Metal foil with carrier, metal-clad laminate and printed circuit board

By adding a carrier and peeling layer on the metal foil and performing surface treatment, its tensile strength and heat resistance are improved, the problem of metal foil breakage under high temperature hot pressing is solved, and the stability of printed circuit board manufacturing is significantly improved. quality.

CN118765232A9Pending Publication Date: 2024-12-06MITSUI MINING & SMELTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023827.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-14
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Under high-temperature hot pressing conditions, the metal foil with the carrier is prone to break or cracking, affecting the manufacturing process of the printed circuit board.

Method used

By adding a carrier and a peeling layer on the metal foil, the tensile strength of the carrier and metal foil is ensured to reach more than 50.0kgf/mm2, and the surface of the metal foil is roughened, rust-proof and silane coupling agent are treated to form a multi-layer structure To improve its strength and heat resistance.

Benefits of technology

It effectively suppresses breakage and cracking of metal foil, improves the stability and operability of the printed circuit board manufacturing process, and extends the service life of the metal foil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765232A9_ABST
    Figure CN118765232A9_ABST
Patent Text Reader

Abstract

Provided is a metal foil with a carrier capable of suppressing the occurrence of breakage or cracking of the metal foil during handling. The metal foil with a carrier comprises a carrier, a peeling layer and a metal foil in this order, and the tensile strength of the carrier is 50.0 kgf / mm 2 Above, and the tensile strength of the metal foil is 50.0kgf / mm 2 above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a metal foil with a carrier, a metal-clad laminate and a printed circuit board. Background Art

[0002] As a material for manufacturing printed circuit boards, metal foil with a carrier is widely used.

[0003] When the metal foil with a carrier is hot-pressed at a high temperature (for example, 250° C. or higher), there is

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2015 / 080052 Summary of the invention

[0007] However, due to the efforts towards SDGs (Sustainable Development Goals) and the promotion of carbon neutrality in recent years,

[0008] The present inventors have obtained the following findings: in a metal foil with a carrier, by

[0009] Therefore, an object of the present invention is to provide a product capable of suppressing breakage or cracking of a metal foil during handling.

[0010] According to the present invention, the following aspects are provided.

[0011] [Method 1]

[0012] A metal foil with a carrier, which comprises a carrier, a peeling layer and a metal foil in this order.

[0013] The tensile strength of the carrier is 50.0 kgf / mm 2 Above, and the tensile strength of the metal foil is

[0014] [Method 2]

[0015] The metal foil with a carrier according to Embodiment 1, wherein after heating at 250° C. for 60 minutes, the front

[0016] [Method 3]

[0017] The metal foil with a carrier according to embodiment 1 or 2, wherein the carrier and the metal foil are

[0018] [Method 4]

[0019] The metal foil with a carrier according to any one of aspects 1 to 3, wherein the thickness of the carrier is

[0020] [Method 5]

[0021] The metal foil with a carrier according to any one of aspects 1 to 4, wherein the thickness of the metal foil is

[0022] [Method 6]

[0023] The metal foil with a carrier according to any one of aspects 1 to 5, wherein

[0024] [Method 7]

[0025] The metal foil with a carrier according to any one of aspects 1 to 6, wherein the release layer and

[0026] [Method 8]

[0027] A metal-clad laminate comprising the metal foil with a carrier according to any one of aspects 1 to 7.

[0028] [Method 9]

[0029] A printed wiring board includes the metal foil with a carrier according to any one of aspects 1 to 7.

[0030] [Method 10]

[0031] A method for manufacturing a printed circuit board, characterized in that the method comprises using any one of methods 1 to 7 BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a process flow chart for producing a metal-clad laminate using a metal foil with a carrier.

[0033] Figure 2 : is a top view of the copper foil with a carrier cut out and used for the measurement of the number of cracks in the examples,

[0034] Figure 3 Yes Figure 2 Flow chart of the twisting process of the copper foil with carrier. DETAILED DESCRIPTION

[0035] Metal foil with carrier

[0036] The metal foil with a carrier of the present invention comprises a carrier, a peeling layer and a metal foil in this order.

[0037] As described above, the occurrence of breakage or cracking of the metal foil during the handling of the metal foil with a carrier may

[0038] The above problems are effectively solved by the metal foil with carrier of the present invention.

[0039] Therefore, the tensile strength of the carrier is 50.0kgf / mm 2 Above, preferably 50.0kgf / mm 2 Above and

[0040] In addition, the tensile strength of the metal foil is 50.0kgf / mm 2 Above, preferably 50.0kgf / mm 2 above

[0041] The ratio of the tensile strength TS2 of the metal foil to the tensile strength TS1 of the carrier (= TS2 / TS1) is preferably

[0042] Further effectively suppressing breakage and cracking of metal foil in the printed circuit board manufacturing process

[0043] The carrier is a support for supporting the metal foil to improve its handling. The typical carrier includes metal

[0044] The metal foil is preferably copper foil or copper alloy foil, more preferably copper foil. The metal foil can be electrolytic foil and

[0045] If necessary, the surface of the metal foil may be roughened to form a roughened layer.

[0046] If necessary, the surface of the metal foil may be subjected to rust-proof treatment to form a rust-proof treatment layer.

[0047] If necessary, the surface of the metal foil may be treated with a silane coupling agent to form a silane coupling agent.

[0048] Therefore, the metal foil with a carrier preferably further comprises a plurality of roughening particles selected from the group consisting of

[0049] The metal foil with carrier has a peeling layer on the carrier. The peeling layer has a peeling strength that weakens the carrier.

[0050] Other functional layers may also be provided between the release layer and the carrier and / or the metal foil.

[0051] Method for producing metal foil with carrier

[0052] The metal foil with a carrier of the present invention can be prepared by (1) preparing a carrier, (2) forming a release film on the carrier,

[0053] (1) Preparation of vector

[0054] First, a carrier is prepared as a support. A typical carrier comprises a metal layer.

[0055] When using electrolytic copper foil as a carrier, the conditions for electrolytic foil production are preferably as follows. That is,

[0056] (2) Formation of the peeling layer

[0057] A peeling layer is formed on the carrier. The peeling layer can be any one of an organic peeling layer and an inorganic peeling layer.

[0058] (3) Formation of metal foil

[0059] The metal foil is formed on the peeling layer. For example, the metal foil can be formed by chemical metal plating and electrolytic metal plating.

[0060] If necessary, the surface of the metal foil can be roughened, rust-proofed and / or silane-treated.

[0061] Metal-clad laminate

[0062] The metal foil with a carrier of the present invention is preferably used for production of a metal-clad laminate for a printed wiring board.

[0063] Printed Circuit Board

[0064] The metal foil with a carrier of the present invention is preferably used for the production of printed circuit boards.

[0065] Example

[0066] The present invention is further specifically described by the following examples.

[0067] Example 1~Example 11

[0068] Copper foil with carrier was produced and evaluated as follows.

[0069] (1) Preparation of vector

[0070] For Examples 1 to 6 and 11, the following copper electrolyte solutions, cathodes and anodes were used:

[0071] <Composition of copper electrolyte>

[0072] -Copper concentration: 80g / L

[0073] - Sulfuric acid concentration: 250g / L

[0074] -Chlorine concentration: 1.5mg / L

[0075] - Gelatin concentration: 2mg / L

[0076] On the other hand, for Examples 7 to 10, the copper electrolyte, cathode and

[0077] <Composition of copper electrolyte>

[0078] -Copper concentration: 80g / L

[0079] - Sulfuric acid concentration: 300g / L

[0080] -Chlorine concentration: 30mg / L

[0081] -Glue concentration: 5mg / L

[0082] (2) Formation of the peeling layer

[0083] The electrode surface of the acid-washed support was placed in a solution containing 1 g / L carboxybenzotriazole (CBTA)

[0084] (3) Formation of auxiliary metal layer

[0085] The support having the organic release layer formed thereon was immersed in a solution containing nickel at a concentration of 20 g / L prepared by using nickel sulfate.

[0086] (4) Formation of ultra-thin copper foil

[0087] The support having the auxiliary metal layer is immersed in a copper solution having the following composition.

[0088] <Solution Composition>

[0089] -Copper concentration: 60g / L

[0090] - Sulfuric acid concentration: 200g / L

[0091] -CBTA concentration: 5.0 ppm (Examples 1, 4-8 and 11) or 0 ppm (Examples 2, 3, 9 and 10)

[0092] (5) Roughening treatment

[0093] The surface of the ultra-thin copper foil thus formed is roughened to form a roughened surface.

[0094] (6) Anti-rust treatment

[0095] The roughened surface of the copper foil with carrier obtained is subjected to a zinc-nickel alloy plating treatment and

[0096] (7) Silane coupling agent treatment

[0097] Roughening treatment of copper foil with carrier by adsorbing a commercially available aqueous solution containing a silane coupling agent

[0098] (8) Heat treatment

[0099] For Examples 3 and 10, the copper foil with carrier treated with silane coupling agent was heated at 175°C for 5 minutes.

[0100] (9) Evaluation

[0101] The copper foil with a carrier thus obtained was evaluated for various properties as follows.

[0102] (9a) Thickness

[0103] The thickness of the carrier and the ultra-thin copper foil included in the copper foil with a carrier was measured as follows.

[0104] (9b) Normal tensile strength

[0105] The tensile strength of the carrier and the ultra-thin copper foil was measured as follows. First, the tensile strength of the carrier and the ultra-thin copper foil was measured according to IPC-TM650 2.4.18.

[0106] (9c) Tensile strength after heating

[0107] Before measuring the tensile strength, the copper with carrier was dried in an oven at 250°C in an atmospheric atmosphere.

[0108] (9d) Determination of crack number

[0109] As an indicator of the damage resistance of the ultra-thin copper foil, the number of cracks was measured as follows.

[0110] [Table 1]

[0111] Table 1

[0113] ★ indicates comparative examples.

Claims

1. A metal foil with a carrier, comprising a carrier, a release layer and a metal foil in this order, The tensile strength of the carrier is 50.0 kgf / mm 2 Above, and the tensile strength of the metal foil is 2. The metal foil with a carrier according to claim 1, wherein Heat at 250°C for 60 minutes 3. The metal foil with a carrier according to claim 1 or 2, wherein The carrier and the gold 4. The metal foil with a carrier according to claim 1 or 2, wherein The thickness of the carrier is 5. The metal foil with a carrier according to claim 1 or 2, wherein The thickness of the metal foil 6. The metal foil with a carrier according to claim 1 or 2, wherein: On the metal foil 7. The metal foil with a carrier according to claim 1 or 2, wherein: In the peeling layer and 8 . A metal-clad laminate comprising the metal foil with a carrier according to claim 1 or 2. 9 . A printed wiring board comprising the metal foil with a carrier according to claim 1 or 2 .

10. A method for manufacturing a printed circuit board, characterized in that: Use of claim 1 or 2