Preparation method for preparing S-doped M-N-C oxygen reduction catalyst based on molecular guest strategy and product thereof
The preparation of S-doped M-N-C catalysts through the molecular guest strategy solves the problem of randomness of the active site structure in the existing technology, achieves high activity and simple preparation of the catalyst, is suitable for large-scale applications, and improves the activity of the oxygen reduction reaction.
Patent Information
- Application Number
- CN202410785985.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-18
AI Technical Summary
The active site structure of existing S-doped M-N-C catalysts is random, difficult to construct accurately, and lacks a universal preparation strategy, which affects its catalytic activity.
Using a preparation method based on a molecular guest strategy, a S-doped M-N-C catalyst is formed by coordinating a metal salt, a sulfur source and a hard template in the solution, followed by room temperature stirring and pyrolysis treatment to ensure the specific interaction between the sulfur atom and the metal center. , to build a stable local coordination structure.
It improves the inherent activity of the catalyst, simplifies the preparation process, has universal applicability and large-scale application potential, and improves the oxygen reduction reaction (ORR) activity.
Smart Images

Figure CN118763233A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of preparation of fuel cell electrocatalysts, and in particular relates to a preparation method of an S-doped MNC oxygen reduction catalyst based on a molecular guest strategy and a product thereof. Background Art
[0002] Oxygen reduction reaction (ORR) is a crucial cathode reaction in the discharge process of zinc-air batteries and fuel cells. Researchers are committed to developing a highly active MNC catalyst. Increasing the active site density of the catalyst is the most direct way to improve the activity of the catalyst. However, the construction of MNC catalysts with high-density active sites is often complex and prone to forming inactive metal clusters. In addition, since the catalytic activity of MNC catalysts is highly dependent on the electronic structure of the metal center, local structural coordination engineering has become a crucial way to improve the intrinsic activity of the active sites in the catalyst. Introducing heteroatoms into the local coordination structure of the active site provides a feasible way to regulate the electronic structure of the active site. In particular, thiophene S and oxidized S formed by S doping can induce charge redistribution at the metal center, thereby improving the intrinsic activity of the MNC catalyst.
[0003] However, the S doping in the S-doped MNC catalysts reported in the literature is all formed during the pyrolysis process, and the precursor does not involve specific interactions between metal atoms and S atoms, resulting in randomness in the active site structure in the final catalyst. It is impossible to guarantee the directional and precise construction of the structural type of the S-doped MNC catalyst, and there is a lack of a general strategy for the preparation of S-doped MNC catalysts. Summary of the invention
[0004] In view of this, the present invention aims to propose a method for preparing an S-doped MNC oxygen reduction catalyst based on a molecular guest strategy and to improve the intrinsic activity of the MNC catalyst.
[0005] The present invention provides a method for preparing an S-doped MNC oxygen reduction catalyst based on a molecular guest strategy, and the specific steps are as follows:
[0006] 1) 1,10-phenanthroline, a sulfur source and a metal salt are weighed according to a formula, and dissolved in ethanol to prepare solution A, solution B and solution C, respectively, wherein the sulfur source is a C atom connected to a S atom having a lone electron pair and at least one amino group;
[0007] 2) Mix solution B and solution C, and stir at room temperature to make them uniform, to obtain solution D;
[0008] 3) Mix solution A and solution D, and stir at room temperature to make them uniform, to obtain solution E;
[0009] 4) Weigh the hard template according to the formula, add it to solution E, and stir it at room temperature to make it uniform, so as to prepare solution F;
[0010] 5) Transfer solution F to a water bath, heat, and stir until dry to obtain product G;
[0011] 6) Grinding the product G into powder, placing it in a tube furnace for primary pyrolysis in an inert gas atmosphere, and cooling it to room temperature to obtain material H;
[0012] 7) transferring material H to an acid solution for etching to remove the hard template and the metal particles generated in step 6), and drying under vacuum to obtain product I;
[0013] 8) The product I is transferred to a tube furnace, subjected to secondary pyrolysis in an inert gas atmosphere, and cooled to room temperature to obtain an S-doped MNC catalyst.
[0014] Further, the use formula of the 1,10-phenanthroline, hard template, sulfur source and metal salt is as follows:
[0015]
[0016] Furthermore, the sulfur source is one or a combination of thiourea, thioacetamide, allylthiourea, and thiocyanate.
[0017] Furthermore, the metal salt is one or a combination of ferric chloride, cobalt chloride, manganese chloride, tin chloride, copper chloride, cerium chloride and ruthenium chloride.
[0018] Furthermore, the hard template is any one of nano-SiO2, nano-ZnO, nano-MgO, nano-Al2O3 and nano-polystyrene spheres or a combination of several of them.
[0019] Furthermore, in step 5), the water bath temperature is 50-70°C.
[0020] Furthermore, in step 6) and step 8), the inert gas is any one of high-purity nitrogen, high-purity argon and argon-hydrogen mixed gas.
[0021] Furthermore, the conditions for the primary pyrolysis and the secondary pyrolysis in step 6) and step 8) are 5°C·min -1 The heating rate is increased from room temperature to 700-1050°C for pyrolysis, and the pyrolysis time is 1-5h.
[0022] Furthermore, in the step 7), the acid solution is one or a combination of hydrofluoric acid, hydrochloric acid and sulfuric acid, the etching time is 6 to 12 hours, and the drying condition is vacuum drying at 60° C. for 12 to 24 hours.
[0023] Another aspect of the present invention further provides an S-doped MNC oxygen reduction catalyst prepared by the above preparation method.
[0024] Beneficial effects:
[0025] (1) The preparation method of the S-doped MNC oxygen reduction catalyst based on the molecular guest strategy provided by the present invention uses the S (C atom connected to the S atom with a lone electron pair is connected to at least one amino group) source as the molecular guest. The molecular guest can not only coordinate with the metal center, but also pyrolysis is more conducive to the formation of active thiophene sulfur (CSC), which can improve the ORR activity in two ways. However, the coordination between the general sulfur source and the metal center is not easy to control, and due to the presence of more O elements, pyrolysis often forms more inactive sulfur oxides (C-SO X ). The metal center with an empty d orbital is used as the host structure. The lone electron of the S atom is filled into the empty orbital of the metal center (coordination bond) to form the MN / SC structure. During the pyrolysis process, the S atom is anchored in the carbon skeleton to form an internally stable local coordination structure. In addition, since the S atom has a lower electronegativity and a larger atomic radius than the N atom, it is beneficial to break the symmetric structure of the MNC, optimize the electronic structure of the metal center, improve the adsorption strength between the active site and the oxygen-containing intermediate, and enhance the ORR activity.
[0026] (2) The preparation process of the S-doped MNC oxygen reduction catalyst prepared based on the molecular guest strategy provided by the present invention is simple, effective and universal, which is conducive to large-scale application and preparation. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a transmission electron microscope (TEM) image of the FeNSC-allylthiourea catalyst prepared in Example 1.
[0028] Figure 2 Linear sweep voltammetry (LSV) curves of the FeNSC-allylthiourea catalyst prepared in Example 1, the FeNSC-thiourea catalyst in Example 2 and the FeNSC-thioacetic acid catalyst in Comparative Example 1.
[0029] Figure 3 LSV diagrams of the FeNSC-allylthiourea catalyst prepared in Example 1 and the FeNSC-A allylthiourea catalyst prepared in Comparative Example 2.
[0030] Figure 4 This is the X-ray photoelectron spectroscopy S2p high-resolution spectrum of the FeNSC-allylthiourea catalyst prepared in Example 1.
[0031] Figure 5X-ray diffraction (XRD) patterns of the MnNSC catalyst prepared in Example 3, the CuNSC catalyst prepared in Example 4, and the CeNSC catalyst prepared in Example 5. DETAILED DESCRIPTION
[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification. The methods described are all conventional methods unless otherwise specified, and the raw materials described can be obtained from public commercial channels unless otherwise specified.
[0033] The term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0034] The preparation method of the S-doped MNC oxygen reduction catalyst prepared based on the molecular guest strategy provided by the present invention comprises the following specific steps:
[0035] 1) 1,10-phenanthroline, a sulfur source and a metal salt are weighed according to a formula, and dissolved in ethanol to prepare solution A, solution B and solution C, respectively, wherein the sulfur source is a C atom connected to a S atom having a lone electron pair and at least one amino group;
[0036] 2) Mix solution B and solution C, and stir at room temperature to make them uniform, to obtain solution D;
[0037] 3) Mix solution A and solution D, and stir at room temperature to make them uniform, to obtain solution E;
[0038] 4) Weigh the hard template according to the formula, add it to solution E, and stir it at room temperature to make it uniform, so as to prepare solution F;
[0039] 5) Transfer solution F to a water bath, heat, and stir until dry to obtain product G;
[0040] 6) Grinding the product G into powder, placing it in a tube furnace for primary pyrolysis in an inert gas atmosphere, and cooling it to room temperature to obtain material H;
[0041] 7) transferring material H to an acid solution for etching to remove the hard template and the metal particles generated in step 6), and drying under vacuum conditions to obtain product I;
[0042] 8) The product I is transferred to a tube furnace, subjected to secondary pyrolysis in an inert gas atmosphere, and cooled to room temperature to obtain an S-doped MNC catalyst.
[0043] According to the present invention, preferably, the sulfur source is one or a combination of thiourea, thioacetamide, allylthiourea, and thiocyanate; the metal salt is one or a combination of ferric chloride, cobalt chloride, manganese chloride, tin chloride, copper chloride, cerium chloride, and ruthenium chloride; the hard template is any one or a combination of nano-SiO2, nano-ZnO, nano-MgO, nano-Al2O3, and nano-polystyrene spheres; the water bath temperature in step 5) is 50-70°C; the inert gas in step 6) and step 8) is any one of high-purity nitrogen, high-purity argon, and argon-hydrogen mixed gas; the conditions for the primary pyrolysis and the secondary pyrolysis in step 6) and step 8) are 5°C·min -1 The heating rate is from room temperature to 700-1050°C for pyrolysis, and the pyrolysis time is 1-5h. The acid solution in step 7) is one or a combination of hydrofluoric acid, hydrochloric acid and sulfuric acid. The etching time is 6-12h. The drying condition is vacuum drying at 60°C for 12-24h.
[0044] Example 1
[0045] 1) Weigh 0.4 g of 1,10-phenanthroline, 0.309 g of allylthiourea and 1 m mol of FeCl3·6H2O, respectively, and dissolve them in ethanol to prepare solution A, solution B and solution C;
[0046] 2) Mix solution B and solution C, and stir at room temperature for 30 minutes to make them uniform, to obtain solution D;
[0047] 3) Solution A and solution D were mixed and stirred at room temperature for 60 min to make them uniform, thereby obtaining solution E;
[0048] 4) Weigh 0.5 g SiO2, add it to solution E, stir at room temperature for 60 min to make it uniform, and prepare solution E;
[0049] 5) Transfer solution E to a water bath, heat to 70° C., and stir until dry to obtain product F;
[0050] 6) Grind the product F into powder, place it in a tube furnace in an inert gas atmosphere at 850° C. for 2 h, and cool it to room temperature to obtain material G;
[0051] 7) transferring material G to hydrofluoric acid for etching to remove the hard template and the metal particles generated in step 6), and drying at 60° C. for 12 h under vacuum to obtain product H;
[0052] 8) The product H was transferred to a tube furnace and subjected to secondary pyrolysis at 850 °C for 2 h in an inert gas atmosphere, and then cooled to room temperature to obtain a S-doped FeNSC catalyst.
[0053] It is denoted as FeNSC-allylthiourea catalyst.
[0054] Transmission electron microscopy (TEM) image of FeNSC-allylthiourea catalyst, such as Figure 1 shown.
[0055] Example 2
[0056] 1) Weigh 0.4 g of 1,10-phenanthroline, 0.202 g of thiourea and 1 m mol FeCl3·6H2O, respectively, and dissolve them in ethanol to prepare solution A, solution B and solution C;
[0057] 2) Mix solution B and solution C, and stir at room temperature for 30 minutes to make them uniform, to obtain solution D;
[0058] 3) Solution A and solution D were mixed and stirred at room temperature for 60 min to make them uniform, thereby obtaining solution E;
[0059] 4) Weigh 2 g of SiO2, add it to solution E, stir at room temperature for 60 min to make it uniform, and prepare solution E;
[0060] 5) Transfer solution E to a water bath, heat to 50° C., and stir until dry to obtain product F;
[0061] 6) Grind the product F into powder, place it in a tube furnace in an inert gas atmosphere at 1050° C. for 1 h, and cool it to room temperature to obtain material G;
[0062] 7) transferring material G to hydrofluoric acid for etching to remove the hard template and the metal particles generated in step 6), and drying at 60° C. for 24 h under vacuum conditions to obtain product H;
[0063] 8) The product H was transferred to a tube furnace and subjected to secondary pyrolysis at 1050 °C for 1 h in an inert gas atmosphere, and then cooled to room temperature to obtain a S-doped FeNSC catalyst.
[0064] It is denoted as FeNSC-allylthiourea catalyst.
[0065] Example 3
[0066] 1) Weigh 0.4 g of 1,10-phenanthroline, 0.202 g of thiourea and 1 m mol of MnCl2·4H2O, respectively, and dissolve them in ethanol to prepare solution A, solution B and solution C;
[0067] 2) Mix solution B and solution C, and stir at room temperature for 30 minutes to make them uniform, to obtain solution D;
[0068] 3) Solution A and solution D were mixed and stirred at room temperature for 60 min to make them uniform, thereby obtaining solution E;
[0069] 4) Weigh 2 g of SiO2, add it to solution E, stir at room temperature for 60 min to make it uniform, and prepare solution E;
[0070] 5) Transfer solution E to a water bath, heat to 50° C., and stir until dry to obtain product F;
[0071] 6) Grind the product F into powder, place it in a tube furnace in an inert gas atmosphere at 900°C for 1 hour, and cool it to room temperature to obtain material G;
[0072] 7) transferring material G to hydrofluoric acid for etching to remove the hard template and the metal particles generated in step 6), and drying at 60° C. for 12 h under vacuum to obtain product H;
[0073] 8) The product H was transferred to a tube furnace and subjected to secondary pyrolysis at 900 °C for 1 h in an inert gas atmosphere, and then cooled to room temperature to obtain a S-doped MnNSC catalyst.
[0074] It is denoted as MnNSC catalyst.
[0075] Example 4
[0076] 1) Weigh 0.4 g of 1,10-phenanthroline, 0.202 g of thiourea and 1 m mol CuCl2·4H2O, respectively, and dissolve them in ethanol to prepare solution A, solution B and solution C;
[0077] 2) Mix solution B and solution C, and stir at room temperature for 30 minutes to make them uniform, to obtain solution D;
[0078] 3) Solution A and solution D were mixed and stirred at room temperature for 60 min to make them uniform, thereby obtaining solution E;
[0079] 4) Weigh 2 g of SiO2, add it to solution E, stir at room temperature for 60 min to make it uniform, and prepare solution E;
[0080] 5) Transfer solution E to a water bath, heat to 50° C., and stir until dry to obtain product F;
[0081] 6) Grind the product F into powder, place it in a tube furnace in an inert gas atmosphere at 950° C. for 3 h, and cool it to room temperature to obtain material G;
[0082] 7) transferring material G to hydrofluoric acid for etching to remove the hard template and the metal particles generated in step 6), and drying at 60° C. for 12 h under vacuum to obtain product H;
[0083] 8) The product H was transferred to a tube furnace and subjected to secondary pyrolysis at 950 °C for 3 h in an inert gas atmosphere, and then cooled to room temperature to obtain a S-doped CuNSC catalyst.
[0084] Recorded as CuNSC catalyst.
[0085] Example 5
[0086] 1) Weigh 0.4 g of 1,10-phenanthroline, 0.202 g of thiourea and 1 m mol CuCl2·4H2O, respectively, and dissolve them in ethanol to prepare solution A, solution B and solution C;
[0087] 2) Mix solution B and solution C, and stir at room temperature for 30 minutes to make them uniform, to obtain solution D;
[0088] 3) Solution A and solution D were mixed and stirred at room temperature for 60 min to make them uniform, thereby obtaining solution E;
[0089] 4) Weigh 3 g of SiO2, add it to solution E, and stir at room temperature for 60 min to make it uniform, to obtain solution E;
[0090] 5) Transfer solution E to a water bath, heat to 50° C., and stir until dry to obtain product F;
[0091] 6) Grind the product F into powder, place it in a tube furnace in an inert gas atmosphere at 950° C. for 3 h, and cool it to room temperature to obtain material G;
[0092] 7) transferring material G to hydrofluoric acid for etching to remove the hard template and the metal particles generated in step 6), and drying at 60° C. for 12 h under vacuum to obtain product H;
[0093] 8) The product H was transferred to a tube furnace and subjected to secondary pyrolysis at 950 °C for 3 h in an inert gas atmosphere, and then cooled to room temperature to obtain a S-doped CeNSC catalyst.
[0094] Recorded as CeNSC catalyst.
[0095] Comparative Example 1
[0096] 1) Weigh 0.4 g of 1,10-phenanthroline, 0.202 g of thioacetic acid and 1 m mol FeCl3·6H2O, respectively, and dissolve them in ethanol to prepare solution A, solution B and solution C;
[0097] 2) Mix solution B and solution C, and stir at room temperature for 30 minutes to make them uniform, to obtain solution D;
[0098] 3) Solution A and solution D were mixed and stirred at room temperature for 60 min to make them uniform, thereby obtaining solution E;
[0099] 4) Weigh 3 g of SiO2, add it to solution E, and stir at room temperature for 60 min to make it uniform, to obtain solution E;
[0100] 5) Transfer solution E to a water bath, heat to 50° C., and stir until dry to obtain product F;
[0101] 6) Grind the product F into powder, place it in a tube furnace in an inert gas atmosphere at 950° C. for 3 h, and cool it to room temperature to obtain material G;
[0102] 7) transferring material G to hydrofluoric acid for etching to remove the hard template and the metal particles generated in step 6), and drying at 60° C. for 12 h under vacuum to obtain product H;
[0103] 8) The product H was transferred to a tube furnace and subjected to secondary pyrolysis at 950° C. for 3 h in an inert gas atmosphere, and then cooled to room temperature to obtain a S-doped FeNSC-thioacetic acid catalyst.
[0104] It is denoted as FeNSC-thioacetic acid catalyst.
[0105] Comparative Example 2
[0106] 1) Weigh 0.4 g of 1,10-phenanthroline, 0.309 g of allylthiourea and 1 m mol of FeCl3·6H2O, respectively, and dissolve them in ethanol to prepare solution A, solution B and solution C;
[0107] 2) Mix solution B and solution C, and stir at room temperature for 30 minutes to make them uniform, to obtain solution D;
[0108] 3) Solution A and solution D were mixed and stirred at room temperature for 60 min to make them uniform, thereby obtaining solution E;
[0109] 4) Weigh 0.5 g SiO2, add it to solution E, stir at room temperature for 60 min to make it uniform, and prepare solution E;
[0110] 5) Transfer solution E to a water bath, heat to 70° C., and stir until dry to obtain product F;
[0111] 6) Grind the product F into powder, place it in a tube furnace in an inert gas atmosphere at 850° C. for 2 h, and cool it to room temperature to obtain material G;
[0112] 7) Transfer material G to hydrofluoric acid for etching to remove the hard template and the metal particles generated in step 6), and dry at 60° C. for 12 h under vacuum conditions to obtain the S-doped FeNSC catalyst.
[0113] Denoted as FeNSC-A allylthiourea catalyst
[0114] The catalysts prepared in the above examples and comparative examples were respectively -2The amount was uniformly loaded on different glassy carbon electrodes as working electrodes, and three-electrode electrochemical test was carried out (with Hg / Hg2SO4 electrode as reference electrode and graphite electrode as counter electrode).
[0115] Figure 2 The linear sweep voltammetry (LSV) curves of the ORR performance of the catalysts prepared in the above-mentioned Examples 1, 2 and Comparative Example 1 in 0.1 mol·L-1 HClO4 aqueous electrolyte are shown, wherein the FeNSC-allylthiourea catalyst prepared in Example 1 has an initial potential of 0.89 V and a half-wave potential of 0.79 V, showing the best ORR catalytic performance. The FeNSC-thiourea catalyst prepared in Example 2 shows an ORR performance similar to that of Example 1, which is better than the FeNSC-thioacetic acid catalyst described in Comparative Example 1.
[0116] Figure 3 The ORR performance diagram of the FeNSC-allylthiourea catalyst prepared in Example 1 and the FeNSC-A allylthiourea catalyst prepared in Comparative Example 2 shows that the secondary pyrolysis is beneficial to improving the ORR activity of the catalyst.
[0117] Figure 4 The X-ray photoelectron spectroscopy S2p high-resolution spectrum of the FeNSC-allylthiourea catalyst prepared in Example 1 proves that the S species in the prepared catalyst exist in two forms: CSC (thiophene S) and C-SOx-C (oxidized S), which is beneficial to adjust the electronic structure of the Fe metal center and enhance the catalytic performance of the catalyst.
[0118] Figure 5 The X-ray diffraction (XRD) patterns of the MnNSC catalyst prepared in Example 3, the CuNSC catalyst prepared in Example 4, and the CeNSC catalyst prepared in Example 5 verified, through analysis, that the catalysts prepared by the strong coordination effect of 1,10-phenanthroline with metal and the spatial isolation strategy of the hard template provided by the present invention did not contain metal particles, and had a certain universality for different metal raw materials.
[0119] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing S-doped MNC oxygen reduction catalyst based on molecular guest strategy, characterized in that: The specific steps are as follows: 1) 1,10-phenanthroline, a sulfur source and a metal salt are weighed according to a formula, and dissolved in ethanol to prepare solution A, solution B and solution C, respectively, wherein the sulfur source is a C atom connected to a S atom having a lone electron pair and at least one amino group; 2) Mix solution B and solution C, and stir at room temperature to make them uniform, to obtain solution D; 3) Mix solution A and solution D, and stir at room temperature to make them uniform, to obtain solution E; 4) Weigh the hard template according to the formula, add it to solution E, and stir it at room temperature to make it uniform, so as to prepare solution F; 5) Transfer solution F to a water bath, heat, and stir until dry to obtain product G; 6) Grinding the product G into powder, placing it in a tube furnace for primary pyrolysis in an inert gas atmosphere, and cooling it to room temperature to obtain material H; 7) transferring material H to an acid solution for etching to remove the hard template and the metal particles generated in step 6), and drying under vacuum conditions to obtain product I; 8) The product I is transferred to a tube furnace, subjected to secondary pyrolysis in an inert gas atmosphere, and cooled to room temperature to obtain an S-doped MNC catalyst.
2. The method for preparing S-doped MNC oxygen reduction catalyst based on molecular guest strategy according to claim 1, characterized in that: The usage formula of the 1,10-phenanthroline, hard template, sulfur source and metal salt is as follows:
3. The method for preparing S-doped MNC oxygen reduction catalyst based on molecular guest strategy according to claim 1, characterized in that: The sulfur source is one or a combination of thiourea, thioacetamide, allylthiourea and thiocyanate.
4. The method for preparing S-doped MNC oxygen reduction catalyst based on molecular guest strategy according to claim 1, characterized in that: The metal salt is one or a combination of ferric chloride, cobalt chloride, manganese chloride, tin chloride, copper chloride, cerium chloride and ruthenium chloride.
5. The method for preparing S-doped MNC oxygen reduction catalyst based on molecular guest strategy according to claim 1, characterized in that: The hard template is any one of nano-SiO2, nano-ZnO, nano-MgO, nano-Al2O3 and nano-polystyrene spheres or a combination of several of them.
6. The method for preparing S-doped MNC oxygen reduction catalyst based on molecular guest strategy according to claim 1, characterized in that: In step 5), the water bath temperature is 50-70°C.
7. The method for preparing S-doped MNC oxygen reduction catalyst based on molecular guest strategy according to claim 1, characterized in that: In step 6) and step 8), the inert gas is any one of high-purity nitrogen, high-purity argon and argon-hydrogen mixed gas.
8. The method for preparing S-doped MNC oxygen reduction catalyst based on molecular guest strategy according to claim 1, characterized in that: The conditions for the primary pyrolysis and the secondary pyrolysis in step 6) and step 8) are 5°C·min -1 The heating rate is increased from room temperature to 700-1050°C for pyrolysis, and the pyrolysis time is 1-5h.
9. The method for preparing S-doped MNC oxygen reduction catalyst based on molecular guest strategy according to claim 1, characterized in that: In the step 7), the acid solution is one or a combination of hydrofluoric acid, hydrochloric acid and sulfuric acid, the etching time is 6 to 12 hours, and the drying condition is vacuum drying at 60° C. for 12 to 24 hours.
10. An S-doped MNC oxygen reduction catalyst prepared by the method for preparing an S-doped MNC oxygen reduction catalyst based on a molecular guest strategy according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method and application of transition metal and sulfur-nitrogen co-doped macroporous carbon electrocatalyst
CN112234213A
Carbon aerogel supported cobalt monatomic catalyst for metal-air battery, and preparation method and application thereof
CN113363514A
Bis-phenanthroline imidazolyl multi-element co-doped carbon-zinc air battery catalyst as well as preparation method and application thereof
CN114361485A
Hollow spherical carbon-based catalyst based on water system ZIF derivation as well as preparation method and application of hollow spherical carbon-based catalyst
CN115133044A
Preparation of iron-based nitrogen-doped porous carbon material and application of iron-based nitrogen-doped porous carbon material in zinc-air battery
CN116239113A