Carbon material heating body and preparation method thereof
By combining carbon fiber, graphene oxide and metal oxide, and using ultrasonic stirring and hot pressing molding technology, the problem of insufficient thermal conductivity and mechanical properties of electric heating elements is solved, and efficient heat conduction and suitable carbon material heating elements are achieved.
Patent Information
- Application Number
- CN202410973078.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-11
AI Technical Summary
Existing electric heating elements such as nickel-chromium alloys have high density, low resistivity, slow heating rate, complex structure, and large thermal inertia. The carbon fiber heating materials are unevenly dispersed in the pulp, resulting in uneven conductivity, posing safety risks.
A heating element combining carbon fiber, graphene oxide and metal oxide is used. Through ultrasonic stirring and hot pressing molding technology, metal-carbon bonds are formed to improve thermal conductivity and mechanical properties, and a carbon material heating element with excellent thermal conductivity and simple structure is prepared.
It achieves efficient heat conduction and heat radiation, improves the thermal conductivity and mechanical properties of the heating element, reduces production costs, and is suitable for various energy fields.
Smart Images

Figure BDA0004955313380000051 
Figure BDA0004955313380000061 
Figure BDA0004955313380000091
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of carbon material heating elements, and in particular relates to a carbon material heating element and a preparation method thereof. Background Art
[0002] Electric heating uses electricity as energy, and provides a source of heat for the human body by converting electricity into heat energy through electric heating elements. It is generally composed of several parts such as power supply, heating element, temperature control device, safety protection device, etc., which are connected to each other by wires.
[0003] Metal heating elements in electric heating systems generally use materials such as metal foil, thin film coating, nickel wire, and metal mesh. The most commonly used heating element is nickel-chromium alloy. However, nickel-chromium alloy is still insufficient in the following aspects: nickel-chromium alloy has a high density and a thickness of several millimeters when used; low resistivity (about 10-6Ω·m), and still has low electrothermal conversion efficiency, low heating rate, and heating elements without automatic constant temperature and power compensation functions, which makes the electric heating system structure complex and has large thermal inertia. Iron-chromium-aluminum is a ferrite alloy, which has room temperature brittleness, 475℃ brittleness, and high temperature brittleness above 1000℃. The low high temperature strength caused by high temperature brittleness ultimately leads to a short service life of the electric heating element; the alloy has poor weldability and is difficult to repair.
[0004] Carbon materials such as carbon fiber, graphene, graphite, etc. are mainly composed of carbon. When carbon atoms are excited by electrons in the current, the electrons in the carbon atoms are in an excited state and produce energy level transitions, which cause vibrations with a wavelength of 4 to 20 microns. The electron vibrations generate heat and transmit heat radiation in the form of electromagnetic waves. It has excellent electrical and thermal conductivity and uniform heat generation. In recent years, it has been often used as a heating element. Due to its light weight and excellent performance, it is used in many fields, such as power transmission, heating films, etc.
[0005] Chinese patent CN117545113 A provides a graphene heating sheet and its preparation method. The patent uses the high electrothermal conversion rate of graphene and compounded with nano silver particles to prepare a graphene heating film element. The preparation process uses sulfur-containing organic solvents such as dimethyl sulfoxide. Sulfide is easily adsorbed on precious metals and is difficult to remove. During the later use, it is released into the air, which is easy to cause secondary pollution. In addition, silver is expensive and is not suitable for large-scale production and application.
[0006] Chinese patent CN102226325A discloses a far-infrared carbon fiber low-temperature conductive heating paper, including a raw pulp board, carbon fiber, nano far-infrared negative ion powder and a diffusant. This solution adds carbon fiber that has been carbonized, treated with water phase, and treated with hydrophilicity to the pulp after pulping, and then takes the mixed pulp to measure its resistance after homogenization and continued pulping. Although this solution has treated the carbon fiber with water phase and hydrophilicity, the resistance error does not fundamentally solve the problem of the hydrophobicity of carbon fiber and the difficulty of uniform dispersion in pulp slurry. The conductive paper has a low yield rate and the heat is not uniform. During use, problems such as electrical breakdown caused by uneven dispersion of carbon fiber may threaten personal safety.
[0007] To this end, it is necessary to prepare a heating element that is simple, universal, and has excellent thermal conductivity. Summary of the invention
[0008] The object of the present invention is to provide an improved carbon material heating element and a preparation method thereof.
[0009] In order to achieve the above object, a technical solution adopted by the present invention is:
[0010] A carbon material heating element, wherein the raw materials of the carbon material heating element include, by weight:
[0011] Carbon fiber: 100;
[0012] Metal oxides: 20-40;
[0013] Graphene oxide: 3-15;
[0014] Binder: 10-30;
[0015] Molding agent: 10~30.
[0016] In the present invention, carbon fiber refers to a fiber material that has been carbonized at high temperature and has a carbon content of more than 90%. Carbon fiber includes carbon fiber and graphite fiber. As a high-performance fiber, it has the advantages of high specific strength, high specific modulus, small thermal expansion coefficient, low friction coefficient, good low temperature resistance, and good thermal conductivity.
[0017] In some embodiments, the carbon fiber may be carbon fiber powder, carbon fiber short fiber, carbon fiber long fiber, carbon fiber filament, carbon fiber cloth, or carbon fiber felt. Considering the thorough mixing with each component and the simplicity of the preparation process, carbon fiber powder is preferred.
[0018] In some embodiments, the average particle size of the carbon fiber is 20 to 200 μm. If the particle size is smaller, it is not conducive to the overall mechanical properties of the heating element. If the particle size is larger, it is easy to cause uneven mixing and uneven heat conduction. More preferably, the average particle size of the carbon fiber is 50 to 150 μm.
[0019] In some embodiments, the metal oxide powder is a powder mainly composed of an oxide composed of two elements, a metal element and an oxygen element, which can bond with a carbon element in a high temperature oxygen-free environment to form a metal-carbon bond without an interface effect and conduct heat more rapidly. The metal oxide is a combination of one or more of iron oxide, nickel oxide, cobalt oxide, copper oxide, aluminum oxide, titanium oxide, and tungsten oxide. For better thermal conductivity, copper oxide and nickel oxide powders are preferred.
[0020] In some embodiments, the amount of the metal oxide powder is 20 to 40 parts by weight. A smaller amount will slow down the heat transfer, and a larger amount will easily cause metal sintering and agglomeration during high-temperature preparation, and uneven metal dispersion will lead to uneven heating. It is more preferably 25 to 35 parts by weight.
[0021] In some embodiments, the average particle size of the metal oxide is 1 to 100 nm, and the particle size of the oxide powder is nanometer-scale, which is conducive to uniform mixing and dispersion with graphene oxide, and more preferably 1 to 50 nm.
[0022] The graphene oxide is an oxide of graphene, wherein the graphene has carbon atoms in the form of sp 2 The single-layer hexagonal honeycomb lattice structure formed by hybrid bonding. The graphene oxide shows excellent physical, chemical and electrical properties, and there are multiple oxygen-containing functional groups coexisting on the basal surface and edge of the graphene oxide sheet skeleton. The functional groups rich in the surface are easy to bond with metal and carbon fiber materials, enhancing the thermal conductivity of the component.
[0023] In some embodiments, the amount of graphene oxide is 3 to 15 parts by weight. A small amount of graphene oxide is not easy to mix with metal oxides; while graphene oxide is light, a large amount affects the overall mechanical properties of the heating element, and its amount is preferably 5 to 13 parts by weight.
[0024] In some embodiments, the specific surface area of the graphene oxide is 500 to 1500 m 2 / g, a smaller specific surface area is not conducive to coating metal oxide powders, and a larger specific surface area requires more graphene oxide, which increases the preparation cost. The specific surface area of graphene oxide is preferably 800-1300m 2 / g.
[0025] The binder is used to bond metal oxides, graphene oxide, and carbon fibers. The amount of the binder is 10 to 30 parts by weight, and is preferably 15 to 25 parts by weight in consideration of bonding properties.
[0026] In some embodiments, the binder may be C1 to C 12 Monohydric alcohol, C2~C 12A combination of one or more of diols or polyethylene glycols, preferably ethylene glycol for better adhesion.
[0027] In some embodiments, the metal oxide powder has an average particle size of 1 to 100 nm.
[0028] In some embodiments, the molding agent includes a combination of one or more of thermoplastic acrylic resin, polyethylene, and polypropylene. Adding the molding agent facilitates hot pressing molding after heating.
[0029] The thermoplastic acrylic resin is a type of thermoplastic resin made by polymerizing acrylic acid, methacrylic acid and its derivatives (such as esters, nitriles, and amides). It can better bond the components of the heating element so that the heating element can have mechanical strength after bonding and molding. Based on 100 parts by weight of carbon fiber, the amount of thermoplastic acrylic resin is 10 to 30 parts by weight; if the amount of thermoplastic acrylic resin is less, the bonding effect of the heating element is not good, resulting in reduced mechanical properties, and even separation of the bonding parts after long-term use; if the amount of thermoplastic acrylic resin is more, the thermoplastic acrylic resin softens in a high temperature environment, resulting in reduced mechanical properties of the bonding parts and separation of the bonding parts. Furthermore, the amount of thermoplastic acrylic resin is preferably 15 to 25 parts by weight.
[0030] In some embodiments, the thermoplastic acrylic resin has a melt index of 5 to 10 g / 10 min at 230°C.
[0031] Another technical solution adopted by the present invention is:
[0032] A method for preparing the carbon material heating element comprises the following steps:
[0033] S1, adding metal oxide to graphene oxide to obtain a first mixture;
[0034] S2, adding the first mixture to a binder to obtain a second mixture;
[0035] S3, adding carbon fiber to the second mixture to obtain a pre-embroided body;
[0036] S4, placing the pre-embroided body into a reactor, and heating, cooling, and grinding the pre-embroided body under nitrogen protection to obtain a heating element;
[0037] S5. Mix the heating element and the forming agent at high temperature, form them into a certain shape by hot pressing, and obtain the carbon material heating element after cooling and pressure relief.
[0038] In some embodiments, in step S1, metal oxide powder is added to graphene oxide, ultrasonicated for 0.5 to 1 hour, and stirred at room temperature for 0.5 to 1 hour to obtain a first mixture. The metal oxide powder is allowed to enter the pores of the graphene oxide powder by mixing in a manner such as ultrasonication and stirring.
[0039] In some embodiments, in step S2, the first mixture is added to the binder, ultrasonicated for 0.5 to 1 hour, and stirred and impregnated at room temperature for 1 to 3 hours to obtain a second mixture. Longer ultrasonic and stirring impregnation can further allow the graphene oxide to cover the metal oxide powder, while bonding the metal oxide powder and graphene oxide, which is conducive to the formation of metal-carbon bonds in the later stage.
[0040] In some embodiments, in step S3, the carbon fiber is added to the second mixture, ultrasonicated for 0.5 to 1 hour, stirred and impregnated at room temperature for 1 to 2 hours, and then mixed for 0.5 to 1 hour using a high-speed ball mill to obtain a pre-embroided body. The components are further uniformly mixed using a high-speed ball mill.
[0041] In some embodiments, in step 4, the pre-embroided body is placed in a reactor, and under nitrogen protection, the temperature is raised to 150-300°C, the residence time is 0.5-2h, and the stirring speed is 300-600r / min; then the temperature is raised to 1000-1500°C, the residence time is 4-8h, the stirring speed is 10-200r / min, and then the temperature is lowered and ground to obtain a heating element. The temperature is raised twice, and the boiling point of the binder such as ethylene glycol is 200°C. Reacting near its boiling point temperature is conducive to sufficient reaction, and the porosity of the material can also be increased, which is conducive to heat transfer; if this temperature is not increased, the binder will vaporize rapidly, the bonding force will be reduced, which is not conducive to the tensile properties of the material. The reaction at 1000-1500°C forms a metal / C bond, which has better thermal conductivity.
[0042] In some embodiments, in step S5, the heating element and the thermoplastic acrylic resin are mixed evenly at a high temperature, and then hot-pressed to obtain the carbon material heating element.
[0043] In some embodiments, in step S5, the temperature is 100-150°C, and the obtained carbon material heating element has better thermal conductivity and mechanical properties.
[0044] In some embodiments, in step S5, the hot pressing pressure is 10-30 MPa, and the obtained carbon material heating element has better thermal conductivity and mechanical properties.
[0045] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0046] The carbon material heating element provided by the present invention coordinates carbon fiber, graphene oxide, and metal oxide, and the obtained carbon material heating element has better thermal conductivity and heat dissipation; the metal is embedded in the carbon body to form a metal-carbon bond, the charge transfer is rapid, and the thermal efficiency is better; the carbon material heating element is easy to prepare into a variety of shapes, meeting a variety of application scenarios, and has strong universality; the carbon material heating element is suitable for a variety of energy fields, such as heating cables, home heaters, etc. DETAILED DESCRIPTION
[0047] The present invention is further described below in conjunction with the illustrated embodiments.
[0048] Provide examples 1-15 and comparative examples 1-7, the raw materials used in each example and comparative example are as follows:
[0049]
Carbon Fiber
[0050] A1: MLD-30, carbon fiber powder produced by Toray Industries, Ltd., Japan, with a fiber length of 30μm.
[0051] A2: MLD-300, carbon fiber powder produced by Toray Industries, Ltd., Japan, with a fiber length of 130μm.
[0052]
Metal oxides
[0053] B1: Copper oxide, DK-CuO nano copper oxide powder produced by Beijing Dekedaojin Technology Co., Ltd., with an average particle size of 40nm.
[0054] B2: Nickel oxide, DK-NiO nano nickel oxide powder produced by Beijing Dekedaojin Technology Co., Ltd., with an average particle size of 30nm.
[0055]
Graphene oxide
[0056] C1: Graphene oxide, RGO01 7440-44-0 graphene oxide produced by Suzhou Carbon Graphene Technology Co., Ltd., with a specific surface area of 1200m 2 / g.
[0057] C2: Graphene oxide, GO03 7440-44-0 graphene oxide produced by Suzhou Tanfeng Graphene Technology Co., Ltd., with a specific surface area of 300m 2 / g.
[0058]
Binder
[0059] D: Ethylene glycol, produced by Sinopharm Chemical Reagent Co., Ltd. 10009818 ethylene glycol.
[0060]
Thermoplastic acrylic resin
[0061] E1: Polymethyl methacrylate, IRS404 produced by Mitsubishi Chemical, melt index 8.5g / 10min at 230℃.
[0062] E2: Polymethyl methacrylate, IRS204 produced by Mitsubishi Chemical, melt index 14.5g / 10min at 230℃.
[0063] The raw material formulas of Examples 1-15 and Comparative Examples 1-7 are shown in Table 1.
[0064] Table 1 Raw material formula of Examples 1-15 and Comparative Examples 1-7
[0065]
[0066]
[0067] The preparation method of the carbon material heating element of Examples 1-13 is as follows:
[0068] S1. Adding metal oxide powder to graphene oxide, ultrasonicating for 0.5 to 1 h, and stirring at room temperature for 0.5 to 1 h to obtain a first mixture;
[0069] S2, adding the first mixture to the binder, ultrasonicating for 0.5 to 1 hour, stirring and impregnating at room temperature for 1 to 3 hours, to obtain a second mixture;
[0070] S3, adding carbon fiber to the second mixture, ultrasonicating for 0.5 to 1 hour, stirring and impregnating at room temperature for 1 to 2 hours, and then using a high-speed ball mill to mix for 0.5 to 1 hour to obtain a pre-embroided body;
[0071] S4, placing the pre-embroided body into a reactor, under nitrogen protection, heating to 200°C, staying for 2 hours, stirring at a speed of 400r / min, then heating to 1300°C, staying for 5 hours, stirring at a speed of 100r / min, then cooling and grinding to obtain a heating element;
[0072] S5. Add thermoplastic acrylic resin to the heating element and mix in an internal mixer at 110°C for 30 minutes. Take out the uniformly mixed material, pour it into a mold, and mold it at 110°C and 20MPa to obtain a carbon material heating element with a length of 10cm, a width of 6cm, and a thickness of 4cm.
[0073] The preparation method of the carbon material heating element of Example 14 is as follows:
[0074] S1. Adding metal oxide powder to graphene oxide, ultrasonicating for 0.5 to 1 h, and stirring at room temperature for 0.5 to 1 h to obtain a first mixture;
[0075] S2, adding the first mixture to the binder, ultrasonicating for 0.5 to 1 hour, stirring and impregnating at room temperature for 1 to 3 hours, to obtain a second mixture;
[0076] S3, adding carbon fiber to the second mixture, ultrasonicating for 0.5 to 1 hour, stirring and impregnating at room temperature for 1 to 2 hours, and then using a high-speed ball mill to mix for 0.5 to 1 hour to obtain a pre-embroided body;
[0077] S4, placing the pre-embroided body into a reactor, heating it to 1300°C under nitrogen protection, staying for 5 hours, stirring at a speed of 100 r / min, and then cooling and grinding to obtain a heating element;
[0078] S5. Add thermoplastic acrylic resin to the heating element and mix in an internal mixer at 110°C for 30 minutes. Take out the uniformly mixed material, pour it into a mold, and press it at 110°C and 20MPa to obtain a carbon material heating element with a length of 10cm, a width of 6cm, and a thickness of 4cm.
[0079] The preparation method of the carbon material heating element of Example 15 is as follows:
[0080] S1. Adding metal oxide powder to graphene oxide, ultrasonicating for 0.5 to 1 h, and stirring at room temperature for 0.5 to 1 h to obtain a first mixture;
[0081] S2, adding the first mixture to the binder, ultrasonicating for 0.5 to 1 hour, stirring and impregnating at room temperature for 1 to 3 hours, to obtain a second mixture;
[0082] S3, adding carbon fiber to the second mixture, ultrasonicating for 0.5 to 1 hour, stirring and impregnating at room temperature for 1 to 2 hours, and then using a high-speed ball mill to mix for 0.5 to 1 hour to obtain a pre-embroided body;
[0083] S4, placing the pre-embroided body into a reactor, under nitrogen protection, heating to 200°C, staying for 2 hours, stirring at a speed of 400r / min, then heating to 900°C, staying for 5 hours, stirring at a speed of 100r / min, then cooling and grinding to obtain a heating element;
[0084] S5. Add thermoplastic acrylic resin to the obtained heating element, mix in an internal mixer at 110°C for 30 minutes, take out the evenly mixed material, pour it into a mold, and press at 110°C and 20MPa pressure to obtain a carbon material heating element with a length of 10cm, a width of 6cm, and a thickness of 4cm.
[0085] Comparative Example 1-2 is to weigh the materials and thermoplastic acrylic resin according to the formula described in Table 1, and mix them in an internal mixer at 110°C for 30 minutes. After taking out the uniformly mixed materials, pour them into a mold and mold them at 110°C and 20MPa pressure to obtain a carbon material heating element with a length of 10cm, a width of 6cm, and a thickness of 4cm.
[0086] The preparation method of the carbon material heating element of Comparative Example 3 is as follows:
[0087] S1, adding graphene oxide to the binder, ultrasonicating for 0.5 to 1 hour, and stirring and impregnating at room temperature for 1 to 3 hours to obtain a first mixture;
[0088] S2, adding carbon fiber to the first mixture, ultrasonically treating for 0.5 to 1 hour, stirring and impregnating at room temperature for 1 to 2 hours, and then mixing for 0.5 to 1 hour using a high-speed ball mill to obtain a pre-embroided body;
[0089] S3, placing the pre-embroided body into a reactor, under nitrogen protection, heating to 200°C, staying for 2 hours, stirring at a speed of 400r / min, then heating to 900°C, staying for 5 hours, stirring at a speed of 100r / min, then cooling and grinding to obtain a heating element;
[0090] S4. Add thermoplastic acrylic resin to the obtained heating element, mix in an internal mixer at 110°C for 30 minutes, take out the evenly mixed material, pour it into a mold, and press at 110°C and 20MPa pressure to obtain a carbon material heating element with a length of 10cm, a width of 6cm, and a thickness of 4cm.
[0091] The preparation method of the carbon material heating element of Comparative Example 4 is as follows:
[0092] S1, adding metal oxide powder to the binder, ultrasonicating for 0.5 to 1 hour, stirring and impregnating at room temperature for 1 to 3 hours to obtain a first mixture;
[0093] S2, adding carbon fiber to the first mixture, ultrasonically treating for 0.5 to 1 hour, stirring and impregnating at room temperature for 1 to 2 hours, and then mixing for 0.5 to 1 hour using a high-speed ball mill to obtain a pre-embroided body;
[0094] S3, placing the pre-embroided body into a reactor, under nitrogen protection, heating to 200°C, staying for 2 hours, stirring at a speed of 400r / min, then heating to 900°C, staying for 5 hours, stirring at a speed of 100r / min, then cooling and grinding to obtain a heating element;
[0095] S4. Add thermoplastic acrylic resin to the obtained heating element, mix in an internal mixer at 110°C for 30 minutes, take out the evenly mixed material, pour it into a mold, and press at 110°C and 20MPa pressure to obtain a carbon material heating element with a length of 10cm, a width of 6cm, and a thickness of 4cm.
[0096] The preparation method of the carbon material heating element of Comparative Example 5 is as follows:
[0097] S1, adding metal oxide powder to graphene oxide, ultrasonicating for 0.5 to 1 h, stirring at room temperature for 1 to 3 h, to obtain a first mixture;
[0098] S2, adding carbon fiber to the first mixture, ultrasonicating for 0.5 to 1 hour, stirring at room temperature for 1 to 2 hours, and then using a high-speed ball mill to mix for 0.5 to 1 hour to obtain a pre-embroided body;
[0099] S3, placing the pre-embroided body into a reactor, under nitrogen protection, heating to 200°C, staying for 2 hours, stirring at a speed of 400r / min, then heating to 900°C, staying for 5 hours, stirring at a speed of 100r / min, then cooling and grinding to obtain a heating element;
[0100] S4. Add thermoplastic acrylic resin to the obtained heating element, mix in an internal mixer at 110°C for 30 minutes, take out the evenly mixed material, pour it into a mold, and press at 110°C and 20MPa pressure to obtain a carbon material heating element with a length of 10cm, a width of 6cm, and a thickness of 4cm.
[0101] The preparation method of the carbon material heating element of Comparative Example 6 is as follows:
[0102] S1. After weighing the metal oxide powder, graphene oxide, binder and carbon fiber according to the formula shown in Table 1, ultrasonically treat for 2-4 hours, and stir and immerse for 3-6 hours at room temperature to obtain a pre-embroided body;
[0103] S2, placing the pre-embroided body into a reactor, under nitrogen protection, heating to 200°C, staying for 2 hours, stirring at a speed of 400r / min, then heating to 1300°C, staying for 5 hours, stirring at a speed of 100r / min, then cooling and grinding to obtain a heating element;
[0104] S3. Add thermoplastic acrylic resin to the heating element and mix in an internal mixer at 110°C for 30 minutes. Take out the uniformly mixed material, pour it into a mold, and mold it at 110°C and 20MPa to obtain a carbon material heating element with a length of 10cm, a width of 6cm, and a thickness of 4cm.
[0105] The preparation method of the carbon material heating element of Comparative Example 7 is as follows:
[0106] S1, adding metal oxide powder to graphene oxide, ultrasonicating for 0.5 to 1 hour, stirring and impregnating at room temperature for 1 to 3 hours, to obtain a first mixture;
[0107] S2, adding carbon fiber to the first mixture, ultrasonically treating for 0.5 to 1 hour, stirring and impregnating at room temperature for 1 to 2 hours, and then mixing for 0.5 to 1 hour using a high-speed ball mill to obtain a pre-embroided body;
[0108] S3, placing the pre-embroided body into a reactor, under nitrogen protection, heating to 200°C, staying for 2 hours, stirring at a speed of 400r / min, then heating to 900°C, staying for 5 hours, stirring at a speed of 100r / min, then cooling and grinding to obtain a heating element;
[0109] The following tests were performed on the carbon material heating elements of Examples 1-15 and Comparative Examples 1-7. Unless otherwise specified, all tests were performed at 25°C.
[0110] 1. Tensile strength: tested according to GB / T 1040.1-2018;
[0111] 2. Thermal conductivity: Tested in accordance with national standard GB / T 10297-2015.
[0112] Table 2 Performance data of carbon material heating elements of Examples 1-15 and Comparative Examples 1-7
[0113]
[0114] As shown in Table 2, compared with Example 1-7, the carbon material heating element prepared in Example 1-15 has better thermal conductivity and superior mechanical properties; the carbon material heating element prepared in Example 1-15 is simple and convenient to prepare, and the prepared heating element has strong adaptability and is convenient for large-scale production.
[0115] In Comparative Example 6, metal oxide powder, graphene oxide, binder, and carbon fiber are mixed at the same time, which is prone to uneven mixing, and the obtained carbon material heating element has poor thermal conductivity and poor mechanical properties. In Examples 1-15, the materials are added layer by layer, and the mixing is more uniform. The obtained carbon material heating element has better thermal conductivity and superior mechanical properties. In Comparative Example 7, no thermoplastic acrylic resin can be formed.
[0116] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A carbon material heating element, characterized in that: In parts by weight, the raw materials of the carbon material heating element include: Carbon fiber: 100; Metal oxides: 20-40; Graphene oxide: 3-15; Binder: 10-30; Molding agent: 10~30.
2. The carbon material heating element according to claim 1, characterized in that: The metal oxide is a combination of one or more of iron oxide, nickel oxide, cobalt oxide, copper oxide, aluminum oxide, titanium oxide, and tungsten oxide.
3. The carbon material heating element according to claim 1, characterized in that: The average particle size of the metal oxide is 1 to 100 nm.
4. The carbon material heating element according to claim 1, characterized in that: The specific surface area of the graphene oxide is 500 to 1500 m 2 / g.
5. The carbon material heating element according to claim 1, characterized in that: The binder is C1~C 12 Monohydric alcohol, C2~C 12 A combination of one or more of diols and polyethylene glycols.
6. The carbon material heating element according to claim 1, characterized in that: The average particle size of the metal oxide powder is 1 to 100 nm; and / or, the average particle size of the carbon fiber is 20 to 200 μm.
7. The carbon material heating element according to any one of claims 1 to 6, characterized in that: The molding agent includes a combination of one or more of thermoplastic acrylic resin, polyethylene and polypropylene.
8. A method for preparing a carbon material heating element according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, adding metal oxide to graphene oxide to obtain a first mixture; S2, adding the first mixture to a binder to obtain a second mixture; S3, adding carbon fiber to the second mixture to obtain a pre-embroided body; S4, placing the pre-embroided body into a reactor, and heating, cooling, and grinding the pre-embroided body under nitrogen protection to obtain a heating element; S5. Mix the heating element and the molding agent at high temperature, and obtain the carbon material heating element by hot pressing.
9. The method for preparing a carbon material heating element according to claim 8, characterized in that: In step S4, the pre-embroided body is placed in a reactor, and under nitrogen protection, the temperature is first raised to 150-300°C, the residence time is 0.5-2h, and the stirring speed is 300-600r / min; then the temperature is raised to 1000-1500°C, the residence time is 4-8h, and the stirring speed is 10-200r / min, followed by cooling and grinding to obtain a carbon material heating element.
10. The method for preparing a carbon material heating element according to claim 8, characterized in that: The method further comprises: In step S5, the high temperature is 100-150°C.