

[0092] In some of the embodiments, the conductive agent includes graphite, such as natural graphite or artificial graphite; carbon materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, super-p and thermal black; conductive fibers, such as carbon fibers and metal fibers; conductive tubes, such as carbon nanotubes; metal powders, such as fluorocarbon powders, aluminum powders and nickel powders; conductive whiskers, such as zinc oxide and potassium titanate; conductive metal oxides, such as titanium oxide; and polyphenylene derivatives, and from the aspect of improving conductivity, the positive electrode conductive agent may preferably be super-p.

[0093] In some embodiments, the specific surface area of ​​the conductive agent may be 80-200 m 2 / g, preferably 100-150m 2 / g

[0094] In some embodiments, the composite positive electrode active material further comprises solid electrolyte powder for improving the ionic conductivity of the composite positive electrode. The present invention does not limit the type of solid electrolyte powder.

[0095] In some of the embodiments, the solid electrolyte powder is selected from at least one of oxide solid electrolyte powder, sulfide solid electrolyte powder, and halide solid electrolyte powder; further, in some of the embodiments, the solid electrolyte powder is selected from halide solid electrolyte powder.

[0096] In some of the embodiments, the solid electrolyte powder accounts for 1 wt%-18 wt% of the composite positive electrode active material. In some of the preferred embodiments, the solid electrolyte powder accounts for 5 wt%-18 wt% of the composite positive electrode active material.

[0097] In some embodiments, the composite positive electrode further includes a positive electrode current collector, in some embodiments, the current collector is selected from a metal foil material, a composite current collector; the composite current collector has a sandwich-like sandwich structure, the middle polymer layer is mainly a polymer insulating resin and other materials, and the metal layer is deposited on both sides of the middle polymer layer by electroplating, chemical plating or other methods. Schematically, the polymer resin includes polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyether ether ketone, polyimide, polyamide, polyethylene glycol, polyamide -imide, polycarbonate, cyclic polyolefin, polyphenylene sulfide, polyvinyl acetate, polytetrafluoroethylene, polymethylene naphthalene, polyvinylidene fluoride, polyethylene naphthalate, polypropylene carbonate, poly(vinylidene fluoride-hexafluoropropylene), poly(vinylidene fluoride-co-chlorotrifluoroethylene), silicone, vinylon, polypropylene, polyethylene, polyvinyl chloride, polystyrene, polyether nitrile, polyurethane, polyphenylene ether, polyester, polysulfone and its derivatives, sodium carboxymethyl cellulose, styrene-butadiene rubber, fluorinated rubber, polyvinyl alcohol or polyvinylidene fluoride, etc. The material of the metal layer is selected from at least one of aluminum, copper, nickel, cobalt, tungsten, tin, lead, iron, silver or gold.

[0098] In some preferred embodiments, the current collector is aluminum foil.

[0099] In one embodiment, the thickness of the composite positive active electrode material layer may be 30 μm-400 μm, for example 30 μm, 40 μm, 50 μm, 80 μm, 110 μm, 200 μm, 300 μm, 400 μm, preferably 50 μm-110 μm.

[0100] A method for preparing the composite positive electrode as described above comprises the following steps:

[0101] S100, mixing the composite positive electrode active material prepared in S2 with a conductive agent, a binder and / or a solid electrolyte, placing the mixture in a high shear force device, performing a fiberization treatment, and a roller pressing treatment to form a composite positive electrode film.

[0102] In some embodiments, the rolling pressure is 550-650 kPa, the rolling time is 3-10 min, and the rolling temperature is 55-65°C.

[0103] In some embodiments, the method for preparing the composite positive electrode further comprises the following steps:

[0104] The composite cathode film is combined with the collective flow through pressing to obtain a composite cathode.

[0105] In a fourth aspect, the present invention provides a battery comprising a composite positive electrode prepared from the composite positive electrode active material described above, an electrolyte and a negative electrode.

[0106] In one embodiment, the battery includes an electrolyte, the electrolyte includes a solvent, and the solvent includes at least one of an ether solvent, propylene carbonate, and fluoroethylene carbonate.

[0107] In one embodiment, the battery includes an electrolyte including an ether solvent.

[0108] In one embodiment, in the electrolyte, the mass proportion of the ether solvent is 5-65%.

[0109] In one embodiment, the electrolyte further includes an electrolyte salt. Exemplarily, it can be at least one of lithium hexafluorophosphate (LiPF6), lithium hexafluoroarsenate (LiAsF6), lithium perchlorate (LiClO4), lithium bisfluorosulfonyl imide (LiFSI), lithium tetrafluoroborate (LiBF4) and bistrifluoromethanesulfonyl imide (LiTFSI), lithium difluorophosphate (LiPO2F2), lithium bisoxalate borate (LiBOB), lithium bisfluorooxalate borate (LiODFB), lithium difluorobisoxalate phosphate (LiODFP) or lithium tetrafluorooxalate phosphate (LiTFOP).

[0110] In one embodiment, based on the total mass of the electrolyte being 100%, the mass percentage of the electrolyte salt is 0.5-25%.

[0111] In one embodiment, the electrolyte contains additives, and the electrolyte also includes additives, and the additives include at least one of 1,3-propane sultone, 1,4-butane sultone, propenyl-1,3-sultone, vinyl sulfate, 4-methyl vinyl sulfate, propenyl sulfate, saturated phosphate compounds and unsaturated phosphate compounds, tris(trimethylsilane) phosphate, tris(trimethylsilane) borate, tris(triethylsilane) borate, succinonitrile, glutaronitrile, ethylene glycol bis(propionitrile) ether, hexane trinitrile, adiponitrile, pimelonitrile, suberonitrile, azelaic acid nitrile, and sebaconitrile.

[0112] In one embodiment, the battery further includes a negative electrode.

[0113] In one embodiment, the negative electrode comprises a negative electrode current collector and a negative electrode active material layer formed on the surface of the negative electrode current collector, wherein the negative electrode active material layer comprises at least a negative electrode active material and a negative electrode binder.

[0114] In one embodiment, the negative electrode active material in the embodiment of the present application is not particularly limited, as long as it is a material that can electrochemically absorb and release S-zone metal ions such as lithium ions, sodium ions, potassium ions, and magnesium ions, such as carbonaceous materials, metal compound materials, or their oxides, carbides, nitrides, silicides, sulfides, phosphides, etc. These materials can be used alone, or two or more can be used in combination.

[0115] In one embodiment, a carbon material can be selected as the negative electrode active material, and specifically one or more of the following can be selected: graphite, needle coke, amorphous carbon, a carbon-containing mesophase, carbon fiber, and a carbon material with a low degree of graphitization. Among them, graphite can include natural graphite, artificial graphite, etc. In addition, materials obtained by coating them with carbon materials, such as amorphous carbon and graphitized materials, can also be used. Amorphous carbon includes but is not limited to particles obtained by firing the entire mesophase, and particles obtained by infusible treatment and firing of a carbon precursor. As carbonaceous particles with a low degree of graphitization, particles obtained by firing organic matter at a temperature generally below 2500°C can be listed.

[0116] In one embodiment, non-metallic materials that can be used as negative electrode active materials also include silicon and its compounds, such as Si, SiOx (0≤x<2). Since silicon-containing materials are prone to expansion, easy to fall off from the negative electrode current collector, and have poor conductivity, they are often mixed with carbon materials, such as a core-shell structure containing a carbon coating layer.

[0117] In one embodiment, metal elements and metal compounds can also be selected as negative electrode active materials, such as compounds containing metals or metalloids such as Li, Ag, Al, Bi, Cu, Ga, Ge, In, Ni, Pb, Sb, Si, Sn, Sr, and Zn.

[0118] In one embodiment, the mass percentage of the negative electrode active material contained in the negative electrode active material layer may be 80-99%, for example, 80%, 85%, 90%, 95%, 97%, 99%, etc., preferably 95-97%.

[0119] In one embodiment, when the negative electrode active material is a non-metallic material such as a carbon material, the negative electrode binder may be an aqueous binder such as one or more of sodium hydroxymethyl cellulose, styrene-butadiene latex, polyacrylic acid, acrylic copolymer, cyclodextrin, etc.;

[0120] In one embodiment, the negative electrode active material layer can be obtained by coating a negative electrode slurry on a negative electrode current collector and then drying the negative electrode slurry, wherein the negative electrode slurry includes at least a negative electrode active material and a negative electrode binder. When an aqueous solvent is used as a liquid medium for forming the negative electrode slurry, a thickener is preferably used for slurrying, and the thickener can generally be used to adjust the viscosity of the slurry.

[0121] In one embodiment, the thickener in the embodiment of the present application can be one or more of the following: carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein and their salts, etc.

[0122] In one embodiment, the mass proportion of the thickener in the negative electrode slurry can be 0.1-5%, for example, 0.1%, 0.2%, 0.5%, 0.6%, 1%, 2%, 3%, 4%, 5%, etc., preferably 0.5-3%, and more preferably 0.6-2%.

[0123] The technical solution of the present invention will be further explained below in conjunction with specific embodiments.

[0124] Example 1

[0125] 1. A composite positive electrode active material, comprising a positive electrode active material, a first coating layer and a second coating layer; the positive electrode active material is lithium manganate; the first coating layer is arranged on the surface of the positive electrode active material particles, between the positive electrode active material and the second coating layer, the first coating layer comprises a first coating material, in this embodiment, the first coating material is polyaniline, the second coating layer is arranged on the surface of the first coating layer away from the positive electrode active material, the second coating layer comprises a second coating material, and the second coating material comprises a halide solid electrolyte Li2ZrCl6.

[0126] In this embodiment, in the first coating layer, the mass ratio of aniline monomer to positive electrode active material is 5:95;

[0127] The mass ratio of the second coating layer to the first positive electrode active material is 1:99.

[0128] The composite positive electrode also includes a conductive agent Super-P, a binder polytetrafluoroethylene (PTFE) and a polyvinylidene fluoride (PVDF). In the composite positive electrode, the mass ratio of the composite positive electrode active material, the binder and the conductive agent is 95:3:2. In the binder, the mass ratio of PTFE to PVDF is 7:3.

[0129] 2. A method for preparing a composite positive electrode active material: comprising the following steps:

[0130] 1) Preparation of the first positive electrode active material:

[0131] 11) Firstly, the positive electrode active material is placed in deionized water, and 1 mol / L hydrochloric acid solution is slowly added dropwise to adjust the pH value to about 2.5, and then 5 wt % of aniline monomer is added, and the whole process is stirred to obtain solution A;

[0132] 12) Place a certain amount of oxidant (such as ammonium persulfate, hydrogen peroxide, sodium vanadate, potassium dichromate, etc.) in deionized water, add 1 mol / L acidic medium (such as hydrochloric acid, sulfuric acid) solution with stirring, adjust the pH value to about 2.5, and obtain solution B.

[0133] 13) Transfer solution A and solution B to an ice water bath, slowly drop solution B into solution A under stirring, and continue the reaction for 3 hours after the dropwise addition is completed, so that the aniline monomer undergoes an oxidative polymerization reaction with the positive electrode active material as a matrix to generate a polymer and uniformly coat the polymer to form a first positive electrode active material;

[0134] 2) Preparing a composite positive electrode active material: weighing a halide solid electrolyte and the first positive electrode active material prepared in step 1) at a mass ratio of 1:99, placing them in a high-speed mixer, and causing friction and collision during the physical mixing process, so that the halide solid electrolyte is evenly dispersed and adsorbed on the surface of the first positive electrode active material to form a second coating layer, thereby preparing a composite positive electrode active material;

[0135] 3) The composite positive electrode active material, the conductive agent and the binder are weighed in a mass ratio of 95:3:2, mixed, put into a high-speed mixer for fiberization, and then rolled to form a composite positive electrode film. The rolling pressure is 600 kPa, the rolling time is 5 minutes, and the rolling temperature is 60°C.

[0136] 4) Roll-pressing the composite positive electrode film prepared in step 3) and the current collector to obtain a composite positive electrode. The current collector is aluminum foil.

[0137] 3. A battery comprising the composite positive electrode as described above, an electrolyte and a negative electrode, wherein the negative electrode comprises a negative electrode active material, and the negative electrode active material comprises graphite.

[0138] Example 2

[0139] The difference between this embodiment and embodiment 1 is that the mass ratio of aniline monomer to positive electrode active material is 1:99.

[0140] Example 3

[0141] The difference between this embodiment and embodiment 1 is that the mass ratio of aniline monomer to positive electrode active material is 10:90.

[0142] Example 4

[0143] The difference between this embodiment and embodiment 1 is that the mass ratio of the first positive electrode active material to the second coating layer is 95:5.

[0144] Example 5

[0145] The difference between this embodiment and embodiment 1 is that the first coating material is polypyrrole and the second coating material is Li3InCl6.

[0146] Comparative Example 1

[0147] The difference between Comparative Example 1 and Example 1 is that the composite positive electrode active material is replaced with a lithium manganate positive electrode active material.

[0148] Comparative Example 2

[0149] The difference between Comparative Example 2 and Example 1 is that the composite positive electrode active material is replaced with a polyaniline-coated lithium manganate positive electrode active material.

[0150] Comparative Example 3

[0151] The difference between Comparative Example 3 and Example 1 is that the composite positive electrode active material is replaced with a lithium manganate positive electrode active material coated with a halide solid electrolyte Li2ZrCl6.

[0152] Test example:

[0153] Test method:

[0154] 1) Cycle life test at room temperature with 80% capacity cutoff

[0155] ① Charge at 0.3C to a final voltage of 4.2V, a cut-off current of 0.05C, and let stand for 30 minutes;

[0156] ②Discharge at 0.3C until the final discharge voltage reaches 3.0V, record the discharge capacity, and let stand for 30 minutes;

[0157] ③ Cycle (1)-(2), test the cycle life at room temperature with a cutoff of 80% capacity. The test results are shown in Table 1.

[0158] 2) 2C discharge capacity retention rate test

[0159] At room temperature (25°C), the battery cell is charged to 4.2V at 2C, and then switched to constant voltage charging with a cut-off current of 0.05C. At this time, the capacity is C0. The fully charged battery is discharged to 3.0V at the required rate (2C). The capacity obtained by the test is C1. C1 / C0 is the 2C discharge capacity retention rate.

[0160] 3)ICP test

[0161] Weigh about 0.1g of negative electrode powder (accurate to ±0.0003g) of two portions of each embodiment, place in a 100ml beaker, add a small amount of distilled water to wet the bottom of the cup, then add 5ml12mol / L HCl (made in Shandong, GR) to dissolve, heat on an electric heating plate for 20min, remove and cool, dilute and test. The prepared series of standard solutions are introduced into an iCAP7000 inductively coupled plasma spectrometer (ICP) (made in the United States), and the intensity of manganese in the standard solution is measured at the wavelength of manganese to be measured. When the linear correlation coefficient of the working curve r≥0.9995, the measurement can be carried out. The test results are shown in Table 1.

[0162] The relevant data are shown in Table 1 below:

[0163] Table 1.

[0164]

[0165]

[0166] From the data in Table 1, it can be seen that the technical solution provided by the present invention selects a conductive polymer as the first layer coating material, a halide solid electrolyte as the second layer coating material, and adopts a coating method of first wet coating and then dry coating to achieve double coating of the polymer and the halide solid electrolyte. The battery prepared by the prepared composite positive electrode active material has a longer life and a higher 2C discharge capacity retention rate than the comparative example. At the same time, through double-layer coating, the generation of divalent manganese ions and the deposition on the negative electrode side can be effectively inhibited. The above is only a speculation on the possibility of the technical solution of the present application, and does not constitute a limitation on the scope of protection of the present application.

[0167] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.

Claims

1. A composite positive electrode active material, It is characterized in that comprising a positive electrode active material, a first coating layer and a second coating layer; The surface of the particles of the positive electrode active material is sequentially coated with the first coating layer and the second coating layer; The positive electrode active material is selected from at least one of lithium manganese oxide, lithium-rich manganese-based positive electrode materials, and nickel-cobalt lithium manganese oxide; The first coating layer includes a first coating material, and the first coating material includes a conductive polymer; The second coating layer includes a second coating material, and the second coating material includes a halide solid electrolyte.

2. The composite positive electrode active material according to claim 1, It is characterized in that The conductive polymer is selected from at least one of polypyridine and polyaniline.

3. The composite positive electrode active material according to claim 1, It is characterized in that The general formula of the halide solid electrolyte is Li x MCl y , where 1≤x≤4, 4≤y≤8; M is a metal element.

4. The composite positive electrode active material according to claim 3, It is characterized in that The M is selected from at least one of V, Cr, Mn, Zn, Cd, Fe, Pb, In, Y, Al, Sc, La, Lu, Ga, Zr, Hf, and Mg.

5. The composite positive electrode active material according to claim 1, It is characterized in that The mass ratio of the conductive polymer monomer to the positive electrode active material is 1-10:90-99.

6. The composite positive electrode active material according to claim 1, It is characterized in that The positive electrode active material is coated with the first coating layer to form a first positive electrode active material; the mass ratio of the first positive electrode active material to the second coating layer is 95-99:1-5.

7. A method for preparing a composite positive electrode active material according to any one of claims 1 to 6, It is characterized in that The following steps are involved: S1: The positive electrode active material is mixed with water, the pH is adjusted to a first pH value, and a monomer of a conductive polymer is added to obtain a solution A; the oxidant is mixed with water, the pH is adjusted to a second pH value, and a solution B is obtained; at a temperature of -5-5°C, solution A and solution B are mixed and reacted to obtain a first positive electrode active material; S2: The first positive electrode active material prepared in S1 is mixed with the second coating material to form a second coating layer to obtain a composite positive electrode active material.

8. A composite positive electrode, It is characterized in that The composite positive electrode comprises the composite positive electrode active material according to any one of claims 1 to 6.

9. The composite positive electrode according to claim 8, It is characterized in that In the composite positive electrode, the mass proportion of the composite positive electrode active material is 78%-99%.

10. A battery, It is characterized in that It comprises the composite positive electrode as claimed in claim 8, an electrolyte and a negative electrode.

Citation Information

Cited By

  • Solid-state battery, positive electrode sheet, positive electrode active material, preparation method, electric device and use

    WO2026098036A1