Loudspeaker diaphragm, sound production device and electronic equipment
By combining ethylene-acrylate rubber and EPDM rubber film layers in the speaker diaphragm, adjusting the density and thickness ratio, and using air pressure molding technology, the problem of insufficient mid-frequency loudness caused by the high density of the speaker diaphragm is solved, and mid-frequency Improved performance and reduced production costs.
Patent Information
- Application Number
- CN202410867972.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-11
AI Technical Summary
The high density of the existing speaker diaphragm results in insufficient mid-frequency loudness and cannot meet the listening needs of users.
A laminated ethylene-acrylate rubber film layer and an ethylene-propylene-diene rubber film layer are used. By adjusting the thickness ratio and the type of reinforcing agent, the density of the speaker diaphragm is reduced, and the processing cost is reduced through air pressure molding technology.
It effectively reduces the weight of the speaker diaphragm, improves the mid-frequency loudness, and solves the problem that EPDM rubber cannot be cross-linked in an aerobic environment, reducing production costs.
Smart Images

Figure CN118764780A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of acoustic equipment, and more specifically, to a loudspeaker diaphragm, a sound-generating device and an electronic device. Background Art
[0002] In the related art, the diaphragm of the sound-emitting device is usually made of acrylic rubber material. The rubber material has a high density and the diaphragm is thick, resulting in a large mass of the diaphragm. The mass of the diaphragm accounts for a relatively high proportion in the entire vibration system, resulting in insufficient mid-frequency loudness of the sound-emitting device and failure to meet the user's listening needs.
[0003] Therefore, it is necessary to provide a new technical solution to solve the above technical problems. Summary of the invention
[0004] An object of the present invention is to provide a new technical solution for a loudspeaker diaphragm.
[0005] According to a first aspect of the present invention, a loudspeaker diaphragm is provided. The loudspeaker diaphragm comprises:
[0006] The ethylene-acrylate rubber film layer and the EPDM rubber film layer are stacked, wherein the ethylene-acrylate rubber film layer is composed of ethylene acrylate carboxylic acid copolymer, and the density of the speaker diaphragm is less than 1.35g / cm 3 .
[0007] Optionally, the thickness of the EPDM rubber membrane layer accounts for 30% to 70% of the total thickness of the loudspeaker diaphragm.
[0008] Optionally, the reinforcing agent of the EPDM rubber film layer is at least one of carbon black, fumed silica, precipitated calcium carbonate and barium sulfate.
[0009] Optionally, the content of the reinforcing agent is 20 to 65 parts in 100 parts of EPDM raw rubber.
[0010] Optionally, the reinforcing agent of the ethylene-acrylate rubber film layer includes at least one of carbon black, fumed silica, precipitated calcium carbonate and barium sulfate.
[0011] Optionally, the content of the reinforcing agent in 100 parts of ethylene-acrylate raw rubber is 40 parts to 120 parts.
[0012] Optionally, the EPDM rubber film layer is cross-linked using a peroxide cross-linking agent.
[0013] Optionally, the peroxide crosslinking agent includes at least one of 1,3-1,4-di(tert-butylperoxyisopropyl)benzene, diisopropylbenzene peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, tert-butylisopropylbenzene peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)-3-hexyne, 4,4'-bis(tert-butylperoxy)valerate, 1,1'-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, and 2,4-dichlorobenzoyl peroxide.
[0014] Optionally, the ethylene-acrylate rubber film layer uses an amine crosslinking agent, and the amine crosslinking agent includes at least one of hexamethylenediamine, hexamethylenediamine carbamate, triethylenetetramine, diphenylamine and di-o-tolylguanidine.
[0015] Optionally, the speaker diaphragm is formed as a two-layer composite structure, the two-layer composite structure includes a layer of the ethylene-acrylate rubber membrane layer and a layer of the EPDM rubber membrane layer; or, the speaker diaphragm is formed as a three-layer composite structure, the three-layer composite structure includes two layers of the ethylene-acrylate rubber membrane layer and a layer of the EPDM rubber membrane layer, the EPDM rubber membrane layer is located between the two layers of the ethylene-acrylate rubber membrane layers.
[0016] Optionally, the loudspeaker diaphragm is formed into a two-layer composite structure, and the loudspeaker diaphragm is formed by air pressure forming, wherein the EPDM rubber membrane layer is located between the ethylene-acrylate rubber membrane layer and the molding mold.
[0017] According to a second aspect of the present application, a sound-generating device is provided, which includes the loudspeaker diaphragm of the above embodiment.
[0018] According to a third aspect of the present application, an electronic device is provided, which includes the sound-generating device of the above embodiment.
[0019] One technical effect of the present application is that the speaker diaphragm of the present application is formed by compounding an ethylene-acrylate rubber membrane layer and an EPDM rubber membrane layer, and the density of the EPDM rubber membrane layer is relatively low, thereby reducing the weight of the speaker diaphragm and improving the mid-frequency loudness of the sound-generating device using the speaker diaphragm. Moreover, by compounding the ethylene-acrylate rubber membrane layer and the EPDM rubber membrane layer to form a composite membrane, the EPDM rubber membrane layer can be isolated from oxygen, providing an oxygen-free environment for the vulcanization of the EPDM rubber, solving the problem that the EPDM rubber cannot be cross-linked in an aerobic environment, thereby the diaphragm can be formed by air pressure, greatly reducing the processing cost of the diaphragm.
[0020] Further features and advantages of the present invention will become apparent from the following detailed description of exemplary embodiments of the present invention with reference to the attached drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the invention and, together with the description, serve to explain the principles of the invention.
[0022] Figure 1 It is a schematic diagram of the structure of a generating device according to an embodiment of the present application.
[0023] Figure 2 It is a schematic structural diagram of a speaker diaphragm according to an embodiment of the present application.
[0024] Figure 3 It is a schematic structural diagram of a speaker diaphragm according to another embodiment of the present application.
[0025] Reference numerals:
[0026] 100, sound-generating device; 10, housing; 20, speaker diaphragm; 30, voice coil; 40, permanent magnet;
[0027] 21. Ethylene-acrylate rubber film layer; 22. EPDM rubber film layer. DETAILED DESCRIPTION
[0028] Various exemplary embodiments of the present invention will now be described in detail with reference to the accompanying drawings. It should be noted that the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present invention unless otherwise specifically stated.
[0029] The following description of at least one exemplary embodiment is merely illustrative in nature and is in no way intended to limit the invention, its application, or uses.
[0030] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.
[0031] In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not limiting. Therefore, other examples of the exemplary embodiments may have different values.
[0032] It should be noted that like reference numerals and letters refer to similar items in the following figures, and therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.
[0033] According to one embodiment of the present application, a speaker diaphragm is provided. Figures 1 to 3As shown, the speaker diaphragm 20 includes a laminated ethylene-acrylate rubber (Alpha-Ethylmescaline Rubber, AEM) film layer 21 and an ethylene-propylene-diene monomer (EPDM) film layer 22, wherein the ethylene-acrylate rubber film layer 21 is composed of ethylene acrylate carboxylic acid copolymer, and the density of the speaker diaphragm is less than 1.35 g / cm 3 .
[0034] In this example, the speaker diaphragm 20 of the present application is composed of an ethylene-acrylate rubber membrane layer 21 and an EPDM rubber membrane layer 22. The density of the EPDM rubber membrane layer 22 is relatively low, thereby reducing the weight of the speaker diaphragm 20 and improving the mid-frequency loudness of the sound-generating device 100 using the speaker diaphragm 20. For example, the ethylene-acrylate rubber membrane layer 21 and the EPDM rubber membrane layer 22 are in direct contact and bonded together to form a composite diaphragm. The ethylene-acrylate rubber membrane layer 21 is composed of an ethylene acrylate carboxylic acid copolymer. Ethylene-acrylate rubber is made of ethylene and methyl acrylate as main raw materials, and is polymerized by high pressure heating under the action of a cross-linking agent. The ethylene-acrylate rubber film layer 21 and the EPDM rubber film layer 22 are compounded to form a composite film, so that the ethylene-acrylate rubber film layer 21 can isolate the EPDM rubber film layer 22 from oxygen, providing an anaerobic environment for the vulcanization of the EPDM rubber, and solving the problem that the EPDM rubber cannot be cross-linked in an aerobic environment. As a result, the diaphragm can be formed by air pressure, greatly reducing the processing cost of the speaker diaphragm 20.
[0035] In this example, the ethylene-acrylate rubber film layer 21 is composed of an ethylene-acrylate carboxylic acid copolymer. That is, the ethylene-acrylate rubber in the ethylene-acrylate rubber film layer 21 contains a carboxylic acid group. The carboxylic acid group enables the ethylene-acrylate rubber to be cross-linked by an amine cross-linking agent in the air at room temperature, and can be formed using air pressure. When the carboxylic acid group is not included, the molding of the ethylene-acrylate rubber uses a peroxide cross-linking agent. The cross-linking reaction of the peroxide cross-linking agent needs to be carried out under high temperature and high pressure. Compared to the process of preparing ethylene-acrylate rubber using a peroxide cross-linking agent, this method of the present application makes the preparation of ethylene-acrylate rubber easier.
[0036] The ethylene-acrylate rubber film layer 21 uses an amine crosslinking agent, and the amine crosslinking agent includes at least one of hexamethylenediamine, hexamethylenediamine carbamate, triethylenetetramine, diphenylamine and di-o-tolylguanidine. All of the above substances can crosslink the raw materials of ethylene-acrylate rubber. The ethylene-acrylate rubber film layer 21 has the characteristics of high and low temperature resistance, oil resistance, and excellent mechanical properties.
[0037] In this example, the mass content of carboxylic acid groups in ethylene-acrylate rubber is 0.5wt% to 5wt%. Carboxylic acid groups react with amine crosslinking agents to form a crosslinked structure. Within a certain range, the more crosslinking points (carboxylic acid groups), the more difficult it is for the molecular chain to move, resulting in an increase in the glass transition temperature, an increase in the damping factor, and a higher mechanical strength of the material, and a decrease in the elongation at break and elastic recovery rate. When the carboxylic acid group content is less than 0.5wt%, too few crosslinking points are formed during the vulcanization process, and the mechanical strength of the material is insufficient. When the carboxylic acid group content is greater than 5wt%, the crosslinking density is too large, the elongation at break of the ethylene-acrylate rubber film layer 21 is reduced, and the phenomenon of film breakage is prone to occur during the vibration of the speaker diaphragm 20. For example, the mass content of carboxylic acid groups in ethylene-acrylate rubber can be 1wt%, 2wt%, 3wt% or 4wt%, etc. Through the above-mentioned range of values, the ethylene-acrylate rubber film layer 21 can have strong mechanical properties, high elongation at break and high elastic recovery rate.
[0038] In this example, the EPDM rubber in the EPDM rubber film layer 22 is a copolymer composed of ethylene, propylene and a small amount of non-conjugated diene. The EPDM rubber has good oxidation resistance, ozone resistance and corrosion resistance. The density of the EPDM rubber film layer 22 is less than that of the ethylene-acrylate rubber film layer 21. By compounding the EPDM rubber film layer 22 and the ethylene-acrylate rubber film layer 21, the overall density of the speaker diaphragm 20 can be reduced, so that the speaker diaphragm of the present application can have a smaller mass.
[0039] In this example, the density of the speaker diaphragm is less than 1.35 g / cm 3 The smaller the density of the speaker diaphragm 20, the greater the thickness of the speaker diaphragm 20 at the same mass, resulting in a smaller vibration space of the diaphragm 20. The greater the density of the speaker diaphragm 20, the greater the mass of the speaker diaphragm 20 at the same thickness, resulting in a small vibration amplitude of the speaker diaphragm 20 and poor mid-frequency performance. The density of the speaker diaphragm 20 is within this range, which can ensure that the density of the speaker diaphragm 20 is moderate, the overall mass is small, and the thickness is moderate, thereby ensuring that the speaker diaphragm 20 has excellent mid-frequency performance.
[0040] For example, the density of the speaker diaphragm 20 may be 1.33 g / cm 3 , 1.30g / cm 3 , 1.28g / cm 3 , 1.25g / cm 3 or 1.2g / cm 3 The density of the loudspeaker diaphragm 20 is within the above value range, which can ensure that the mass of the loudspeaker diaphragm 20 is small and the sound-generating device 100 using the loudspeaker diaphragm 20 of the present application has excellent intermediate frequency performance.
[0041] In this example, the density of the speaker diaphragm 20 can be adjusted by adjusting the proportion of the EPDM rubber membrane layer 22, so that the density of the speaker diaphragm 20 meets the requirements. For example, by setting the thickness of the EPDM rubber membrane layer 22 to account for 30% to 70% of the total thickness of the speaker diaphragm, the density of the speaker diaphragm 20 is adjusted to be within a suitable range, thereby making the mass of the speaker diaphragm 22 smaller.
[0042] In this example, when the thickness of the EPDM rubber film layer 22 accounts for less than 30%, the ethylene-acrylate rubber film layer 21 accounts for too large a proportion, and the overall density of the speaker diaphragm 20 is high. When the thickness of the EPDM rubber film layer 22 accounts for more than 30%, the composite film density can be less than 1.35 g / cm 3 When the thickness of the EPDM rubber film layer 22 accounts for more than 70%, the ethylene-acrylate rubber film layer 21 accounts for too small a proportion, resulting in low overall damping of the speaker diaphragm 20 and low listening yield.
[0043] For example, the thickness ratio of the EPDM rubber film layer 22 can be 35%, 40%, 50%, 60% or 65%, etc. By adjusting the thickness ratio of the EPDM rubber film layer 22 to the above value range, the density of the speaker diaphragm 20 can be adjusted to be less than 1.35 g / cm 3 .
[0044] In one example, the reinforcing agent of the EPDM rubber film layer 22 is at least one of carbon black, fumed silica, precipitated calcium carbonate and barium sulfate.
[0045] In this example, the EPDM rubber film layer 22 is made of EPDM raw rubber, which is a non-reinforced rubber with a low density. The strength can be increased by adding a reinforcing agent, and the density of the material can also be increased. For example, the density of the EPDM rubber film layer 22 is 1 g / cm 3 Up to 1.2g / cm 3 , which is beneficial to improving the overall strength and vibration stability of the speaker diaphragm 20.
[0046] Take carbon black as a reinforcing agent as an example. Carbon black is an amorphous structure, and particles form aggregates through physical and chemical bonding with each other. The primary structure of carbon black is composed of aggregates, and there are van der Waals forces or hydrogen bonds between the aggregates, which can aggregate into a spatial network structure, that is, the secondary structure of carbon black. The surface of carbon black has hydrogen, carboxyl, lactone, free radical, quinone and other groups that can undergo substitution, reduction, oxidation reactions, etc. When it is added to EPDM rubber, due to the strong interaction between the carbon black surface and the EPDM rubber interface, when the material is subjected to force, the molecular chain is easier to slide on the carbon black surface, but it is not easy to separate from the carbon black. The EPDM rubber and carbon black form a strong bond that can slide, and the mechanical strength is increased.
[0047] In this example, the content of the reinforcing agent in 100 parts, i.e. parts by weight, of EPDM raw rubber (i.e., EPDM raw rubber) is 20 to 65 parts. That is, 20 to 65 parts of the reinforcing agent are added to every 100 parts of EPDM raw rubber.
[0048] For example, the reinforcing agent is carbon black, as shown in Table 1. Table 1 shows the elongation at break, tensile strength and density of the EPDM rubber film layer 22 at different carbon black contents.
[0049] Table 1- Comparison of elongation at break, tensile strength and density of EPDM rubber membrane
[0050] Carbon black content / part Elongation at break / % Tensile strength / MPa <![CDATA[Density g / cm 3 > 10 620 5.5 0.95 35 592 17 1.1 50 552 22 1.16 100 238 12 1.32
[0051] As shown in Table 1, when the amount of carbon black is 10 parts, the elongation at break of the EPDM rubber film layer 22 is high, the tensile strength of the EPDM rubber film layer 22 is too low, and the density is low. As the amount of carbon black increases, the elongation at break decreases slightly, while the tensile strength increases more and the density increases. Among them, when the amount of carbon black is 50 parts, the tensile strength is the highest. As the amount of carbon black increases to 100 parts, the elongation at break of the EPDM rubber film layer 22 decreases significantly, the tensile strength decreases, and the density increases to 1.32 g / cm 3 .
[0052] In this example, the content of the reinforcing agent in the EPDM rubber film layer 22 can also be 30 parts, 40 parts, 55 parts or 60 parts, etc. By setting the reinforcing agent content within the above value range, the tensile strength of the EPDM rubber film layer 22 can be effectively improved, thereby improving the strength of the speaker diaphragm 20 and ensuring that the density of the speaker diaphragm 20 is low.
[0053] In addition, fumed silica as a reinforcing agent can improve the hardness, durability and vibration stability of the EPDM rubber film layer 22. Talc as a reinforcing agent can improve the stability, tensile strength and anti-aging performance of the EPDM rubber film layer 22. Precipitated calcium carbonate as a reinforcing agent can improve the tensile strength, tear strength and wear resistance of the EPDM rubber film layer 22.
[0054] Of course, the reinforcing agent may also be other types or a combination of multiple types, and those skilled in the art may determine according to actual conditions, and no specific limitation is made here.
[0055] In one example, the reinforcing agent of the ethylene-acrylate rubber film layer 21 includes at least one of carbon black, fumed silica, precipitated calcium carbonate and barium sulfate.
[0056] In this example, the ethylene-acrylate rubber membrane layer 21 is made of AEM raw rubber. The reinforcing agent can improve the mechanical strength of the ethylene-acrylate rubber membrane layer 21, thereby improving the overall strength and vibration stability of the speaker diaphragm 20.
[0057] Take carbon black as a reinforcing agent as an example. Carbon black is an amorphous structure, and particles form aggregates through physical and chemical bonding with each other. The primary structure of carbon black is composed of aggregates, and there are van der Waals forces or hydrogen bonds between the aggregates, which can aggregate into a spatial network structure, which is the secondary structure of carbon black. The surface of carbon black has hydrogen, carboxyl, lactone, free radical, quinone and other groups that can undergo substitution, reduction, oxidation reactions, etc. When it is added to ethylene-acrylate rubber, due to the strong interaction between the carbon black surface and the ethylene-acrylate rubber interface, when the material is subjected to force, the molecular chain is easier to slide on the carbon black surface, but it is not easy to separate from the carbon black. The ethylene-acrylate rubber and carbon black form a strong bond that can slide, and the mechanical strength is increased.
[0058] In this example, the reinforcing agent is contained in 40 to 120 parts of 100 parts, i.e. parts by weight, of ethylene-acrylate rubber (i.e., AEM rubber). That is, 40 to 120 parts of reinforcing agent are added to every 100 parts of ethylene-acrylate rubber.
[0059] For example, the reinforcing agent is carbon black, as shown in Table 2, which shows the elongation at break, tensile strength and density of the ethylene-acrylate rubber film layer 21 at different carbon black contents.
[0060] Table 2 - Elongation at break, tensile strength and density comparison of ethylene-acrylate rubber film
[0061] Carbon black content / part <![CDATA[Density g / cm 3 > Damping Elongation at break / % 30 1.25 0.11 485 70 1.37 0.19 372 100 1.45 0.22 312 200 1.62 0.26 89
[0062] As shown in Table 2 above, adding carbon black to the ethylene-acrylate rubber film layer 21 helps to improve the damping of the ethylene-acrylate rubber film layer 21. According to the data in Table 2, when the amount of carbon black is 30 parts, the density of the ethylene-acrylate rubber film layer 21 is relatively low, which is 1.25 g / cm 3 , the elongation at break is high, for example, 485%, but the damping is low, only 0.11. When the carbon black content is 70 and 100 parts, the damping is high, reaching about 0.2, the elongation at break is greater than 300%, and the density is between 1.3g / cm 3 Up to 1.5g / cm 3 When the amount of carbon black is increased to 200 parts, the density of the ethylene-acrylate rubber film layer 21 is too large, reaching 1.62g / cm 3 The elongation at break is less than 100%, which is not satisfactory for use.
[0063] In this example, the content of the reinforcing agent in the ethylene-acrylate rubber film layer 21 can also be 40 parts, 45 parts, 55 parts, 60 parts, etc. By setting the reinforcing agent content within the above value range, the strength of the ethylene-acrylate rubber film layer 21 can be effectively improved, thereby improving the strength of the speaker diaphragm 20, and ensuring that the density of the speaker diaphragm 20 is low.
[0064] In addition, fumed silica as a reinforcing agent can improve the hardness, durability and vibration stability of the ethylene-acrylate rubber film layer 21. Talc as a reinforcing agent can improve the stability, tensile strength and anti-aging performance of the ethylene-acrylate rubber film layer 21. Precipitated calcium carbonate as a reinforcing agent can improve the tensile strength, tear strength and wear resistance of the ethylene-acrylate rubber film layer 21.
[0065] Of course, the reinforcing agent may also be other types or a combination of multiple types, and those skilled in the art may determine according to actual conditions, and no specific limitation is made here.
[0066] In one example, the EPDM rubber film layer 22 is cross-linked using a peroxide cross-linking agent.
[0067] In this example, the EPDM rubber film layer 22 includes EPDM raw rubber, peroxide crosslinking agent, crosslinking aid, reinforcing agent, plasticizer, antioxidant, etc. The crosslinking agent plays a role of chemical crosslinking. At a certain temperature, the peroxide generates free radicals, which react with the EPDM raw rubber to form a crosslinked network structure.
[0068] The peroxide crosslinking agent includes at least one of 1,3-1,4-di(tert-butylperoxyisopropyl)benzene, diisopropylbenzene peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, tert-butylisopropylbenzene peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)-3-hexyne, 4,4'-bis(tert-butylperoxy)valerate, 1,1'-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane and 2,4-dichlorobenzoylperoxide.
[0069] In this example, the main function of the crosslinking aid is to promote the crosslinking reaction, and the crosslinking aid includes at least one of trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, N,N'-m-phenylene bismaleimide, diallyl phthalate, triallyl isocyanate and triallyl cyanate.
[0070] In this example, the main function of the plasticizer is to improve the processing performance of EPDM rubber. The processing performance of EPDM rubber is poor in rubber rolling, material absorption and dispersion. At least one of paraffin oil, aromatic oil and cyclohexane oil can be added.
[0071] In this example, the antioxidant includes at least one of antioxidant N-445, antioxidant 246, antioxidant 4010, antioxidant SP, antioxidant RD, antioxidant ODA, antioxidant OD, and antioxidant WH-02.
[0072] The amount of antioxidant added is 0.2wt% to 5wt%. Preferably, the amount of antioxidant added is 0.5wt% to 3wt%. During the use of the speaker diaphragm 20, as time goes by, the molecular chain breaks to generate free radicals, which accelerates its own aging. The addition of antioxidant stops the self-catalytic active free radicals generated by EPDM rubber. Too little addition will not achieve the effect of extending the service life, while too much addition will make it difficult to disperse evenly due to its inability to dissolve well with EPDM rubber, resulting in a decrease in the mechanical properties of the material.
[0073] In one example, the ethylene-acrylate rubber film layer 21 includes AEM raw rubber, an amine cross-linking agent, a reinforcing agent, a plasticizer, an antioxidant, a processing aid, and the like.
[0074] In this example, the processing aid is a release agent including at least one of stearic acid, octadecylamine and alkyl phosphate, α-octadecyl-ω-hydroxy polyoxyethylene phosphate. The internal release agent is added in an amount of 0.5-5 parts, preferably 1-3 parts. The Mooney viscosity and raw rubber strength of ethylene-acrylate rubber are relatively low, resulting in process problems such as sticking to the roller and sticking to the mold, so it is necessary to add an internal release agent to the rubber to improve its processing properties, and a small amount of addition is difficult to achieve the problem of improving the mucous membrane, and an excessive amount of addition will cause the adhesion of the AEM rubber to the adhesive layer in the later stage.
[0075] The plasticizer includes at least one of aliphatic dibasic acid esters, phthalic acid esters (including phthalic acid esters and terephthalic acid esters), polyphenylene esters, benzoic acid esters, polyol esters, chlorinated hydrocarbons, epoxies, citrates, and polyesters.
[0076] The amount of plasticizer added is 3-7 parts. The polar groups on the plasticizer and the polar groups on the ethylene acrylate molecules have a mutual attraction effect, which reduces the interaction of the polar groups on the ethylene acrylate molecules. Therefore, the addition of plasticizer is equivalent to covering the polar groups on the ethylene acrylate molecules, which has a shielding effect, resulting in a reduction in physical crosslinking points. On the other hand, the plasticizer molecules are smaller than the ethylene acrylate molecules and are easier to move. They can provide the space required for the chain segment to move, reduce the glass transition temperature of the material, increase the cold resistance of the material, and improve the processing performance of the material; while excessive plasticizers will precipitate from the inside of the material and reduce the mechanical properties of the material.
[0077] In one example, the speaker diaphragm 20 is formed into a two-layer composite structure, which includes a layer of the ethylene-acrylate rubber membrane layer 21 and a layer of the EPDM rubber membrane layer 22. Alternatively, the speaker diaphragm 20 is formed into a three-layer composite structure, which includes two layers of the ethylene-acrylate rubber membrane layer 21 and a layer of the EPDM rubber membrane layer 22, and the EPDM rubber membrane layer 22 is located between the two layers of the ethylene-acrylate rubber membrane layer 21.
[0078] like Figure 2 As shown, the speaker diaphragm 20 is formed into a two-layer composite structure, which includes a layer of the ethylene-acrylate rubber membrane layer 21 and a layer of the EPDM rubber membrane layer 22. The EPDM rubber membrane layer 22 is bonded to one side of the ethylene-acrylate rubber membrane layer 21 along the thickness direction. The structure of the speaker diaphragm 20 is simple, and the processing technology is simple. The thickness of the speaker diaphragm 20 can be made thinner.
[0079] like Figure 3 As shown, the ethylene-acrylate rubber film layer 21 is set as two layers, and the EPDM rubber film layer 22 is a single layer. That is, the EPDM rubber film layer 22 is the middle layer, and the ethylene-acrylate rubber film layer 21 is the skin layer. The two layers of ethylene-acrylate rubber film layers 21 are respectively bonded to the two sides of the EPDM rubber film layer 22 along the thickness direction. The ethylene-acrylate rubber film layer 21 has good tensile strength and elastic recovery rate, which enables the speaker diaphragm to undergo elastic deformation when subjected to external force, reducing the risk of deformation and damage to the speaker diaphragm.
[0080] In this example, the EPDM rubber film layer 22 is the middle layer. The crosslinking agent of the EPDM rubber film layer 22 is a peroxide crosslinking agent. Since oxygen hinders polymerization, it cannot undergo a crosslinking reaction during air vulcanization. However, by setting the EPDM rubber film layer 22 as the middle layer, the ethylene-acrylate rubber film layer 21 of the epidermis can isolate oxygen, provide an oxygen-free environment for the vulcanization of the EPDM rubber, and solve the problem that the EPDM rubber cannot be crosslinked in an aerobic environment. Thus, the diaphragm can be formed by air pressure, thereby reducing production costs.
[0081] In one example, the loudspeaker diaphragm 20 is formed into a two-layer composite structure, and the loudspeaker diaphragm 20 is formed by air pressure forming, wherein the EPDM rubber membrane layer 22 is located between the ethylene-acrylate rubber membrane layer 21 and the molding mold.
[0082] In this example, the speaker diaphragm 20 is a two-layer structure. During the vulcanization molding process, the EPDM rubber film layer 22 is attached to the molding plastic mold, the ethylene-acrylate rubber film layer 21 is located on one side of the EPDM rubber film layer 22, and the other side of the ethylene-acrylate rubber film layer 21 is in contact with the punching air. The ethylene-acrylate rubber film layer 21 is laid on the top of the EPDM rubber film layer 22 to block the entry of oxygen. The EPDM rubber film layer 22 can undergo a cross-linking reaction under this process mode, reducing costs.
[0083] The following is a comparison of the damping, sound yield, density and mid-frequency performance of the speaker diaphragm under different thickness ratios of the EPDM rubber membrane layer 22. The material formula of the membrane layer of the embodiment and the comparative example is shown in Table 4. The details are as follows:
[0084] Embodiment 1:
[0085] The loudspeaker diaphragm 20 includes a stacked EPDM rubber film layer 22 and an ethylene-acrylate rubber film layer 21. The thickness of the EPDM rubber film layer 22 accounts for 40%, and the thickness of the ethylene-acrylate rubber film layer 21 accounts for 60%.
[0086] Embodiment 2:
[0087] The loudspeaker diaphragm 20 includes a stacked EPDM rubber film layer 22 and an ethylene-acrylate rubber film layer 21. The thickness of the EPDM rubber film layer 22 accounts for 60%, and the thickness of the ethylene-acrylate rubber film layer 21 accounts for 40%.
[0088] Comparative Example 1:
[0089] The thickness of the single-layer EPDM rubber film layer 22 accounts for 100%, and the sample is manufactured by compression molding.
[0090] Comparative Example 2:
[0091] The thickness of the single-layer ethylene-acrylate rubber film layer 21 accounts for 100%.
[0092] The total thickness of the loudspeaker diaphragms of Examples 1 to 2 and Comparative Examples 1 to 2 is about 100±10 μm. The length of the loudspeaker diaphragm is about 17 mm, and the width is about 12 mm.
[0093] Table 3 - Physical properties of the loudspeaker diaphragms of Examples 1, 2 and Comparative Examples 1, 2
[0094]
[0095] The thickness of each film layer is adjusted so that the F0 (for example, F0 refers to the lowest vibration frequency at which the sound-generating device can generate sound) of Example 1 and Example 2 is similar to that of Comparative Example 1 and Comparative Example 2. The parameters of the EPDM rubber film layer and the ethylene-acrylate rubber film layer used in Examples 1 and 2 and Comparative Examples 1 and 2 are shown in Table 4.
[0096] Table 4 Material formula used in the examples and comparative examples
[0097]
[0098]
[0099] It can be seen that according to Examples 1 and 2 compared with Comparative Example 2, the thickness of the EPDM rubber film layer 22 is too small, or the speaker diaphragm prepared with a single layer of ethylene-acrylate rubber film layer will cause the density of the speaker diaphragm 20 to be too large, which can easily lead to the mass of the speaker diaphragm 20 being too large.
[0100] According to the comparison between Examples 1 and 2 and Comparative Example 1, if the thickness of the EPDM rubber film layer 22 is too large or the speaker diaphragm is made of a single EPDM rubber film layer, the damping of the speaker diaphragm 20 will be low, and noise will appear during the listening process, so the listening yield is low. Although the speaker diaphragm of Comparative Example 2 has a high listening yield, its density is high, which makes the quality of the speaker diaphragm 20 high, resulting in a lower mid-frequency performance than the speaker diaphragm 20 of Examples 1 and 2.
[0101] The speaker diaphragms of Embodiments 1 and 2 are formed by a composite ethylene-acrylate rubber membrane layer and an EPDM rubber membrane layer. The density of the EPDM rubber membrane layer is relatively small, for example, less than 1.35 g / cm 3 , thereby reducing the weight of the speaker diaphragm 20 and improving the mid-frequency loudness of the sound-generating device 100 using the speaker diaphragm.
[0102] The damping test method of the material of the loudspeaker diaphragm 20 can be performed using dynamic mechanical analysis (DMA), with a test frequency of 1 Hz, a strain of 0.2%, and a loss factor at 23° C. as the damping of the material.
[0103] The density test method is as follows: after the raw materials of ethylene-acrylate rubber and EPDM rubber are mixed, they are vulcanized into a shape at a vulcanization temperature of 200°C, a time of 10 minutes, and a pressure of 10 MPa. They are prepared into a hard block of approximately 5cm*5cm*1.5cm and tested using the drainage method.
[0104] The method for testing the intermediate frequency performance is: at a voltage of 0.8V, testing the intermediate frequency response curve of the sound-generating device 100 using the speaker diaphragm 20, for example, taking the performance when the vibration frequency is 2000Hz.
[0105] According to another embodiment of the present application, a sound generating device 100 is provided. Figure 1 As shown, the sound-generating device 100 includes the speaker diaphragm 20 of the above embodiment.
[0106] In this example, the speaker diaphragm 20 of the present application is composed of an ethylene-acrylate rubber membrane layer 21 and an EPDM rubber membrane layer 22, so that the mass of the speaker diaphragm 20 is small, and the sound-generating device 100 using the speaker diaphragm 20 can have good mid-frequency loudness. Of course, the sound-generating device 100 of the present application also includes at least all the beneficial effects of the above-mentioned embodiments, which will not be repeated here.
[0107] In this example, the sound-generating device 100 may be a sound-generating device such as a speaker unit or a speaker assembly, and those skilled in the art may determine it according to actual conditions, and no specific limitation is made here.
[0108] like Figure 1 As shown, the sound-generating device 100 may include a housing 10, a magnetic circuit system and a vibration system, wherein the magnetic circuit system includes a permanent magnet 40, and the permanent magnet 40 is used to form a magnetic gap. The vibration system includes a speaker diaphragm 20 and a voice coil 30. The speaker diaphragm 20, the voice coil 30 and the permanent magnet 40 are all connected to the housing 10. The permanent magnet 40 is arranged on one side of the speaker diaphragm 20 along the thickness direction. One end of the voice coil 30 is connected to the speaker diaphragm, and the other end is located in the magnetic gap.
[0109] In this example, the speaker diaphragm 20 may be a folded ring diaphragm. The folded ring diaphragm includes a central portion, a folded ring portion, and a fixed portion connected in sequence from the inside to the outside. The fixed portion is used to connect to the housing 10. The central portion is provided with a dome, and the voice coil 20 is connected to the central portion.
[0110] In other examples, the speaker diaphragm 20 may also be a flat diaphragm or other structures. Those skilled in the art may determine this according to actual conditions, and no specific limitation is made here.
[0111] According to another embodiment of the present application, an electronic device is provided. The electronic device includes the sound generating device 100 described in the above embodiment. Of course, the electronic device of the present application also includes at least all the beneficial effects of the above embodiment, which will not be described in detail here.
[0112] The electronic device may be a mobile phone, a stereo, a tablet computer, a laptop computer, or the like, or may be a device used for underwater work, etc. Those skilled in the art may determine the method according to actual conditions, and no specific limitation is made here.
[0113] In this example, the electronic device includes the sound generating device of the above embodiment, so that the electronic device can have better intermediate frequency loudness.
[0114] The above embodiments focus on the differences between the various embodiments. As long as the different optimization features between the various embodiments are not contradictory, they can be combined to form a better embodiment. Considering the simplicity of the text, they will not be repeated here.
[0115] Although some specific embodiments of the present invention have been described in detail by way of example, it will be appreciated by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present invention. It will be appreciated by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present invention. The scope of the present invention is defined by the appended claims.
Claims
1. A loudspeaker diaphragm, characterized in that: include: The ethylene-acrylate rubber film layer and the EPDM rubber film layer are stacked, wherein the ethylene-acrylate rubber film layer is composed of ethylene acrylate carboxylic acid copolymer, and the density of the speaker diaphragm is less than 1.35g / cm 3 .
2. The loudspeaker diaphragm according to claim 1, characterized in that: The thickness of the EPDM rubber membrane layer accounts for 30% to 70% of the total thickness of the loudspeaker diaphragm.
3. The loudspeaker diaphragm according to claim 1, characterized in that: The reinforcing agent of the EPDM rubber film layer is at least one of carbon black, fumed silica, precipitated calcium carbonate and barium sulfate.
4. The loudspeaker diaphragm according to claim 3, characterized in that: In 100 parts of EPDM raw rubber, the content of the reinforcing agent is 20 parts to 65 parts.
5. The loudspeaker diaphragm according to claim 1, characterized in that: The reinforcing agent of the ethylene-acrylate rubber film layer includes at least one of carbon black, fumed silica, precipitated calcium carbonate and barium sulfate.
6. The loudspeaker diaphragm according to claim 5, characterized in that: In 100 parts of ethylene-acrylate raw rubber, the content of the reinforcing agent is 40 parts to 120 parts.
7. The loudspeaker diaphragm according to claim 1, characterized in that: The EPDM rubber film layer is cross-linked using a peroxide cross-linking agent.
8. The loudspeaker diaphragm according to claim 7, characterized in that: The peroxide crosslinking agent includes at least one of 1,3-1,4-di(tert-butylperoxyisopropyl)benzene, diisopropylbenzene peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, tert-butylisopropylbenzene peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)-3-hexyne, 4,4'-bis(tert-butylperoxy)valerate, 1,1'-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, and 2,4-dichlorobenzoylperoxide.
9. The loudspeaker diaphragm according to claim 1, characterized in that: The ethylene-acrylate rubber film layer uses an amine crosslinking agent, and the amine crosslinking agent includes at least one of hexamethylenediamine, hexamethylenediamine carbamate, triethylenetetramine, ethylenediphenylamine and di-o-tolylguanidine.
10. The loudspeaker diaphragm according to claim 1, characterized in that: The loudspeaker diaphragm is formed into a two-layer composite structure, wherein the two-layer composite structure includes a layer of the ethylene-acrylate rubber membrane layer and a layer of the EPDM rubber membrane layer; Alternatively, the loudspeaker diaphragm is formed into a three-layer composite structure, which includes two layers of the ethylene-acrylate rubber membrane layers and one layer of the EPDM rubber membrane layer, and the EPDM rubber membrane layer is located between the two layers of the ethylene-acrylate rubber membrane layers.
11. The loudspeaker diaphragm according to claim 10, characterized in that: The loudspeaker diaphragm is formed into a two-layer composite structure, and the loudspeaker diaphragm is formed by air pressure forming, wherein the EPDM rubber membrane layer is located between the ethylene-acrylate rubber membrane layer and the molding mold.
12. A sound-generating device, characterized in that: Comprising the loudspeaker diaphragm according to any one of claims 1 to 11.
13. An electronic device comprising the sound generating device according to claim 12.