Separator having different porosities in thickness direction and method for manufacturing same
By designing structures with different porosity along the thickness direction in the separator of lithium secondary batteries, the problem of battery performance degradation caused by the difference in ionic conductivity between the positive electrode and the negative electrode is solved, achieving higher battery capacity and life, and reducing the resistor.
Patent Information
- Application Number
- CN202411011511.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-19
- Filing Date
- 2020-09-02
- Publication Date
- 2024-10-11
AI Technical Summary
The difference in ionic conductivity between the positive and negative electrodes in lithium secondary batteries leads to battery performance degradation, and existing technologies have not been able to effectively solve this problem.
Design a separator with different porosity along the thickness direction, by setting an electrode with high ion conductivity on the side with low porosity of the separator and an electrode with low ion conductivity on the side with high porosity, and pass the roller through The pressing process forms the main body of the separator with different porosity, ensuring that the porosity changes continuously along the thickness direction.
It effectively alleviates the problem of ionic conductivity imbalance between the positive and negative electrodes, increases the capacity and life of the battery, reduces the initial resistance, and improves the capacity retention rate.
Abstract
Description
[0001] This application is a divisional application of a Chinese patent application with an application date of September 2, 2020, application number "202080052278.7", and invention name "Partition with different porosities along the thickness direction and its manufacturing method". Technical Field
[0002] This application claims the benefit of Korean Patent Application No. 2019-0115296, filed on September 19, 2019, the disclosure of which is incorporated herein by reference in its entirety.
[0003] The present invention relates to a separator for a secondary battery having different porosities in a thickness direction, and more particularly, to a separator body having different porosities in a thickness direction so as to prevent performance degradation due to a difference in ion conductivity between a positive electrode and a negative electrode. Background Art
[0004] Among separators of lithium secondary batteries, safety enhanced separators (hereinafter referred to as "SRS separators") are widely used. The SRS separator is configured to have a structure in which a coating including an inorganic material and a binder is formed on a polyolefin-based substrate, thereby providing high safety against high temperatures.
[0005] The coating of the SRS separator is formed into a porous structure by inorganic materials and binders. With the help of the porous structure, the volume of the liquid electrolyte solution is increased, thereby improving the lithium ion conductivity and the electrolyte impregnation rate of the SRS separator. Therefore, the SRS separator can improve the performance and stability of lithium secondary batteries at the same time.
[0006] The positive and negative electrodes constituting a lithium secondary battery have different ion conductivities of lithium ions depending on the type of active material, thickness and conductivity of the electrode. If the ion conductivities of the positive and negative electrodes with a separator disposed therebetween are different, battery performance may deteriorate.
[0007] In order to make the total mass transfer rate of the positive electrode and the negative electrode having different ionic conductivities the same, the areas of the electrodes may be set differently or the thicknesses of the electrodes may be designed differently.
[0008] Korean Patent Application Publication No. 2013-0123568 (November 13, 2013) (hereinafter referred to as "Patent Document 1") discloses a separator having a structure in which the sizes of an inorganic material coated on a first surface of a separator body and an inorganic material coated on a second surface of the separator body are different from each other so as to increase the impregnation amount of an electrolyte and lithium ion conductivity by increasing the porosity of the separator. The separator of Patent Document 1 has only the effect of increasing the porosity of the coating layer.
[0009] Korean Patent Application Publication No. 2016-0118586 (October 12, 2016) (hereinafter referred to as "Patent Document 2") discloses a multilayer electrode, characterized in that in an electrode including three or more electrode mixture layers, the porosity of the electrode mixture layer close to the current collector is relatively smaller than the porosity of the electrode mixture layer far from the current collector.
[0010] Patent Document 2 is a technology for improving adhesion by forming an electrode mixture layer structure having a porosity difference and preventing electrode detachment even when volume expansion and contraction occur due to charge and discharge.
[0011] Korean Patent Application Publication No. 2016-0097537 (August 18, 2016) (hereinafter referred to as "Patent Document 3") discloses a separator configured to improve adhesion between the separator and the positive electrode or between the separator and the negative electrode by forming a coating including a binder having affinity with the positive electrode binder on a surface in contact with the positive electrode and forming a coating including a binder having affinity with the negative electrode binder on a surface in contact with the negative electrode.
[0012] Patent Document 3 discloses a configuration for improving adhesion between a separator and an electrode, but does not address the difference in ion conductivity between a positive electrode and a negative electrode.
[0013] As mentioned above, various methods have been proposed to solve the problem of battery performance degradation due to the difference in ionic conductivity between the positive and negative electrodes. However, none of them is a clear solution.
[0014] (Prior art literature)
[0015] (Patent Document 1) Korean Patent Application Publication No. 2013-0123568 (November 13, 2013)
[0016] (Patent Document 2) Korean Patent Application Publication No. 2016-0118586 (October 12, 2016)
[0017] (Patent Document 3) Korean Patent Application Publication No. 2016-0097537 (August 18, 2016) Summary of the invention
[0018] Technical issues
[0019] The present invention has been made in view of the above problems, and an object of the present invention is to provide a separator for a secondary battery and a method for manufacturing the same, the separator being capable of preventing the life and capacity of the battery from being deteriorated due to the difference in ion conductivity between a positive electrode and a negative electrode.
[0020] Technical Solution
[0021] According to the present invention, the above and other objects can be achieved by providing a separator for a secondary battery, wherein the separator may include a separator body having a porous structure including polyolefin, and the separator body may be configured to have a structure having different porosities along a thickness direction.
[0022] The separator body may not have an interface where porosity differs, and may be configured to have a form in which porosity continuously changes.
[0023] The separator body may include at least one of a portion where porosity increases in a thickness direction and a portion where porosity decreases in the thickness direction.
[0024] The separator body may have a maximum porosity at the center in a thickness direction.
[0025] The separator may further include a first coating layer formed on a first surface of the separator body and a second coating layer formed on a second surface of the separator body.
[0026] Furthermore, the hardness of the first coating layer and the hardness of the second coating layer may be different from each other.
[0027] The first coating layer may include a first inorganic material and a first binder, and the second coating layer may include a second inorganic material and a second binder, wherein the first inorganic material and the second inorganic material may have the same hardness and different content ratios, or may have different hardnesses regardless of the content ratio.
[0028] Furthermore, the present invention may selectively combine any one or more combinations of the above-mentioned constructions, and it is obvious to those skilled in the art that physically impossible or inappropriate situations are excluded.
[0029] The present invention also provides a method for manufacturing the separator, the method comprising the following steps:
[0030] 1) preparing a separator body having a porous structure including polyolefin;
[0031] 2) forming a first coating layer on a first surface of the separator body of step 1) and forming a second coating layer on a second surface of the separator body of step 1); and
[0032] 3) Press the partition from step 2).
[0033] Meanwhile, the method may further include a step of removing the first coating layer and the second coating layer after step 3).
[0034] The hardness of the first coating layer and the hardness of the second coating layer may be different from each other.
[0035] Furthermore, the compression ratio on the first surface side of the separator body and the compression ratio on the second surface side of the separator body may be different.
[0036] The first coating layer may include a first inorganic material and a first binder, and the second coating layer may include a second inorganic material and a second binder, wherein the rolling strength of the first coating layer and the second coating layer may depend on the types and content ratios of the first inorganic material, the second inorganic material, the first binder, and the second binder.
[0037] In step 3), the same pressure is applied to the separator body from the outside of the first coating layer and the second coating layer.
[0038] Furthermore, the present invention provides an electrode assembly having a stacked structure in which the separator manufactured by the above method is interposed between a positive electrode and a negative electrode.
[0039] Between the positive electrode and the negative electrode, an electrode with high ion conductivity may be disposed in a direction having low porosity in the separator, and an electrode with low ion conductivity may be disposed in a direction having high porosity in the separator.
[0040] Furthermore, any one or more configurations of the manufacturing methods may be selectively combined, and it is obvious to those skilled in the art that physically impossible or inappropriate cases are excluded. DETAILED DESCRIPTION
[0041] Hereinafter, the preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings so that the preferred embodiments of the present invention can be easily implemented by those skilled in the art to which the present invention belongs. However, when describing in detail the operating principle of the preferred embodiments of the present invention, when the detailed description of the known functions and configurations contained therein may obscure the subject matter of the present invention, the detailed description of them will be omitted.
[0042] Inclusion of an element does not mean exclusion of other elements but means that these elements may be further included unless otherwise stated.
[0043] Unless otherwise specifically limited, the detailed description by limitation or addition of elements may apply to all inventions and is not limited to a specific invention.
[0044] The present invention relates to a separator for a secondary battery, wherein the separator may include a separator main body having a porous structure including polyolefin, and the separator main body may be configured to have a structure having different porosities in a thickness direction.
[0045] In lithium secondary batteries, charging and discharging are performed as lithium ions move through a separator disposed between a positive electrode and a negative electrode. The positive electrode and the negative electrode differ in ion conductivity of lithium ions depending on the type of active material, thickness and conductivity of the electrode.
[0046] When the difference in ionic conductivity between the positive and negative electrodes is large, the capacity and life of the battery may decrease due to the increased irreversibility of lithium ions.
[0047] Since the present invention provides a separator for a secondary battery, which has a porosity difference along the thickness direction, the present invention can alleviate the problem of ion conductivity imbalance between the positive electrode and the negative electrode by disposing an electrode with high ion conductivity on the side of the separator with low porosity and disposing an electrode with low ion conductivity on the side of the separator with high porosity.
[0048] In order to manufacture a separator having a porosity difference along the thickness direction as described above, the following process can be performed, including: preparing a separator body having a porous structure containing polyolefin; forming a first coating on a first surface of the separator body and forming a second coating on a second surface of the separator body; and pressing the separator on which the first coating and the second coating are formed.
[0049] Specifically, when the partition body includes a first surface and a second surface and the same pressure is applied to the partition body from the outside of the first coating and the second coating, since the coating with high hardness has a high rolling strength relative to the partition body, the porosity of the partition body is greatly reduced and the coating with high hardness has a relatively low porosity, and since the coating with low hardness has a low rolling strength relative to the partition body, the porosity of the partition body is slightly decreased and the coating with low hardness has a relatively high porosity.
[0050] Specifically, assuming that the first coating and the second coating themselves are hardly compressed, and the pressure applied to the first coating and the second coating is directly applied to the partition body, the compression ratio of the first surface side of the partition body is different from the compression ratio of the second surface side of the partition body because of the difference in rolling strength due to the hardness difference between the first coating and the second coating.
[0051] Therefore, it is possible to manufacture a separator in which a porosity difference is generated between the first surface side and the second surface side of the separator body.
[0052] Since the porosity difference of the separator is formed by the rolling process, the porosity difference does not occur based on a specific interface, and the separator can be configured in a form in which the porosity continuously changes in the thickness direction of the separator.
[0053] For example, since the pressure applied to the outside of the separator body is greater than the pressure applied to the center of the separator body in the thickness direction, the first and second surfaces subjected to the greatest pressure may show the greatest change in porosity and the porosity at the center may be greatest.
[0054] Therefore, the porosity may increase from the first surface of the separator body toward the center of the separator body and increase from the second surface of the separator body toward the center of the separator body.
[0055] The first coating layer may include a first inorganic material and a first binder, and the second coating layer may include a second inorganic material and a second binder, wherein the first inorganic material and the second inorganic material may have the same hardness and different content ratios.
[0056] For example, when the same material is used as the first inorganic material and the second inorganic material, in order to configure the first coating layer and the second coating layer to have different hardnesses, the content ratio of the first inorganic material and the second inorganic material used in each coating layer may be different.
[0057] Furthermore, the first inorganic material and the second inorganic material may allow the first coating layer and the second coating layer to have different hardnesses by using materials having different hardnesses regardless of the content ratio.
[0058] The first inorganic material and the second inorganic material are not particularly limited as long as they are commonly used in the manufacture of separator coatings for secondary batteries. The first inorganic material and the second inorganic material can be at least one selected from the group consisting of: (a) an inorganic material having piezoelectricity; and (b) an inorganic material having lithium ion transport capability.
[0059] Inorganic materials with piezoelectricity are non-conductors under normal pressure, but when a certain pressure is applied to them, the internal structure changes, thereby becoming conductive. In particular, inorganic materials with piezoelectricity exhibit high dielectric constant characteristics of 100 or more, and have a potential difference between two faces due to charges generated when particles are stretched or compressed under a certain pressure, with one face being charged by a positive electrode and the other face being charged by a negative electrode.
[0060] In the case of using an inorganic material having the above characteristics as a porous active layer component, a short circuit may occur in the positive electrode and the negative electrode due to an external impact such as a needle-like conductor, whereby the positive electrode and the negative electrode may not directly contact each other due to the inorganic material coated on the separator, and a potential difference may be generated in the particles due to the piezoelectricity of the inorganic material. Therefore, electron migration, that is, a fine current flow, is achieved between the positive electrode and the negative electrode, whereby the voltage of the battery is gradually reduced, and thus the stability can be improved.
[0061] Examples of the inorganic material having piezoelectricity may be at least one selected from the group consisting of BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb 1-x La x Zr1-y Ti y O3 (PLZT), Pb(Mg 1 / 3 Nb 2 / 3 )O3 - PbTiO3 (PMN - PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiC and combinations thereof, but the present invention is not limited thereto.
[0062] An inorganic material having lithium ion transport ability refers to an inorganic material that contains lithium element, does not store lithium, and transports lithium ions. The inorganic material having lithium ion transport ability can transport and convey lithium ions through (defects) present in the particle structure. Therefore, the lithium ion conductivity in the battery is improved, and thus the battery performance can be improved.
[0063] Examples of inorganic materials having lithium ion transport ability may be at least one selected from the group consisting of: lithium phosphate (Li3PO4); lithium titanium phosphate (Li x Ti y (PO4)3, where 0 < x < 2 and 0 < y < 3); lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, where 0 < x < 2, 0 < y < 1, and 0 < z < 3); (LiAlTiP) x O y -based glass (where 0 < x < 4 and 0 < y < 13), such as 14Li2O - 9Al2O3 - 38TiO2 - 39P2O5; lithium lanthanum titanate (Li x La y TiO3, where 0 < x < 2 and 0 < y < 3); lithium germanium thiophosphate (Li x Ge y P z S w , where 0 < x < 4, 0 < y < 1, 0 < z < 1, and 0 < w < 5), such as Li 3.25 Ge 0.25 P 0.75 S4; lithium nitride (Li x N y , where 0 < x < 4 and 0 < y < 2), such as Li3N; SiS2 - based glass (Li x Si y S z , where 0 < x < 3, 0 < y < 2, and 0 < z < 4), such as Li3PO4 - Li2S - SiS2; P2S5 - based glass (Li x Py S z , where 0 < x < 3, 0 < y < 3, and 0 < z < 7), such as LiI-Li2S-P2S5; and combinations thereof, but the present invention is not limited thereto.
[0064] In addition, the first inorganic material and the second inorganic material may be metal hydroxides or hydroxides of metal oxides represented by the following formula.
[0065] M(OH)x (wherein in this formula, M is B, Al, Mg, Co, Cu, Fe, Ni, Ti, Au, Hg, Zn, Sn, Zr, or their oxides, and x is an integer from 1 to 4).
[0066] The composition ratio of the binder polymer to the first inorganic material and the second inorganic material is not greatly limited, and the composition ratio of the first inorganic material and the second inorganic material to the binder can be controlled in the range of 10:90 to 99:1 based on the weight ratio, preferably in the range of 80:20 to 99:1.
[0067] When the binder polymer is more than 90% by weight based on the total weight of the first inorganic material, the second inorganic material, and the binder polymer, the amount of the binder polymer increases excessively, resulting in a decrease in the pore diameter and porosity due to the reduction in the interstitial volume formed between the inorganic materials, and, correspondingly, the final battery performance deteriorates. On the contrary, when the binder polymer is less than 1% by weight based on the total weight of the first inorganic material, the second inorganic material, and the binder polymer, the amount of the binder polymer is too low, thus weakening the bonding strength between the inorganic materials, and, correspondingly, the mechanical properties of the final organic / inorganic composite porous separator may deteriorate.
[0068] There are no particular limitations on the first binder and the second binder as long as they are commonly used in the manufacture of separator coatings for secondary batteries. For example, the first binder and the second binder can use any one of the binder polymers selected from the group consisting of: polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethyl methacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate, poly(ethylene oxide), cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethylated amylose, cyanoethylated polyvinyl alcohol, cyanoethylated cellulose, cyanoethylated sucrose, amylose, and carboxymethyl cellulose, or a mixture of two or more of them.
[0069] In the separator according to the present invention, the rolling strength of the first coating layer and the second coating layer depends on the types and content ratios of the first inorganic material, the second inorganic material, the first adhesive, and the second adhesive. Therefore, a separator body with appropriate porosity can be manufactured by controlling the rolling strength according to the types and content ratios of the first inorganic material, the second inorganic material, the first adhesive, and the second adhesive.
[0070] In a specific example, after the rolling step in the method of manufacturing the separator, a step of removing the first coating layer and the second coating layer may be further included.
[0071] The separator body is in a state of forming a structure having a porosity difference by the rolling step, and therefore, even if the first coating layer and the second coating layer are removed, the minimum purpose of reducing the efficiency reduction due to the electrodes having an ion conductivity difference can be achieved.
[0072] Furthermore, when the first coating layer and the second coating layer are removed, the initial resistance may be lower and the capacity retention rate may be higher than before the removal.
[0073] A coating layer including an inorganic material may be added again as needed on both surfaces of the separator main body from which the first coating layer and the second coating layer have been removed.
[0074] The present invention provides an electrode assembly having a stacked structure in which a separator manufactured by the above-mentioned method for manufacturing a separator is interposed between a positive electrode and a negative electrode, and provides a lithium secondary battery having a structure in which the electrode assembly is impregnated with a non-aqueous electrolyte containing a lithium salt.
[0075] For example, the positive electrode may be manufactured by applying a positive electrode mixture including a positive electrode active material on a positive electrode current collector and drying the positive electrode mixture. The positive electrode mixture may optionally further include a binder, a conductive agent, a filler, and the like as needed.
[0076] In general, the positive electrode collector is manufactured to have a thickness of 3 μm to 500 μm. There is no particular limitation on the positive electrode collector, as long as the positive electrode collector shows high conductivity and the positive electrode collector does not cause any chemical changes in the battery to which the positive electrode collector is applied. For example, the positive electrode collector may be made of stainless steel, aluminum, nickel, titanium or calcined carbon. Alternatively, the positive electrode collector may be made of aluminum or stainless steel with a surface treated with carbon, nickel, titanium or silver. In addition, the positive electrode collector may have a microscale uneven pattern formed on its surface to increase the adhesion of the positive active material. The collector may be configured in various forms such as a film, a sheet, a foil, a mesh, a porous body, a foam body, and a non-woven fabric body.
[0077] The positive electrode active material may be a material capable of undergoing an electrochemical reaction, and includes a lithium transition metal oxide containing two or more transition metals, for example, a layered compound such as lithium cobalt oxide (LiCoO2) and lithium nickel oxide (LiNiO2) substituted by one or more transition metals; a lithium manganese oxide substituted by one or more transition metals; a lithium nickel oxide represented by LiNi1-yMyO2 (wherein M = Co, Mn, Al, Cu, Fe, Mg, B, Cr, Zn or Ga, the oxide containing at least one of these elements, and y satisfies 0.01≤y≤0.7); a lithium nickel oxide represented by Li 1+z Ni b Mn c Co 1-(b+c+d) M d O (2-e) A e (wherein -0.5≤z≤0.5, 0.1≤b≤0.8, 0.1≤c≤0.8, 0≤d≤0.2, 0≤e≤0.2, b+c+d<1, M=Al, Mg, Cr, Ti, Si or Y, and A=F, P or Cl) represented by a lithium nickel cobalt manganese composite oxide, such as Li 1+ Zn 1 / 3 Co 1 / 3 Mn 1 / 3 O2 and Li 1+ Zn 0.4 Mn 0.4 Co 0.2 O2; by Li 1+x M 1-y M' y PO 4-z X z (wherein M is a transition metal, preferably Fe, Mn, Co or Ni, M'=Al, Mg or Ti, X=F, S or N, and -0.5≤x≤0.5, 0≤y≤0.5, 0≤z≤0.1) represented by olefin-based lithium metal phosphate, but not limited thereto.
[0078] Based on the total weight of the compound including the positive electrode active material, the conductive agent is generally added so that the conductive agent accounts for 1 wt % to 30 wt %. The conductive agent is not particularly limited as long as the conductive agent shows high conductivity while not causing any chemical changes in the battery to which the conductive agent is applied. For example, the following materials can be used as the conductive agent: graphite, such as natural graphite or artificial graphite; carbon black, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermal black; conductive fibers, such as carbon fibers or metal fibers; carbon fluoride powder; metal powder, such as aluminum powder or nickel powder; conductive whiskers, such as zinc oxide or potassium titanate; conductive metal oxides, such as titanium oxide; or conductive substances such as polyphenylene derivatives.
[0079] Binder is a component that helps the combination between active material and conductive agent and the combination with current collector. Based on the total weight of the mixture including positive active material, the amount of binder generally added is 1 wt % to 30 wt %. Examples of binders can be polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, and various copolymers.
[0080] The filler is an optional component for suppressing electrode expansion. The filler is not particularly limited as long as it does not cause any chemical changes in the battery to which the filler is applied and is made of a fiber material. As examples of the filler, olefin polymers such as polyethylene and polypropylene; and fiber materials such as glass fiber and carbon fiber can be used.
[0081] For example, the negative electrode may be manufactured by applying a negative electrode mixture including a negative electrode active material on a negative electrode current collector and drying the negative electrode mixture. The negative electrode mixture may optionally further include the aforementioned components such as a conductive agent, a binder, a filler, and the like as needed.
[0082] In general, the negative electrode collector is manufactured to have a thickness of 3 μm to 500 μm. There is no particular limitation on the negative electrode collector, as long as the negative electrode collector shows high conductivity and the negative electrode collector does not cause any chemical changes in the battery to which the negative electrode collector is applied. For example, the negative electrode collector may be made of copper, stainless steel, aluminum, nickel, titanium or calcined carbon. Alternatively, the negative electrode collector may be made of copper or stainless steel, or an aluminum-cadmium alloy, the surface of which is treated with carbon, nickel, titanium or silver. In addition, the negative electrode collector may have a microscale uneven pattern formed on its surface to increase the adhesion of the negative electrode active material in the same manner as the positive electrode collector. The negative electrode collector may be configured in various forms such as a film, a sheet, a foil, a mesh, a porous body, a foam body, and a non-woven fabric body.
[0083] The negative electrode active material may include, for example: carbon, such as non-graphitizable carbon and graphite-based carbon; metal composite oxides, such as Li x Fe2O3(0≤x≤1), Li x WO2(0≤x≤1), Sn x Me 1-x Me' y O z(Me=Mn, Fe, Pb, Ge; Me'=Al, B, P, Si, elements of Groups 1, 2 and 3 of the periodic table, halogens; 0≤x≤1; 1≤y≤3; 1≤z≤8); lithium metal; lithium alloys; silicon-based alloys; tin-based alloys; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, and Bi2O5; conductive polymers such as polyacetylene; or Li-Co-Ni based materials.
[0084] The binder, the conductive agent, and components added as necessary are the same as those described for the positive electrode.
[0085] Depending on the situation, a filler may be optionally added as a component for suppressing expansion of the negative electrode. There is no particular limitation on the filler as long as it does not cause any chemical changes in the battery to which the filler is applied and is made of a fiber material. As examples of the filler, olefin polymers such as polyethylene and polypropylene; and fiber materials such as glass fiber and carbon fiber can be used.
[0086] Furthermore, other components such as a viscosity control agent and an adhesion promoter may be optionally further included or may be further included in combination of two or more.
[0087] The viscosity control agent is a component for controlling the viscosity of the electrode mixture to facilitate mixing of the electrode mixture and coating on the current collector, and can be added in an amount of 30% by weight based on the total weight of the negative electrode mixture. Examples of viscosity control agents include, but are not limited to, carboxymethyl cellulose and polyvinylidene fluoride. Depending on the circumstances, the above solvents may be used as viscosity control agents at the same time.
[0088] The adhesion promoter is an auxiliary component added to enhance the adhesion between the electrode active material and the electrode current collector, and can be added in an amount of 10 wt % or less based on the amount of the binder. Examples of adhesion promoters include, but are not limited to, oxalic acid, adipic acid, formic acid, acrylic acid derivatives, and itaconic acid derivatives.
[0089] The separator is interposed between the positive electrode and the negative electrode, and, as the separator, a thin insulating film having high ion permeability and excellent mechanical strength is used. The separator generally has a pore size of 0.01 μm to 10 μm and a thickness of 5 μm to 300 μm. As the separator, a sheet or non-woven fabric made of an olefin polymer such as polypropylene and / or glass fiber or polyethylene having chemical resistance and hydrophobicity is used. When a solid electrolyte such as a polymer is used as an electrolyte, the solid electrolyte can also be used as a separator.
[0090] The lithium salt-containing nonaqueous electrolyte is composed of a nonaqueous electrolyte and a lithium salt. As the nonaqueous electrolyte, a nonaqueous organic solvent, an organic solid electrolyte, an inorganic solid electrolyte or the like can be used.
[0091] Examples of the nonaqueous organic solvent include aprotic organic solvents such as N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.
[0092] Examples of the organic solid electrolyte may include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, agitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, polymers having ion dissociative groups, or the like.
[0093] Examples of inorganic solid electrolytes may include Li nitrides, halides, and sulfates, such as Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, Li3PO4-Li2S-SiS2, or the like.
[0094] The lithium salt used herein is a material that is easily dissolved in a non-aqueous electrolyte and may include, for example, LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, (CF3SO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylate, lithium 4-phenylborate, lithium imide, or the like.
[0095] In addition, in order to improve the charge-discharge characteristics and flame retardancy, for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, ethylene glycol dimethyl ether, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N, N-substituted imidazolidinones, ethylene glycol dialkyl ethers, ammonium salts, pyrroles, 2-methoxyethanol, aluminum chloride or the like can be added to the electrolyte. As needed, in order to impart incombustibility, the electrolyte may further include a halogenated solvent such as carbon tetrachloride and trifluoroethylene. In addition, in order to improve high temperature storage characteristics, the electrolyte may further include carbon dioxide gas. Fluoro-ethylene carbonate (FEC, Fluoro-Ethylene Carbonate) and propene sultone (PRS, Propenesultone) and the like may be further included in the electrolyte.
[0096] In a preferred embodiment, a lithium salt such as LiPF6, LiClO4, LiBF4, LiN(SO2CF3)2 and the like can be added to a mixture of a cyclic carbonate of EC or PC as a high dielectric solvent and a linear carbonate of DEC, DMC or EMC as a low viscosity solvent to prepare a lithium salt-containing non-aqueous electrolyte.
[0097] Hereinafter, the present invention will be described with reference to the following examples. These examples are provided only to illustrate the present invention and should not be construed as limiting the scope of the present invention.
[0098] Manufacturing of partitions
[0099] A separator body having a porous structure made of a polyolefin material is prepared.
[0100] In order to form a coating layer having a low hardness, a first coating layer including 80 wt % of Al 2 O 3 as an inorganic material and 20 wt % of polyvinylidene fluoride as a binder was prepared.
[0101] In order to form a coating layer having high hardness, a second coating layer including 80 wt % of BaTiO 2 as an inorganic material and 20 wt % of carboxymethyl cellulose as a binder was prepared.
[0102] Cathode Manufacturing
[0103] By using 95 wt% of Li(Ni 0.6 Mn 0.2 Co 0.2)O2, 2.0 wt% Super-P as a conductive agent, and 3.0 wt% polyvinylidene fluoride as a binder were added to NMP (N-methyl-2-pyrrolidone) as a solvent to prepare a positive electrode mixture slurry. The positive electrode mixture slurry was coated on an aluminum foil, and then dried and pressed to manufacture a positive electrode.
[0104] Negative electrode manufacturing
[0105] A negative electrode mixture slurry was prepared by adding 96 wt % of natural graphite as a negative electrode active material, 1.0 wt % of Super-P as a conductive agent, 2.0 wt % of styrene-butadiene rubber as a binder, and 1.0 wt % of carboxymethyl cellulose as a thickener to H 2 O as a solvent. The negative electrode mixture slurry was coated on a copper foil, and then dried and pressed to manufacture a negative electrode.
[0106] <Example 1>
[0107] The separator is manufactured by coating a first coating layer on a first surface of the separator body and coating a second coating layer on a second surface of the separator body. The electrode assembly is manufactured by disposing a positive electrode on the first coating layer and a negative electrode on the second coating layer.
[0108] A pressing process is performed on the electrode assembly using a pair of pressing rollers, thereby completing the manufacture of the electrode assembly having a porosity difference.
[0109] The pressing process using the pressing roller was performed by applying a pressure of 3 MPa at a temperature of 80° C. for 0.5 seconds.
[0110] <Comparative Example 1>
[0111] An electrode assembly is manufactured in the same manner as in Example 1, except that a first coating is applied to the first and second surfaces of the separator body of Example 1, a positive electrode is disposed on the first coating on the first surface of the separator body, and a negative electrode is disposed on the first coating on the second surface of the separator body.
[0112] <Comparative Example 2>
[0113] An electrode assembly is manufactured in the same manner as in Example 1, except that a second coating is coated on the first and second surfaces of the separator body of Example 1, a positive electrode is disposed on the second coating on the first surface of the separator body, and a negative electrode is disposed on the second coating on the second surface of the separator body.
[0114] <Example 2>
[0115] An electrode assembly was manufactured in the same manner as in Example 1, except that the negative electrode was disposed on the first coating layer of Example 1, and the positive electrode was disposed on the second coating layer of Example 1.
[0116] <Comparative Example 3>
[0117] An electrode assembly was manufactured in the same manner as Example 1, except that a negative electrode was disposed on the first coating layer of the first surface of the separator body of Comparative Example 1, and a positive electrode was disposed on the first coating layer of the second surface of the separator body of Comparative Example 1.
[0118] <Comparative Example 4>
[0119] An electrode assembly was manufactured in the same manner as Example 1, except that a negative electrode was disposed on the second coating layer on the first surface of the separator body of Comparative Example 2, and a positive electrode was disposed on the second coating layer on the second surface of the separator body of Comparative Example 2.
[0120] <Example 3>
[0121] An electrode assembly was manufactured in the same manner as in Example 1, except that the first coating layer and the second coating layer were removed from the separator of Example 1.
[0122] <Comparative Example 5>
[0123] An electrode assembly was manufactured in the same manner as in Example 1, except that the first coating layer and the second coating layer were removed from the separator of Comparative Example 1.
[0124] <Comparative Example 6>
[0125] An electrode assembly was manufactured in the same manner as in Example 1, except that the first coating layer and the second coating layer were removed from the separator of Comparative Example 2.
[0126] <Example 4>
[0127] An electrode assembly was manufactured in the same manner as in Example 1, except that the first coating layer and the second coating layer were removed from the separator of Example 2.
[0128] <Comparative Example 7>
[0129] An electrode assembly was manufactured in the same manner as in Example 1, except that the first coating layer and the second coating layer were removed from the separator of Comparative Example 3.
[0130] <Comparative Example 8>
[0131] An electrode assembly was manufactured in the same manner as in Example 1, except that the first coating layer and the second coating layer were removed from the separator of Comparative Example 4.
[0132] <Test Example 1> Determination of initial resistance
[0133] The battery cells including the electrode assemblies manufactured in Examples 1 to 4 and Comparative Examples 1 to 8 were CC / CV charged under the conditions of 4.2 V, 0.33 C, and 0.5% cutoff, and CC discharged twice under the conditions of 2.5 Vm and 0.33 C.
[0134] Thereafter, the voltage drop generated when the SOC 50% battery was discharged at a current of 2.5 C for 30 seconds was recorded, and the DC resistance value was calculated using R=V / I (Ohm's law). The results are shown in Table 1 below.
[0135] <Test Example 2> Determination of capacity retention
[0136] For the secondary batteries including the electrode assemblies prepared in Examples 1 to 4 and Comparative Examples 1 to 8, the capacity retention rate was measured by measuring the discharge capacity when repeating 50 cycles, wherein each cycle included charging the battery to 4.2 V in a constant current / constant voltage (CC / CV) charging mode of 1C, and then discharging the battery in a constant current (CC) discharge mode under a cutoff condition of 1C and 2.5V. The results are shown in Table 1 below.
[0137] [Table 1]
[0138] Initial resistance(Ohm) Capacity retention rate (%) Example 1 (positive electrode / separator / negative electrode) 0.87 94 Comparative Example 1 (positive electrode / separator / negative electrode) 1.24 87 Comparative Example 2 (positive electrode / separator / negative electrode) 1.11 90 Example 2 (negative electrode / separator / positive electrode) 1.15 88 Comparative Example 3 (negative electrode / separator / positive electrode) 1.23 87 Comparative Example 4 (negative electrode / separator / positive electrode) 1.11 91 Example 3 (positive electrode / separator / negative electrode) 0.78 95 Comparative Example 5 (positive electrode / separator / negative electrode) 1.12 88 Comparative Example 6 (positive electrode / separator / negative electrode) 0.99 91 Example 4 (negative electrode / separator / positive electrode) 1.04 89 Comparative Example 7 (negative electrode / separator / positive electrode) 1.11 88 Comparative Example 8 (negative electrode / separator / positive electrode) 0.99 92
[0139] Referring to Table 1, when Example 1, in which the positive electrode is disposed on a first coating layer having low hardness and the negative electrode is disposed on a second coating layer having high hardness, is compared with Comparative Examples 1 and 2, Example 1 having a porosity difference using a separator manufactured by applying the first coating layer and the second coating layer is measured to have an initial resistance of 0.87 ohms, showing the lowest initial resistance and the highest capacity retention rate.
[0140] On the other hand, when Example 2, in which the negative electrode is provided on the first coating layer and the positive electrode is provided on the second coating layer and there is a porosity difference in the thickness direction, is compared with Comparative Examples 3 and 4, Example 2 is measured to have a higher initial resistance and a lower capacity retention rate than Comparative Example 4, although Example 2 is in a form with a porosity difference by applying the first coating layer and the second coating layer. Therefore, it can be seen that in a separator having a porosity difference in the thickness direction, it is preferred to provide an electrode having a high ion conductivity on the side having a lower porosity and to provide an electrode having a low ion conductivity on the side having a higher porosity.
[0141] Furthermore, when Comparative Examples 1 and 3, and Comparative Examples 2 and 4 were compared, in which coatings having the same hardness were formed on both sides of the separator body, separators having no porosity difference were used, similar results were shown to each other.
[0142] Referring to the results of Example 3, Example 4, and Comparative Examples 5 to 8 in which the first coating layer and the second coating layer were washed and removed, Example 3 in which the positive electrode was disposed on the first surface side of the separator body and the negative electrode was disposed on the second surface side of the separator body was measured to have an initial resistance of 0.78 ohms, exhibiting the lowest initial resistance compared to Comparative Examples 5 to 8, and exhibiting excellent capacity retention.
[0143] In addition, when the results of Example 1, Example 2 and Comparative Examples 1 to 4 are compared with the results of Example 3, Example 4 and Comparative Examples 5 to 8, it can be seen that under the same conditions, the results of the separator with the coating removed and the separator with the coating not removed have the same trend.
[0144] Therefore, it can be seen that when a separator having a porosity difference in a thickness direction of the separator body is used, the resistance is reduced and the capacity retention ratio is increased compared to when a separator having a constant porosity is used.
[0145] In addition, since differences in initial resistance and capacity retention may occur depending on whether the electrode attached to the first and second surfaces of the separator is a positive electrode or a negative electrode, it can be seen that the direction in which the positive and negative electrodes are combined with the separator greatly affects the performance of the secondary battery.
[0146] Those skilled in the art to which the present invention pertains will appreciate that various applications and modifications may be made based on the above description without departing from the scope of the present invention.
[0147] Industrial Applicability
[0148] As is apparent from the above description, the separator for a secondary battery according to the present invention is configured so that the surface facing the positive electrode and the surface facing the negative electrode have different porosities, and thus the problem of ion conductivity imbalance caused by the difference in thickness and conductivity between the positive and negative electrodes can be improved.
[0149] Furthermore, when an electrode assembly manufactured using a separator having such characteristics is used, the capacity and cycle characteristics of a secondary battery may be improved.
[0150] Furthermore, since the positive electrode and the negative electrode exhibit similar performance, the capacities of the positive electrode and the negative electrode can be designed to be the same, thereby increasing the overall energy density of the secondary battery.
[0151] In addition, since the roll-pressing process is performed to manufacture separators having different porosities, the thickness of the separator can be reduced while maintaining the strength of the separator.
Claims
1. An electrode assembly having a stacked structure, wherein a separator is interposed between a positive electrode and a negative electrode, wherein the separator comprises a separator body having a porous structure comprising polyolefin, wherein the separator body is configured to have different porosities in a thickness direction by a rolling process, and the separator has a porosity difference between a first face side and a second face side of the separator body, wherein the separator body has no interface where porosity differs, and is configured to have a form in which porosity varies continuously, wherein the separator body has a maximum porosity at the center in the thickness direction, wherein the porosity of the first side of the separator body is greater than the porosity of the second side of the separator body, and in, Between the positive electrode and the negative electrode, an electrode having high ion conductivity is provided on the second face side of the separator, and an electrode having low ion conductivity is provided on the first face side of the separator. 2 . The electrode assembly according to claim 1 , wherein the separator body includes at least one of a portion in which porosity increases in a thickness direction and a portion in which porosity decreases in the thickness direction. 3 . The electrode assembly according to claim 1 , wherein the separator further comprises a first coating layer formed on a first surface of the separator body and a second coating layer formed on a second surface of the separator body. 4 . The electrode assembly of claim 3 , wherein hardness of the first coating layer and hardness of the second coating layer are different from each other.
5. The electrode assembly according to claim 3, wherein The first coating layer includes a first inorganic material and a first binder, and The second coating layer includes a second inorganic material and a second binder, The first inorganic material and the second inorganic material have the same hardness and different content ratios, or have different hardnesses regardless of the content ratio.
6. The electrode assembly according to claim 1, wherein: The electrode with high ionic conductivity is the negative electrode, and the electrode with low ionic conductivity is the positive electrode.