Laminated film

By designing a regular arrangement of three different thermoplastic resin layers, the problem of interlayer peeling in reflective light control films during long-term use was solved, achieving high reflectivity and low-cost optical properties, suitable for electronic information equipment and automotive fields.

CN118765233APending Publication Date: 2024-10-11TORAY INDUSTRIES INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380023909.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2023-03-08
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing reflective light control films are prone to interlayer delamination during long-term use, making it difficult to maintain broadband/high reflectivity optical properties, and they are also costly to manufacture.

Method used

A laminated film design consisting of three different thermoplastic resin layers arranged in a regular pattern to meet specific thickness ratio and refractive index conditions is adopted. By adjusting the combination of thermoplastic resin layers and the lamination process, interlayer delamination is reduced and reflectivity and interlayer adhesion are improved.

Benefits of technology

It achieves reduced interlayer delamination during long-term use, maintains broadband/high reflectivity optical properties, reduces manufacturing costs, and is suitable for light control films in electronic information equipment and automotive fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765233A_ABST
    Figure CN118765233A_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a laminated film that does not undergo interlayer peeling even in long-term continuous use and exhibits excellent visible light reflection characteristics, and is characterized by continuously having three or more regular arrangements comprising three different types of thermoplastic resin layers, and the following condition X and the following condition Y are satisfied at the same time. Condition X: When three different types of thermoplastic resin layers are set as A layer, B layer, and C layer, the thickness ratio (A / B) of A layer to B layer in the regular arrangement is 0.60-5.00 inclusive, and the thickness ratio (C / B) of C layer to B layer in the regular arrangement is 0.70-5.00 inclusive. Condition Y: The maximum reflectance at a wavelength of 400-800 nm is 35% or more and 100% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a laminated film which can reduce interlayer delamination even in long-term continuous use and exhibits excellent visible light reflection characteristics. Background Art

[0002] Light control films that can selectively block / transmit light of a specific wavelength band have been put into practical use in a variety of fields for the purpose of preventing the internal environment of the product or the components from deteriorating due to environmental factors such as light and heat rays, or extracting only light of a specific wavelength band to develop a desired color tone. In particular, there is a high demand for light control films in the field of electronic information equipment. With the trend of thinner displays in recent years, the demand for thinner light control films as one of the components has also increased. In addition, even in the automotive field, when developing electric vehicles, for the purpose of lightweighting, the components that used to use metal have been replaced by resin molded products and sheets that show a metallic tone. Metallic-toned films and sheets that show a high visible light reflectivity like metals have also received attention.

[0003] As a method for selectively shielding light of a specific wavelength band, an absorption-type light control film in which a light absorber such as a dye / pigment / ultraviolet absorber / heat ray absorber is added to the resin constituting the film has become popular (Patent Document 1). However, the light absorption characteristics of such an absorption-type light control film depend on the product of the added concentration of the light absorber and the film thickness, and the added concentration of the light absorber needs to be high in order to thin the film. However, if the amount of the light absorber is increased in order to maintain the light absorption characteristics, surface precipitation becomes significant depending on the type of the light absorber, and film defects caused by contamination of the film-making process become a problem. On the other hand, if the amount of the light absorber is reduced in order to avoid the above-mentioned problems, insufficient light absorber and reduced light absorption characteristics become a problem. Furthermore, since the light absorber needs to be selected according to the wavelength band to be shielded, in the case of shielding a wide wavelength band, a large amount of addition is required by using multiple light absorbers in combination. In addition, when dyes and pigments are selected, the former lacks light resistance, and the latter also has the disadvantages of not being able to obtain color selectivity due to the absorption performance covering a wide range.

[0004] As a light control film that overcomes the shortcomings of such an absorption-type light control film, a reflective light control film that utilizes interference reflection based on the light interference theory by laminating layers having different refractive indices along the film thickness direction has attracted attention. As an example of a method for manufacturing a reflective light control film, it is known that a method is used to repeatedly laminate metal thin film layers showing different refractive indices by sputtering / evaporation technology. However, when obtaining a light control film by such a method, since a plurality of different metal layers need to be repeatedly laminated in sequence, a large number of processes are repeated, thereby increasing the manufacturing cost. In addition, in such a light control film, there are also problems such as cracking / peeling of the sputtered / evaporated film due to fatigue and impairment of the reflective properties in applications requiring bending.

[0005] Therefore, as a different reflective light control film, a light control film in which not only a metal thin film layer but also a thermoplastic resin layer having different refractive indices is laminated is actively studied. A light control film in which thermoplastic resin layers having different refractive indices are laminated is obtained by laminating thermoplastic resins derived from different extruders in a desired arrangement in dozens to hundreds of layers at a time using a special lamination device such as a square mixer or a feed block. Such a light control film is different from a film composed of a laminate containing a metal thin film layer, and also has the advantage that the target reflection band can be easily changed by only changing the thickness of the film through a stretching process, etc.

[0006] Among them, a light control film composed of (AB)x (x is a natural number indicating the number of repetitions) in which two thermoplastic resin layers (A layer and B layer) having different refractive indices are alternately stacked has been reported by multiple known technologies. For example, the following multiple technologies have been reported: a technology for reflecting light in a wide band by continuously imparting an inclined distribution to the layer thickness, a technology for designing the optical thickness to be 1 / 4 of the wavelength in order to suppress unnecessary reflection bands on the short wavelength side (called higher-order reflection) generated other than the desired band (patent documents 2 and 3), a technology for implementing a special layer thickness pattern formation with a ratio of 1:7:1 (patent documents 4 and 5), etc.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2013-210598

[0010] Patent Document 2: Japanese Patent Application No. 2004-503402

[0011] Patent Document 3: Japanese Patent Publication No. 8-503312

[0012] Patent Document 4: U.S. Patent No. 5,360,659

[0013] Patent Document 5: Japanese Patent Application Publication No. 2018-205615 Summary of the invention

[0014] Problems to be solved by the invention

[0015] However, in the reflective light control film composed of (AB)x (x is a natural number indicating the number of repetitions) disclosed in patent documents 2 to 5, in order to expand the reflection band (broadband) and improve the reflectivity (high reflectivity), it is necessary to increase the number of layers or increase the refractive index difference between the two thermoplastic resin layers. In the former case, since the film becomes thicker due to the increase in the number of layers, it becomes a solution that goes against the trend of thin filmization in recent years. On the other hand, in the latter case, since it is required to laminate thermoplastic resin layers using thermoplastic resins with very different molecular skeleton structures, interlayer peeling is likely to occur at the interface of adjacent different thermoplastic resin layers. Therefore, as in the case of the metal thin film layer, there is a problem that the original laminated structure of the laminated film cannot be maintained due to fatigue during repeated use such as bending, and long-term use in harsh environments, which damages the original performance of broadband / high reflectivity. Therefore, although the reflective light control film composed of (AB)x disclosed in patent documents 2 to 5 is a thin film, it is difficult to apply it to applications requiring broadband / high reflectivity.

[0016] Therefore, an object of the present invention is to provide a laminated film that can reduce interlayer delamination even in long-term continuous use and can maintain optical properties of broadband / high reflectivity for a long period of time.

[0017] Means for solving problems

[0018] In order to solve the above-mentioned problems, the first laminated film of the present invention, the second laminated film of the present invention, and the third laminated film of the present invention include the following configurations.

[0019] The first laminated film of the present invention is a laminated film characterized by having three or more layers of three different thermoplastic resins arranged in a continuous regular pattern and satisfying the following conditions X and Y at the same time.

[0020] Condition X: When three different thermoplastic resin layers are set as A layer, B layer, and C layer, the thickness ratio A / B of the A layer to the B layer in the regular arrangement is greater than or equal to 0.60 and less than or equal to 5.00, and the thickness ratio C / B of the C layer to the B layer in the regular arrangement is greater than or equal to 0.70 and less than or equal to 5.00.

[0021] Condition Y: The maximum reflectance at a wavelength of 400 to 800 nm is 35% or more and 100% or less.

[0022] The second laminated film of the present invention is a laminated film, characterized in that it continuously has a regular arrangement of more than three thermoplastic resin layers having different refractive indices, and when the above three thermoplastic resin layers are set as a layer, b layer, and c layer in order of refractive index from high to low, the thickness ratio a / b of the above a layer relative to the above b layer and the thickness ratio c / b of the above c layer relative to the above b layer in the regular arrangement show a regular arrangement of more than 1.40, and, within the wavelength range of 300 to 2600nm, it has a reflection band that continuously shows a reflectivity of more than 20% within a range of more than 100nm.

[0023] The third laminated film of the present invention is a laminated film, characterized in that it continuously has three or more regularly arranged layers consisting of three different thermoplastic resins, and has a reflection band that continuously shows a reflectivity of more than 75% within a range of more than 100 nm in a wavelength range of 400 to 800 nm, and more than 30% and less than 80% of the total number of layers of the regularly arranged thermoplastic resin layers are thermoplastic resin layers with a layer thickness of more than 1 nm and less than 25 nm.

[0024] Effects of the Invention

[0025] Through the present invention, even when thermoplastic resin layers with different molecular skeleton structures that show interlayer delamination if stacked adjacently are used, interlayer delamination is greatly reduced. As a result, a laminated film can be obtained that can maintain the broadband / high reflectivity optical properties in the visible light region by utilizing the refractive index difference of these thermoplastic resin layers for a longer period of time. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a schematic diagram showing the relationship between the depth in the thickness direction and the contrast difference (grayscale) in a cross-sectional observation image of one embodiment of a laminated film having a regular arrangement of (ABCB)x.

[0027] Figure 2 A scheme showing a regularly arranged stacked film with (ABCB)x (with Figure 1 Schematic diagram of the relationship between the depth in the thickness direction and the contrast difference (grayscale) in the cross-sectional observation image of different schemes).

[0028] Figure 3 This is a schematic diagram showing the relationship between the depth in the thickness direction and the contrast difference (grayscale) in a cross-sectional observation image of a laminated film having an (AB)x alternating laminate arrangement.

[0029] Figure 4 It is a schematic diagram showing the wavelength band Π, the reflection bandwidth λ, and the maximum reflectivity in the reflection spectrum of the stacked film involved in one embodiment of the present invention.

[0030] Figure 5 To illustrate an embodiment of the present invention (with Figure 4 Schematic diagram of band Π, reflection bandwidth λ and maximum reflectivity in the reflection spectral spectrum of the stacked film involved in different schemes (different schemes).

[0031] Figure 6 To illustrate an embodiment of the present invention (with Figure 4 , 5 Schematic diagram of band Π, reflection bandwidth λ and maximum reflectivity in the reflection spectral spectrum of the stacked film involved in different schemes (different schemes).

[0032] Figure 7 To illustrate an embodiment of the present invention (with Figure 4 , 5 , a schematic diagram of band Π, reflection bandwidth λ, and maximum reflectivity in the reflection spectral spectrum of the stacked film involved in scheme 6 (a different scheme).

[0033] Figure 8 Schematic diagram showing a loss tangent tan δ spectrum obtained in the dynamic viscoelasticity measurement of the laminated film of the present invention.

[0034] Fig. 9 This is a schematic diagram showing measurement points when the laminated film of the present invention is attached to a light source unit for evaluation. DETAILED DESCRIPTION

[0035] The following is a detailed description of the laminated film of the present invention. The laminated film of the present invention includes the first laminated film of the present invention, the second laminated film of the present invention, and the third laminated film of the present invention. It should be noted that, hereinafter, unless otherwise specified, the so-called "laminated film of the present invention" refers to all of them. In addition, in order to illustrate the layer structure of the laminated film of the present invention, expressions such as (ABCB)x, (abcb)x, (αβγβ)x, etc. are sometimes used. In such expressions, the symbols in brackets are regularly arranged, and x is a natural number representing a repeating unit. For example, if it is (ABCB)x, it means that the A layer, the B layer, the C layer, and the B layer are arranged in a regular manner in sequence and repeated x times. In addition, the so-called "refractive index" in the present invention refers to the refractive index in the in-plane direction (in-plane refractive index), and its measurement method is described below.

[0036] The first laminated film of the present invention is a laminated film characterized by having three or more layers of three different thermoplastic resins arranged in a continuous regular pattern and satisfying the following conditions X and Y at the same time.

[0037] Condition X: When three different thermoplastic resin layers are set as A layer, B layer, and C layer, the thickness ratio A / B of the A layer to the B layer in the regular arrangement is greater than or equal to 0.60 and less than or equal to 5.00, and the thickness ratio C / B of the C layer to the B layer in the regular arrangement is greater than or equal to 0.70 and less than or equal to 5.00.

[0038] Condition Y: The maximum reflectance at a wavelength of 400 to 800 nm is 35% or more and 100% or less.

[0039] The second laminated film of the present invention is a laminated film, characterized in that it continuously has a regular arrangement of more than three thermoplastic resin layers having different refractive indices, and when the above three thermoplastic resin layers are set as a layer, b layer, and c layer in order of refractive index from high to low, the thickness ratio a / b of the above a layer relative to the above b layer and the thickness ratio c / b of the above c layer relative to the above b layer in the regular arrangement show a regular arrangement of more than 1.40, and, within the wavelength range of 300 to 2600nm, it has a reflection band that continuously shows a reflectivity of more than 20% within a range of more than 100nm.

[0040] The third laminated film of the present invention is a laminated film, characterized in that it continuously has three or more regularly arranged layers consisting of three different thermoplastic resins, and has a reflection band that continuously shows a reflectivity of more than 75% within a range of more than 100 nm in a wavelength range of 400 to 800 nm, and more than 30% and less than 80% of the total number of layers of the regularly arranged thermoplastic resin layers are thermoplastic resin layers with a layer thickness of more than 1 nm and less than 25 nm.

[0041] The first and third laminated films of the present invention need to have three different thermoplastic resin layers. In the laminated films of these inventions, the thermoplastic resin layers are "different", which means at least one of (1) different compositions, (2) different glass transition temperatures and melting points in differential scanning calorimetry (DSC), and (3) different contrasts in stained images when cross-sections are observed by transmission electron microscopy (TEM).

[0042] The term "different composition" means that it does not correspond to the conditions described below that are regarded as "same composition". The term "same composition" means that the repeating units of the chemical structure of the thermoplastic resin constituting each thermoplastic resin layer are 95 mol% or more and 100 mol% or less in common, or when the constituent components of each thermoplastic resin layer are compared, 95 mass % and 100 mass % or less of the components are in common.

[0043] For example, in the former, if it is polyethylene terephthalate, it has a structural unit (ethylene terephthalate unit) in which an ethylene glycol unit and a terephthalic acid unit are bonded by an ester bond as the main structural unit, but in the case where the resin constituting the layer has a common chemical structure such as polyethylene terephthalate but the amount of the copolymer component exceeds 5 mol%, such as a layer formed of homopolyethylene terephthalate and a layer formed of polyethylene terephthalate copolymerized with 10 mol% of isophthalic acid, the two compositions are considered to be different. In addition, in the latter, in the case where the same structural component is used as the main component but the components exceeding 5 mass% are different from each other, such as a layer formed of only homopolyethylene terephthalate and a layer containing 90 mass% of homopolyethylene terephthalate and the remaining 10 mass% of other components, the two compositions are also considered to be different. The repeating unit structure of the specific composition / chemical structure of each thermoplastic resin layer can be determined by the method described in the layer composition of the measurement method described later, and then the thermoplastic resin layer can be cut and removed, or the layer can be scraped off to expose the outermost layer, thereby specifying it using infrared spectroscopy (FT-IR method, nano-IR method), gas chromatography / mass spectrometer (GC-MS), nuclear magnetic resonance device (NMR), etc.

[0044] On the other hand, when it is difficult to identify the composition by the above method after each thermoplastic resin layer is extracted, the thermoplastic resin layers constituting the laminated film can be judged as "different" by showing different melting points and / or glass transition temperatures in differential scanning calorimetry (DSC). It should be noted that in the first and third laminated films of the present invention, showing different melting points and different glass transition temperatures means that the melting point and glass transition temperature differ by 0.1°C or more, preferably 2.0°C or more (in other words, the difference in melting point and glass transition temperature of the thermoplastic resin layer is 0.1°C or more, preferably 2.0°C or more.). As the easiest example to explain, when differential scanning calorimetry of the laminated film is performed, any one of three different glass transition temperatures, crystallization temperatures (exothermic peaks), and melting points (endothermic peaks) is confirmed. On the other hand, sometimes, in the measurement temperature range of 25°C or more and 300°C or less described in the differential scanning calorimetry (DSC) in the measurement method described later, the thermoplastic resin layer does not show a glass transition temperature and a melting point. When one thermoplastic resin layer shows a glass transition temperature or a melting point and the other thermoplastic resin layer does not, it cannot be calculated as a temperature difference and is interpreted as a different thermoplastic resin layer. For example, when three glass transition temperatures are observed and only two melting points are observed, it can be interpreted that one of the three thermoplastic resin layers is formed of an amorphous thermoplastic resin without a melting point. In addition, as another scheme, when three melting points can be confirmed and only two or less glass transition temperatures or crystallization temperatures can be confirmed within the above temperature range, it can be interpreted as a thermoplastic resin layer having a glass transition temperature or a crystallization temperature in a low temperature region outside the temperature range. It should be noted that the measurement using DSC in the present invention can be performed by the method of JIS-K-7122 (1987), which is described in detail below.

[0045] The above two methods require that a corresponding thermoplastic resin layer be separated from the film for analysis, and it is sometimes difficult to identify the composition. Therefore, for the first and third laminated films of the present invention, for simplicity, the layer interface formed by the contrast difference can be identified using the cross-sectional image observed in the transmission electron microscope observation. When it is confirmed by the method described in the item of layer interface (contrast difference) in the measurement method described later that the difference in the average brightness of two adjacent layers is greater than any of the standard deviations of the brightness in each layer of the adjacent thermoplastic resin layer, the contrast of the image after dyeing is different, and it is judged that the composition of the adjacent thermoplastic resin layer is "different".

[0046] This contrast difference is caused by the difference in electron beam scattering, crystal diffraction, etc. between thermoplastic resin layers. Therefore, when the composition of the thermoplastic resin layer is different according to the above-mentioned criteria, the crystallinity and electron density state are different according to the type of thermoplastic resin constituting each thermoplastic resin layer and the copolymerization amount of the thermoplastic resin combined, and the electron staining state is also different. Therefore, in the case of having thermoplastic resin layers with different compositions, each thermoplastic resin layer can be recognized as a layer structure with a contrast difference in the cross-sectional image of the laminated film.

[0047] In the case of a laminated film having three different thermoplastic resin layers as in the first and third laminated films of the present invention, since a certain brightness is displayed in each thermoplastic resin layer, when the depth in the thickness direction is displayed on the horizontal axis and the brightness / contrast (grayscale in grayscale display) of each point is displayed on the vertical axis, the following graph is obtained: Figure 1 , Figure 2 The brightness changes in stages as shown in the figure. Figure 1 , 2 Schematic diagram showing the relationship between the depth in the thickness direction and the contrast difference (grayscale) in a cross-sectional observation image of one embodiment of a laminated film having a regular arrangement of (ABCB)x. Figure 3 This is a schematic diagram showing the relationship between the depth in the thickness direction and the contrast difference (grayscale) in a cross-sectional observation image of a laminate film having an (AB)x alternating stacking arrangement. Figures 1 to 3 In the figure, symbols 1 to 5 represent, respectively, a spectrum showing the relationship between the depth in the thickness direction of a stacked film having a regular ABCB arrangement and the contrast (grayscale) change, the layer thickness of layer A, the layer thickness of layer B, the layer thickness of layer C, and the layer thickness of the interface layer of a stacked film having an AB alternating stacking arrangement.

[0048] In the case of a conventional structure consisting of two thermoplastic resin layers showing a regular arrangement of (AB)x, as shown in FIG. Figure 3 Thus, the image is repeated up and down between the brightness of two points. Here, the area between the brightness of the two points indicated by the symbol 5 is defined as the interface layer. Although the idea of ​​including three thermoplastic resin layers is also found, in the first and third laminated films of the present invention, such a scheme is not treated as a case where there are three different thermoplastic resin layers. That is, in these inventions, the definition of the interface layer formed by the contrast difference is used to determine whether there are three different thermoplastic resin layers. It should be noted that the presence or absence of contrast difference can be evaluated by the method described below.

[0049] The second laminated film of the present invention needs to have three thermoplastic resin layers with different refractive indices. The so-called thermoplastic resin layers with different refractive indices are determined from the dielectric constants of each thermoplastic resin layer obtained by electron energy loss spectrum measurement (EELS measurement) according to the method described in the measurement method described later. More specifically, it can be determined by the following steps. First, the main orientation axis direction of the laminated film cross section is determined by the phase difference measurement device KOBRA-WPR manufactured by Oji Instruments Co., Ltd. (as other devices capable of performing the same measurement, there is KOBRA-21ADH, which can also be used.) and a cross-sectional sample of the laminated film is obtained in a manner including the direction and the thickness direction of the laminated film. Next, each thermoplastic resin layer in the cross-sectional sample is irradiated with electron beams, and its dielectric constant is analyzed to read the dielectric constant at a loss energy of 2.5 eV. When the difference in the dielectric constant of the obtained thermoplastic resin layer is greater than 0.01, it is determined that the refractive index of the thermoplastic resin layer is "different". According to Maxwell's electromagnetic theory, the dielectric constant is generally equal to the square of the refractive index in a non-magnetic material that hardly absorbs light, such as the thermoplastic resin (described later) that can be suitably used in the laminated film of the present invention. Therefore, based on the different dielectric constants of the thermoplastic resin layers, it can be judged that the refractive index of the thermoplastic resin layers is different, and the magnitude relationship of the dielectric constant of the thermoplastic resin layer is consistent with the magnitude relationship of the refractive index. It should be noted that, as described in detail below, in the first and third laminated films of the present invention, the magnitude relationship of the refractive index in the above-mentioned EELS measurement can also be applied.

[0050] Representative thermoplastic resins that can be used to form the thermoplastic resin layer of the laminated film of the present invention are shown below, but the thermoplastic resins that can be used in the present invention are not limited to the substances shown below. For example, polyolefin resins represented by polyethylene, polypropylene, poly(1-butene), poly(4-methylpentene), polyisobutylene, polyisoprene, polybutadiene, polyvinylcyclohexane, polystyrene, poly(α-methylstyrene), poly(p-methylstyrene), polynorbornene, polycyclopentene, etc., polyamide resins represented by nylon 6, nylon 11, nylon 12, nylon 66, etc., copolymer resins of vinyl monomers represented by ethylene / propylene copolymers, ethylene / vinylcyclohexane copolymers, ethylene / vinylcyclohexene copolymers, ethylene / alkyl acrylate copolymers, ethylene / methacrylate copolymers, ethylene / norbornene copolymers, ethylene / vinyl acetate copolymers, propylene / butadiene copolymers, isobutylene / isoprene copolymers, vinyl chloride / vinyl acetate copolymers, etc. can be used. Acrylic resins represented by polyacrylate, polyisobutyl methacrylate, polymethacrylate, polymethyl methacrylate, polybutyl acrylate, polyacrylamide, polyacrylonitrile, etc., polyester resins represented by polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene 2,6-naphthalate, etc., biodegradable polymers represented by polylactic acid, polybutyl succinate, etc., and polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, polyvinyl butyral, polyacetal, polyglycolic acid, polycarbonate, polyketone, polyether sulfone, polyether ether ketone, modified polyphenylene ether, polyphenylene sulfide, polyetherimide, polyimide, polysiloxane, tetrafluoroethylene resin, trifluoroethylene resin, trifluorochloroethylene resin, tetrafluoroethylene-hexafluoropropylene copolymer, polyvinylidene fluoride, etc.

[0051] The following describes in detail a laminated film composed of three different thermoplastic resin layers. Three completely different thermoplastic resins may be combined, or two different thermoplastic resins may be used to form three different thermoplastic resins by alloying, blending, copolymerizing, etc. Furthermore, three different thermoplastic resin layers may be formed by using one thermoplastic resin as a base and using different copolymer components.

[0052] In the case of two or three different thermoplastic resins, as described in the manufacturing method described later, since different thermoplastic resins coexist in the lamination device, it is preferable to use a thermoplastic resin that is required to have the same degree of heat resistance and lamination properties (viscosity, compatibility, etc.), and also has the transparency and strength required for the obtained laminated film. If two different thermoplastic resins are used, for example, as a combination of resins for lamination, polyester resin and polycarbonate resin, polyester resin and polyamide resin, polyester resin and polyolefin resin such as polypropylene, polyester resin and acrylic resin, polyester resin and polyvinylidene fluoride resin, polycarbonate resin and acrylic resin, polycarbonate resin and polyvinylidene fluoride resin, polylactic acid and polyvinylidene fluoride resin, etc. can be cited. When three different thermoplastic resins are used, polyester resin, polycarbonate resin, and acrylic resin, polyester resin, polystyrene resin, and acrylic resin, polycarbonate resin, polystyrene resin, and acrylic resin, polycarbonate resin, acrylic resin, and polyvinylidene fluoride resin may be used.

[0053] Furthermore, in order to obtain the high reflectivity, transparency and interlayer adhesion characteristics of the laminated film of the present invention, as preferred combinations of thermoplastic resins, it is preferred to use: a combination of three different thermoplastic resins with one thermoplastic resin as the copolymer component; a combination of a copolymer of a polyester resin and a polyester resin and an acrylic resin, a copolymer of a polyester resin and a polyester resin and a polyamide resin, and a copolymer of a polyester resin and a polyester resin and a polyolefin resin when two thermoplastic resins are used as the basis; and a combination of a polyester resin, a polycarbonate resin and an acrylic resin, a polyester resin, a polystyrene resin and an acrylic resin, and a polycarbonate resin, a polystyrene resin and an acrylic resin when three thermoplastic resins are used as the basis.

[0054] In each thermoplastic resin layer, these thermoplastic resins may be used alone or two or more thermoplastic resins may be blended or alloyed. By blending or alloying, in addition to obtaining physical / chemical properties that cannot be obtained by one thermoplastic resin, when laminating thermoplastic resin layers with greatly different skeleton structures, if a component common to the polymer skeleton structure contained in the thermoplastic resin layer on the opposite side can be applied to the thermoplastic resin layer on one side of the adjacent thermoplastic resin layer as a copolymer component, the interlayer adhesion at the interface can be improved.

[0055] In each thermoplastic resin layer constituting the laminated film of the present invention, from the viewpoint of rheological properties related to strength / heat resistance / transparency / laminability, the thermoplastic resin forming the thermoplastic resin layer is preferably selected from polyolefin resins, polyester resins, acrylic resins, polycarbonate resins, and polyamide resins. From the viewpoint above, polyester resins are more preferably used, and polyester resins obtained by polymerization of monomers having aromatic dicarboxylic acids or aliphatic dicarboxylic acids and diols as main components are further preferred.

[0056] Here, as aromatic dicarboxylic acids, for example, terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 4,4'-diphenyl dicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid, 4,4'-diphenyl sulfone dicarboxylic acid, etc. can be cited. As aliphatic dicarboxylic acids, for example, adipic acid, suberic acid, sebacic acid, dimer acid, dodecanedioic acid, cyclohexane dicarboxylic acid and their ester derivatives can be cited. Among them, terephthalic acid and 2,6-naphthalene dicarboxylic acid can be preferably cited. It should be noted that these acid components can be used alone or in combination of two or more, and further, hydroxy acids such as hydroxybenzoic acid can be partially copolymerized.

[0057] In addition, as diols, for example, ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, neopentyl glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, diethylene glycol, triethylene glycol, polyalkylene glycol, 2,2-bis(4-hydroxyethoxyphenyl)propane, isosorbide, spiroglycol, etc. can be mentioned. Among them, ethylene glycol is preferably used. These diol components can be used alone or in combination of two or more.

[0058] In each thermoplastic resin layer constituting the laminated film of the present invention, among the above-mentioned polyester resins, it is particularly preferable to use a polyester resin selected from polyethylene terephthalate and its copolymers, polyethylene naphthalate and its copolymers, polybutylene terephthalate and its copolymers, polybutylene naphthalate and its copolymers, further polyhexamethylene terephthalate and its copolymers, and polyhexamethylene naphthalate and its copolymers.

[0059] The laminated film of the present invention needs to continuously have three or more regular arrangements of three different thermoplastic resin layers (in the case of the first and third laminated films of the present invention), or a regular arrangement of three thermoplastic resin layers with different refractive indices (in the case of the second laminated film of the present invention). Specifically, "a regular arrangement of three thermoplastic resin layers" refers to a laminated structure in which the "three different" thermoplastic resin layers in the first and third laminated films of the present invention are laminated according to a certain regular arrangement, as defined above. In addition, the so-called "a regular arrangement of three thermoplastic resin layers with different refractive indices" refers to a laminated structure in which the "three different" thermoplastic resin layers in the second laminated film of the present invention are laminated according to a certain regular arrangement, as defined above. In this case, the "three different thermoplastic resin layers" or "three thermoplastic resin layers having different refractive indices" can be formed by thermoplastic resins having mutually different skeleton structures to form each thermoplastic resin layer. Alternatively, thermoplastic resins having two skeleton structures can be used and designed in such a way that their mixing ratios or copolymerization amounts are different in the three thermoplastic resin layers.

[0060] In the first laminated film of the present invention, different thermoplastic resin layers are defined in alphabetical order as layer A, layer B, and layer C in the order in which they first appear when observed from the outermost surface of the laminated film, and the thermoplastic resin serving as the main component of each thermoplastic resin layer is defined as thermoplastic resin A, thermoplastic resin B, and thermoplastic resin C.

[0061] In the second laminated film of the present invention, three thermoplastic resin layers with different refractive indices are defined as layer a, layer b, and layer c in descending order of refractive index (dielectric constant) according to the magnitude relationship of the dielectric constant at the loss energy of 2.5 eV obtained by the above-mentioned EELS measurement, and the thermoplastic resin serving as the main component of each thermoplastic resin layer is defined as thermoplastic resin a, thermoplastic resin b, and thermoplastic resin c.

[0062] In the third laminated film of the present invention, the presence of three kinds of thermoplastic resins is determined by the definition of the "different" thermoplastic resin layer in the first laminated film of the present invention. In addition, according to the magnitude relationship of the dielectric constant measured by the above-mentioned EELS, the dielectric constant (refractive index) can be defined as an α layer, a β layer, and a γ layer in descending order, and the thermoplastic resins as the main components of each thermoplastic resin layer are defined as thermoplastic resin α, thermoplastic resin β, and thermoplastic resin γ. The third laminated film of the present invention is different from the first laminated film of the present invention in that the α layer, β layer, and γ layer are not necessarily defined in sequence from the outermost layer. That is, the outermost layer of the third laminated film of the present invention can be any one of the α layer, β layer, and γ layer, and it is sufficient as long as there are three or more regular arrangements of α layers, β layers, and γ layers continuously in the laminated film.

[0063] The so-called main component described here refers to a component containing more than 50% by mass and less than 100% by mass in the layer. As a secondary component that is not a main component, for example, an inorganic component, a low molecular weight organic component other than a thermoplastic resin, etc., as a specific example, a light absorber (ultraviolet absorber, dye, pigment, heat ray absorber), an antioxidant, a light stabilizer, a matting agent, a heat stabilizer, a weathering stabilizer, an organic lubricant, a filler, an antistatic agent, a nucleating agent, a flame retardant, etc. can be cited. These secondary components can be freely added to each layer to the extent that the original physical properties / functions of the film are not damaged.

[0064] Among these secondary components, depending on the type of thermoplastic resin constituting each thermoplastic resin layer, it sometimes absorbs high-energy ultraviolet rays and promotes degradation, so it is preferable to include an ultraviolet absorber for the purpose of suppressing light degradation by reaction competition. Furthermore, the light absorber itself is sometimes affected by degradation caused by heat and oxygen in the resin extrusion process, and by light degradation caused by reaction with ultraviolet rays and oxygen. Therefore, for the former, an antioxidant can be used, and for the latter, a light stabilizer and a matting agent can be used as additives, and added to the layer containing the thermoplastic resin that may be degraded to a degree that does not damage the original physical properties and functions of the film.

[0065] In the first laminated film of the present invention, when different thermoplastic resin layers are defined as A layer, B layer, and C layer in the order of being arranged from the outermost surface of the laminated film, the so-called regular arrangement of the laminated film of the present invention can be exemplified by (ABC)x, (ABCB)x, (ABAC)x, (ABCAB)x, (ABCAC)x, (ABABC)x, (ABCBCB)x, etc. This can also be explained in the same way in the a layer, b layer, and c layer in the second laminated film of the present invention, and the α layer, β layer, and γ layer in the third laminated film of the present invention by replacing them from the above-mentioned A layer, B layer, and C layer, respectively. It should be noted that in the second and third laminated films of the present invention, the a layer and the α layer may be arranged regularly without necessarily being located at the outermost surface.

[0066] In order to enable a laminated film using thermoplastic resins having different physical / chemical properties such as skeleton structure and viscoelasticity / viscosity characteristics to maintain its laminated structure for a long time without interfacial delamination and without damaging the necessary functions, it is necessary to study a combination of thermoplastic resin layers with good compatibility (compatibility, surface free energy, etc.) for adjacent thermoplastic resin layers forming the interface of different thermoplastic resin layers contained in the laminated film.

[0067] Therefore, in order to avoid complicating the resin design of the entire laminate film, it is preferred that the number of combinations of interfaces formed by adjacent thermoplastic resin layers is small. Specifically, if the first laminate film of the present invention is taken as an example, the interfaces formed by three different thermoplastic resin layers can be AB interface, BC interface, and CA interface. In the above regular arrangement, (ABCB)x and (ABCBCB)x are preferred in that only two types of interfaces, AB interface and BC interface, exist. In such a scheme, the resin design can be performed in a manner that interlayer peeling between layer A and layer B, and between layer B and layer C is not likely to occur, and the combination of layer A and layer C can be ignored. It should be noted that this also applies to the second and third laminate films of the present invention.

[0068] That is, in such a scheme, if the resin design is such that interlayer peeling between layer A and layer B, or between layer B and layer C is not likely to occur, layer B plays the role of a buffer layer between layer A and layer C. As a result, interlayer peeling is not likely to occur in the laminated film as a whole, and the original optical characteristics and physical properties of the laminated film can be maintained even when used for a long time. It should be noted that the laminated film of the present invention can also be provided with a hard coating layer, an easy-adhesion layer, a gas barrier layer, an adhesive layer, etc. as functional layers on the outermost surface, and an interface is formed with the outermost thermoplastic resin layer constituting the laminated film, but the so-called interface here refers only to the regularly arranged interface constituting the laminated film.

[0069] Furthermore, in order to improve the reflective properties of the laminated film of the present invention, the number of the above-mentioned regular arrangements contained in the laminated film is important. The more the number of regular arrangements, the higher the optical properties such as high reflectivity and broadband can be. Therefore, since the laminated film having the regular arrangement of (ABCB)x, that is, the laminated film having the arrangement of A layer, B layer, C layer, and B layer in sequence has a small number of layers and the thickness of the laminated film is thin, and the target optical properties can be obtained at the same time, it is the most preferred (if it is the second laminated film of the present invention, then the regular arrangement of the same layers every other layer such as (abcb)x is equivalent to it, and if it is the third laminated film of the present invention, then the regular arrangement of the same layers every other layer such as (αβγβ)x is equivalent to it.). Such an arrangement can be achieved by designing the resin distribution flow path of the laminated device used when manufacturing the laminated film.

[0070] Such a regular arrangement can control interference reflection by the optical geometric arrangement formed by the refractive index and layer thickness of the thermoplastic resin layer, so in addition to being able to improve the reflectivity of the laminated film and expand the reflection band, for example, when a non-crystalline thermoplastic resin is used as a thermoplastic resin with different viscosity and viscoelastic properties in a part of the thermoplastic resin layer, it can be easily co-stretched to follow the stretchability of the crystalline thermoplastic resin repeatedly present in the laminated film, thereby improving the uniformity of the laminated layers in the surface of the manufactured film. As a result, the state of the layer interface also becomes good in the film surface, and it is not easy to peel off at the interface, so it becomes easy to obtain a laminated film suitable for long-term use as the target of the present invention.

[0071] In order to realize the above-mentioned interference reflection, the laminated film of the present invention needs to have a number of regular arrangements continuously included of 3 or more, preferably 20 or more, more preferably 50 or more, and further preferably 100 or more. The more such regular arrangements, the more preferred it is from the viewpoint of uniform stretching and optical performance of the laminated film. However, if the increase in manufacturing cost accompanying the large-scale manufacturing device, the disorder of lamination accompanying the complication of the lamination process, the deterioration of operability caused by the thickening of the film, etc. are taken into consideration, it is realistic to have a number of regular arrangements of 500 or less. Regular arrangements can construct a prescribed number of regular arrangements in a lamination device at one go, and after constructing a certain number of regularly arranged laminated bodies in the lamination device, the number of laminates can be effectively multiplied by a known square mixer to increase the number of regular arrangements.

[0072] In the second laminated film of the present invention, when the a layer, b layer, and c layer are preferably arranged in descending order of refractive index, the b layer exists every other layer in the thickness direction of the laminated film. By configuring the b layer as the second highest refractive index layer among the three thermoplastic resin layers in this way, the b layer optically plays a buffering role between the a layer and the c layer. Usually, the refractive index of the thermoplastic resin layer is greatly influenced by the properties of the polymer such as the molecular structure of the thermoplastic resin constituting the thermoplastic resin layer, the orientation state of the main chain skeleton, the polarizability, and the softness of the main chain. That is, the properties of the thermoplastic resin constituting the b layer with the second highest refractive index are intermediate properties between the thermoplastic resin constituting the a layer and the thermoplastic resin constituting the c layer. It should be noted that such a layer structure can be achieved by adjusting the structure of a laminating device such as a feed block.

[0073] In addition, in order to show the preferred optical properties for a long time, it is important for the three thermoplastic resin layers to show good close contact at each interface in the same manner as described above. Therefore, the b layer that shows the effect of the intermediate buffer layer is often adjacent to the a layer or c layer of the thermoplastic resin layer that is different from the b layer, and it is preferred regardless of the regular arrangement. Therefore, the b layer preferably exists every other layer in the thickness direction of the laminated film. As a preferred regular arrangement that can show such a state, (abcb)x, (abcbcb)x, etc., (cbab)x, (cbabab)x, etc., in which the a layer and the c layer are interchanged, can be cited. Such a regular arrangement can be achieved by using a multi-manifold, slit-type feed block used when making a film laminated film, and implementing a polymer flow path design inside it so that the three thermoplastic resins are arranged in the above-mentioned regular arrangement.

[0074] The laminated film of the present invention preferably has the above-mentioned regular arrangement, and at the same time, the two surface layers as the outermost layers are configured with the same thermoplastic resin layer. If the preferred regular arrangement in the first laminated film of the present invention is taken as an example, it is a scheme represented by laminated patterns such as (ABCB)xA, (ABCBCB)xA. Since the two surface layers are composed of thermoplastic resin layers with the same thermoplastic resin as the main component, in the manufacturing method described later, it is not necessary to finely adjust the roller temperature, material, etc. according to the thermal properties of the thermoplastic resin layer in contact with the roller in order to prevent the adhesion between the roller and the film during roller stretching, and various conditions can be set according to the thermal properties of the thermoplastic resin constituting the thermoplastic resin layer configured in the two outermost layers. That is, the scheme in which the two surface layers as the outermost layers are configured with the same thermoplastic resin layer is preferred because the laminated film can be obtained under the same film making conditions as in the case of a single film film with the thermoplastic resin of the outermost layer as the main component.

[0075] In the first laminated film of the present invention, the dielectric constant at a loss energy of 2.5 eV obtained by EELS measurement is preferably in the order of A layer, B layer, and C layer from large to small. By becoming such a scheme, when a laminated pattern such as (ABCB)xA, (ABCBCB)xA is formed, the B layer plays a role in improving the interlayer adhesion of the laminated film. In addition, when the dielectric constant is in the order of A layer, B layer, and C layer from large to small, for example, in the case of having a regular arrangement as described above, in the preferred layer thickness ratio conditions (described later) for achieving the high reflectivity of the first laminated film of the present invention, the middle B layer exists in a thin state compared with the A layer and the C layer. Therefore, the B layer, which should usually have an effect on the reflection characteristics due to the refractive index difference at the interface with the A layer and the C layer, has a thickness that can be ignored optically, and the influence of reflection at the interface between the A layer and the B layer, and the B layer and the C layer becomes extremely small. Thus, the optical reflection characteristics brought by only the A layer and the C layer having the largest refractive index difference appear as the optical characteristics of the laminated film, and the laminated film can exhibit high reflectivity characteristics that are not usually obtained. It should be noted that, in the third laminated film of the present invention, from the same viewpoint, when the three thermoplastic resin layers are set as the α layer, the β layer, and the γ layer, the dielectric constant at the loss energy of 2.5 eV obtained by EELS measurement is preferably from the largest to the smallest in the order of the α layer, the β layer, and the γ layer.

[0076] The above contents related to the first laminated film of the present invention are valid even if the magnitude relationship of the dielectric constants of the A layer and the C layer is changed, but in the first laminated film of the present invention in which the outermost layer is the A layer, it is appropriate to arrange the refractive index from high to low in the order of the A layer, the B layer, and the C layer in consideration of the stability of the manufacturing method. The reason is that, generally, a crystalline thermoplastic resin layer has a high dielectric constant, so the film formation becomes easy by making the A layer the layer with the highest dielectric constant.

[0077] In the laminated film of the present invention, the dielectric constant ratio of the thermoplastic resin layer with the highest refractive index at a loss energy of 2.5 eV to the thermoplastic resin layer with the lowest refractive index, which is preferably obtained by EELS measurement, is 1.10 or more and 1.60 or less. In order to improve the reflectivity of the laminated film of the present invention, it is important to make the refractive index difference between the layer with the highest refractive index and the layer with the lowest refractive index among the regularly arranged thermoplastic resin layers large, but the refractive index of the thermoplastic resin layer is affected to some extent by the composition of the thermoplastic resin constituting the layer, the basic skeleton, etc. That is, in order to make the refractive index difference between the layer with the highest refractive index and the layer with the lowest refractive index large, it is required to make the composition of the thermoplastic resin constituting these layers very different and the basic skeleton different. More specifically, for example, in order to make the refractive index of the thermoplastic resin layer high, it can be achieved by applying a thermoplastic resin having a structural unit containing an aromatic ring and showing crystallinity as the thermoplastic resin constituting the layer. On the other hand, in order to make the refractive index of the thermoplastic resin layer low, for example, it can be achieved by using a resin composition with a non-crystalline and aliphatic structural unit as the main structural unit, or with a structural unit containing an aromatic ring as the main structural unit and a structural unit derived from aliphatic with a copolymerization amount of 20 mol% or more and less than 50 mol%. Here, the so-called main structural unit refers to the structural unit that is most contained among the structural units of the thermoplastic resin. On the other hand, if the composition, basic skeleton, etc. of the thermoplastic resin constituting the thermoplastic resin layer are greatly different, the interlayer adhesion is poor. Therefore, for the laminated film with an alternating laminated structure formed by two thermoplastic resins as the main body in the past, it is difficult to achieve the improvement of interlayer adhesion and high reflectivity at the same time. On the other hand, for the laminated film of the present invention, by using three different thermoplastic resins including a resin thermoplastic resin layer with intermediate characteristics, even if the dielectric constant ratio of the thermoplastic resin layer with the highest refractive index to the thermoplastic resin layer with the lowest refractive index is 1.10 or more, which is usually difficult to laminate, the lamination of the thermoplastic resin layer becomes easy, so these characteristics can be combined. In addition, the upper limit of the dielectric constant ratio is preferably 1.60. Even if a buffer layer with intermediate properties is provided, if the dielectric constant ratio of the thermoplastic resin layer with the highest dielectric constant to the thermoplastic resin layer with the lowest dielectric constant exceeds a certain level, the dielectric constant ratio of these layers to the buffer layer with intermediate properties also increases proportionally, so there is a possibility that the interlayer adhesion is impaired. By suppressing the dielectric constant to be below 1.60, sufficient interlayer adhesion can be ensured.

[0078] From the viewpoint of achieving both improved interlayer adhesion and high reflectivity, the dielectric constant ratio is preferably 1.10 to 1.60, more preferably 1.20 to 1.50, and even more preferably 1.30 to 1.50. As a means for satisfying such a preferred dielectric constant ratio between the thermoplastic resin layer with the highest refractive index and the thermoplastic resin layer with the lowest refractive index, for example, a method can be cited in which at least one preferred thermoplastic resin described later is included, and the thermoplastic resin as the main component of the thermoplastic resin layer with the highest dielectric constant is different from the thermoplastic resin as the main component of the thermoplastic resin layer with the lowest dielectric constant.

[0079] In the laminated film of the present invention, at least one of the three different thermoplastic resin layers is preferably a thermoplastic resin layer showing crystallinity (in the second laminated film of the present invention, "three different thermoplastic resin layers" refers to "three thermoplastic resin layers with different refractive indices".). In the case where all the thermoplastic resins forming the thermoplastic resin layers constituting the laminated film are amorphous resins, when stretched in the manufacturing method described later, stress is sometimes not generated and uneven stretching of the laminated film occurs, and the uniformity of the physical properties of the laminated film is greatly impaired. Therefore, at least one is preferably a crystalline thermoplastic resin layer that can physically hold the other thermoplastic resin layers laminated at the same time and perform co-stretching. The judgment of crystallinity can be judged by cutting and extracting the thermoplastic resin layer, using a differential scanning calorimetry (DSC) device, and confirming the presence or absence of a melting point (endothermic peak). In particular, in the laminated film of the present invention, a thermoplastic resin layer whose integrated melting enthalpy with the base line in the endothermic peak corresponding to the melting point shows 10 J / g or more is defined as a crystalline thermoplastic resin layer.

[0080] In addition, a thermoplastic resin layer showing crystallinity is preferably used for the thermoplastic resin layer located on the outermost layer (the A layer in the case of the first laminated film of the present invention). When the thermoplastic resin layer located on the outermost layer is formed of an amorphous thermoplastic resin, the laminated film may easily adhere to a roller, a jig, etc., resulting in poor stretching and deterioration of the surface state caused by adhesion to the manufacturing equipment.

[0081] Furthermore, it is preferred that the three different thermoplastic resin layers forming the laminated film of the present invention are a combination of thermoplastic resin layers showing crystallinity / semi-crystalline / amorphous, or crystallinity / amorphous / amorphous (in the second laminated film of the present invention, "three different thermoplastic resin layers" refer to "three thermoplastic resin layers with different refractive indices."). The crystallinity, semi-crystalline, and amorphous properties described here can all be determined using a differential scanning calorimetry (DSC) device. The thermoplastic resins constituting the crystalline and semi-crystalline thermoplastic resin layers are characterized by showing three points: a glass transition temperature, a crystallization enthalpy as an endothermic peak, and a melting enthalpy as an exothermic peak. Depending on the type of crystalline thermoplastic resin, the glass transition temperature may not fall within the measurement range described below, so the degree of crystallinity is determined here by the size of the melting enthalpy. As described above, in the laminated film of the present invention, crystallinity is defined as a melting enthalpy of 10 J / g or more, and semi-crystallinity is defined as a melting enthalpy of 0.1 J / g or more and less than 10 J / g. Amorphous is defined as a case where neither of the above is satisfied.

[0082] By combining the crystallinity / semi-crystalline / amorphous or crystallinity / amorphous / amorphous described herein, even in the case of laminating thermoplastic resin layers with a large refractive index difference and a completely different skeleton structure, for example, in order to improve the reflective characteristics, the semi-crystalline or amorphous thermoplastic resin layers arranged therebetween also cause the entanglement of molecular chains and the reaction of functional groups at the interface, thereby forming a laminated film that is not prone to interlayer delamination. The semi-crystalline or amorphous thermoplastic resin layers arranged therebetween can be formed by, for example, laminating a thermoplastic resin that exhibits semi-crystalline or amorphous properties by melt extruding it from an extruder. In addition, as another method, a method can be used in which a thermoplastic resin layer that exhibits semi-crystalline or amorphous properties as the target is formed by extruding a thermoplastic resin with higher crystallinity and melting the crystalline phase by heat treatment in a transverse stretching process.

[0083] In the latter case in particular, as a crystalline thermoplastic resin layer, it is necessary to use a thermoplastic resin layer having a higher melting point than a thermoplastic resin layer showing semi-crystalline or amorphous properties. As the thermoplastic resin used for such a crystalline thermoplastic resin layer, in addition to extrudability, stretchability, and versatility, it is particularly preferred to select from polyethylene terephthalate and its copolymers, polyethylene naphthalate and its copolymers having a small number of methylene chains as polyol components among the above-mentioned preferred polyester resins, from the viewpoint of the magnitude of the refractive index of the thermoplastic resin layer when crystallization is important when the laminated film has a high reflectivity, and from the viewpoint of the melt viscosity behavior related to the lamination accuracy. From the above viewpoint, even if any of the above methods is adopted as a method of achieving a combination of crystalline / semi-crystalline / amorphous properties or crystalline / amorphous / amorphous properties, it is particularly preferred that the thermoplastic resin as the main component of the thermoplastic resin layer showing crystalline properties is polyethylene terephthalate or polyethylene naphthalate.

[0084] The laminated film of the present invention preferably has an amorphous thermoplastic resin layer having either an acrylic resin or a polyester having an alicyclic structure as a main component. As the amorphous thermoplastic resin that can be preferably used in the laminated films of these inventions, it is preferred that the thermoplastic resin has a large refractive index difference with the above-mentioned polyester resin in order to improve the reflectivity, and further, in order to form a laminated film showing good lamination properties, it is preferred to select from acrylic resins and polyester resins showing an alicyclic structure among the above-mentioned thermoplastic resins. The acrylic resin itself is an amorphous resin and has a refractive index of 1.49, and the polyester resin showing an alicyclic structure becomes an amorphous resin showing a refractive index of 1.52 to 1.55 by becoming a copolymer. By laminating thermoplastic resin layers with an amorphous thermoplastic resin having such a refractive index as the main component, the refractive index difference can be expanded to a maximum of about 0.25 to 0.30 within a regular arrangement, and a laminated film showing high reflectivity can be achieved, which is difficult to achieve due to interface peeling when using previous alternating lamination technology.

[0085] Examples of polyester resins having an amorphous alicyclic structure that can be preferably used as the main component of the amorphous thermoplastic resin layer of the laminated film of the present invention include polyester resins obtained by copolymerizing cyclohexanedicarboxylic acid, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, isosorbide, spiroglycol and the like as the alicyclic structure.

[0086] In addition, as the main component of the thermoplastic resin layer showing amorphous properties, amorphous polyamide resins can also be used, which are not preferred resins from the viewpoints of stretchability and film-forming properties because of their high glass transition temperature. As amorphous polyamide resins, for example, polyamide PA12 / MACMI (PA12 / 3,3-dimethyl-4,4-diaminocyclohexylmethane, isophthalic acid), PA12 / MACMT (PA12 / 3,3-dimethyl-4,4-diaminocyclohexylmethane, terephthalic acid), PA MACM 12 (3,3-dimethyl-4,4-diaminocyclohexylmethane, decanedicarboxylic acid or laurolactam), PAMC 12 (PA12, 1,3-bis(aminomethyl)cyclohexane), PA6I / 6T, PA6I / 6T / MACMI, etc. can be used.

[0087] When the first laminated film of the present invention sets three different thermoplastic resin layers as A layer, B layer and C layer, it is important that the thickness ratio A / B of the A layer relative to the B layer in the regular arrangement is greater than 0.60 and less than 5.00, and the thickness ratio C / B of the C layer relative to the B layer in the regular arrangement is greater than 0.70 and less than 5.00. Here, the A layer, the B layer and the C layer are defined in the order in which they are arranged from the outermost surface of the laminated film as described previously. In order to improve the reflectivity of the laminated film, it is roughly determined by the difference in refractive index between the thermoplastic resin layer with the highest refractive index and the thermoplastic resin layer with the lowest refractive index among the thermoplastic resins contained in the regular arrangement. Hereinafter, as described as the above-mentioned preferred conditions, the dielectric constant decreases from large to small in the order of the A layer, the B layer and the C layer, and the A layer and the C layer are described as layers corresponding to the thermoplastic resin layers with the highest and lowest refractive indexes, respectively. However, in reality, light is reflected at the interface of each thermoplastic resin layer. It is ideal that these thermoplastic resin layers with high refractive index difference are adjacent to each other, that is, layer A is adjacent to layer C, but in the case of having both interface adhesion, such a laminate design becomes very difficult. Therefore, the presence of a thermoplastic resin layer (layer B) having the function of a buffer layer that can improve interface adhesion and show high reflective properties for a long time as in the present invention becomes important. Although the reflectivity of the laminated film is roughly determined by the maximum refractive index difference of the thermoplastic resin layers in the regular arrangement, the refractive index difference of the adjacent thermoplastic resin layers becomes smaller by passing through the thermoplastic resin layer equivalent to the buffer layer, so the reflectivity of the laminated film also becomes a slightly smaller value.

[0088] Therefore, for the first laminated film of the present invention, the thickness of the thermoplastic resin layer (B layer) disposed in the middle and corresponding to the buffer layer is designed to be thinner than the phase (wavelength value) of the light to be reflected, so that the influence of the refractive index difference at the interface with the thermoplastic resin layer corresponding to the buffer layer on the reflection characteristics can be reduced. By adopting such a scheme, the influence of the reflection characteristics brought by the B layer is suppressed, so that the reflectivity can be improved as in the case of the interface between the thermoplastic resin layers with the highest refractive index difference (the interface between the A layer and the C layer). In order to achieve this, the design of the thickness ratio A / B of the A layer / B layer and the thickness ratio C / B of the C layer / B layer becomes important, taking the thermoplastic resin layer (B layer) corresponding to the buffer layer as a reference.

[0089] When the thickness ratio A / B is less than 0.60 and the thickness ratio C / B is less than 0.70, the thermoplastic resin layer (B layer) corresponding to the intermediate buffer layer is sufficiently thick relative to the target reflection wavelength, so the A layer / B layer interface and the B layer / C layer interface with a low refractive index difference act as interfaces that reflect light, and the laminated film cannot show a sufficient reflectivity that can be expected from the refractive index of the laminated thermoplastic resin layer. In particular, when compared with the case where each thickness ratio shows 1.0, the reflectivity may be reduced by about 10%.

[0090] On the other hand, when the thickness ratio A / B or the thickness ratio C / B exceeds 5.00, the thickness of the B layer that plays the role of the intermediate buffer layer becomes thinner, so the reflectivity is expected to rise. On the other hand, it is easy to be affected by the disorder of the resin flow and it becomes very difficult to maintain the laminated structure. In particular, when a non-Newtonian resin showing shear dependence of melt viscosity is used as a thermoplastic resin forming the intermediate buffer layer, the disorder becomes more significant. The higher the thickness ratio is, the thinner the thickness of the intermediate buffer layer B layer is, and the higher the reflectivity can be achieved. Therefore, the thickness ratio A / B is preferably 0.90 or more, more preferably 1.30 or more, particularly preferably more than 1.3, and most preferably more than 1.50. The thickness ratio C / B is preferably 1.00 or more, more preferably more than 1.30, and particularly preferably more than 1.50.

[0091] Furthermore, the first laminated film of the present invention preferably has a thickness ratio A / C of layer A to layer C in a regular arrangement of not only the above-mentioned thickness ratio relationship but also a thickness ratio A / C of layer A to layer C of 0.70 or more and not more than 1.40. Controlling layer A, which is equivalent to a crystalline thermoplastic resin layer with the highest refractive index, and layer C, which is an amorphous thermoplastic resin layer with the lowest refractive index, within the range of this thickness ratio means that the thicknesses of the two thermoplastic resin layers are roughly uniform, thereby making it possible to design the laminated structure in such a way that the phases of the lights reflected at the interface of the thermoplastic resin layers are consistent with each other and the lights reflected at different interfaces strongly interfere with each other, and thus a laminated film showing a high reflectivity can be obtained. From the above-mentioned viewpoint, the thickness ratio A / C of layer A to layer C is more preferably 0.80 or more and 1.25 or less, further preferably 0.80 or more and 1.20 or less, and particularly preferably 0.80 or more and 1.00 or less.

[0092] The above-mentioned thickness ratios A / B, C / B, and A / C can be realized by adjusting the discharge ratio from each extruder in consideration of the specific gravity of each thermoplastic resin in addition to the slit design (slit thickness, gap) in the lamination device. In addition, these thickness ratios can be obtained by analyzing the observation images of a transmission electron microscope, which is described in detail below (the same is true for other items related to the layer structure (number of layers, regular arrangement, layer thickness of each layer, distribution of layer thickness).).

[0093] In order to present the appearance of a metallic film, the first laminated film of the present invention needs to have a maximum reflectivity of 35% or more and 100% or less at a wavelength of 400nm to 800nm, in addition to making the above-mentioned thickness ratios A / B and C / B within the above-mentioned range. The so-called maximum reflectivity described here is measured at a 1nm interval using a spectrophotometer in an absolute reflection measurement mode using mirror reflection, as described below in the embodiment, and is calculated by reading the obtained reflection spectroscopic spectrum. The maximum reflectivity at a wavelength of 400nm to 800nm ​​corresponding to the visible light region is less than 35%, which means that the light transmittance is high to the extent that the background can be recognized when the laminated film is recognized. Alternatively, when the transmittance in the visible light region is low and the maximum reflectivity is also low, the visible light is absorbed and a black appearance is displayed. It should be noted that the maximum reflectivity can be measured by a known spectrophotometer, which is described in detail below (hereinafter, the second and third laminated films of the present invention are also included, and other parameters representing the reflection characteristics are also the same.).

[0094] In order to show a metallic appearance to the extent that the background is not easily discernible, the maximum reflectivity of the laminated film at a wavelength of 400nm to 800nm ​​is required to be 35% or more. From the above viewpoint, the maximum reflectivity is preferably 50% or more, more preferably 80% or more, further preferably 85% or more, and most preferably 90% or more. It should be noted that in the case of absolute reflection measurement, since the state in which the light of the light source is guided to the detector without being diffused by specular reflection is set to 100% for measurement, it is impossible in principle for the reflectivity of the measured sample to exceed 100%, and the upper limit of the reflectivity of the laminated film of the present invention becomes 100%. In order to make the maximum reflectivity of the laminated film at a wavelength of 400 to 800nm ​​35% or more or the above preferred range, the number of layers that reflect the target wavelength band by increasing the number of regular arrangements, the inclination of the layer thickness distribution is relaxed, and the combination of thermoplastic resins that are the main components of the A layer and the C layer is selected in a manner that the refractive index difference becomes higher (these can also be used in combination as appropriate). Furthermore, it is also effective to adjust the thickness ratios A / B, C / B, and A / C to appropriate ranges in combination with the previously described method.

[0095] It should be noted that, from the perspective of making the maximum reflectivity at a wavelength of 400nm to 800nm ​​35% or more or the above-mentioned preferred range, the thermoplastic resin of each layer is preferably selected so that the refractive index difference between layer A and layer C is 0.09 or more, more preferably 0.16 or more, further preferably 0.18 or more, and particularly preferably 0.20 or more. The larger the refractive index difference, the better, and there is no particular upper limit, but it is considered to be 0.30 from the perspective of feasibility. It should be noted that, regarding the preferred refractive index difference, if layer A and layer C are replaced by layer a and layer c in the second laminated film of the present invention, the same is true, and if layer A and layer C are replaced by the layer with the highest and lowest refractive index among the α layer, β layer, and γ layer in the third laminated film of the present invention, the same is true.

[0096] The reflection band in the reflection spectrum when the maximum reflectivity at a wavelength of 400 to 800 nm shows the above range can be the main reflection band of the laminated film (the widest reflection band observed on the longest wavelength side, equivalent to the reflection band Π described later), or it can be a high-order reflection band observed in the 1 / n band (hereinafter, n is referred to as the order, a natural number) when there is a main reflection band at a longer wavelength position. The latter can freely control the occurrence of high-order reflection by changing the thickness ratio (discharge ratio of the extruder) of the laminated film of the present invention. However, since the bandwidth of high-order reflection is reduced to 1 / n relative to the order relative to the main reflection band, in the case of the latter, in order to achieve reflection throughout the entire visible light region in order to display the target metallic tone, it is necessary to increase the number of layers and expand the main reflection band. Therefore, in the case of the latter, since it also has disadvantages such as the large-scale lamination device and the thick film of the laminated film accompanied by the increase in the number of layers, the former design is preferred.

[0097] The second laminated film of the present invention needs to have a regular arrangement in which the thickness ratio a / b of the a layer relative to the b layer and the thickness ratio c / b of the c layer relative to the b layer both show a regular arrangement of 1.40 or more for more than 90% when the three thermoplastic resin layers are arranged in descending order of refractive index as the a layer, the b layer, and the c layer. In the case of such a scheme, the b layer of the thermoplastic resin layer showing intermediate properties between the a layer and the c layer as the refractive index is the intermediate value between the a layer and the c layer is relatively thinner. By such a thickness ratio condition, firstly, like the B layer in the first laminated film of the present invention, the b layer can play the role of a buffer layer and an adhesive layer between the a layer and the c layer. Therefore, although the previous alternating lamination technology of two thermoplastic resin layers is difficult to alternately laminate the a layer and the c layer without damaging the interlayer adhesion, by such a scheme, the interlayer adhesion can be not damaged, and a laminated film showing high reflectivity can be obtained by a laminated structure including the a layer and the c layer. Such a laminated film can be suitable for use in, for example, improving the brightness of an image display device.

[0098] Furthermore, by designing the thickness ratio a / b and the thickness ratio c / b in the regular arrangement to be above 1.40, in addition to the relatively thin b layer compared with the a layer and the c layer, the b layer can also be sufficiently thin relative to the reflection wavelength of the laminated film. Therefore, the reflection at the interface between the b layer and the adjacent a layer and the c layer is so low that it can be ignored, and the effect brought by the refractive index difference between the a layer and the c layer is further improved, thereby further improving the reflectivity relative to the reflection wavelength. Considering these aspects, it is an important element to thin-film the b layer showing the intermediate refractive index in a manner that satisfies the thickness ratio condition from the perspective of both improving interlayer adhesion and high reflectivity. The upper limit is not particularly set, but when the b layer is infinitely thinned, the flow of the c layer is easily crushed by the flow of the polymer layer of the adjacent a layer and the c layer, so that the laminated film of the desired b layer film cannot be stably obtained. Therefore, in reality, the thickness ratio a / b and the thickness ratio c / b are preferably less than 10.

[0099] In addition, the second laminated film of the present invention needs to show that more than 90% of the regular arrangements showing the above-mentioned thickness ratio exist. It should be noted that the so-called "more than 90% of the regular arrangements showing the above-mentioned thickness ratio exist" here means that when the number of regular arrangements constituting the laminated film is set to n, more than 0.9n regular arrangements show the above-mentioned thickness ratio. When a laminated film composed of the same thermoplastic resin layer is compared, the presence of a regular arrangement showing a thickness ratio of less than 1.4 means that the thickness ratio of each regular arrangement is uneven, and there is a deviation between the wavelength showing high reflectivity and the wavelength not showing high reflectivity in the reflection band. In particular, since the thickness ratio of less than 1.4 is a thickness ratio condition for identifying the interface between the b layer and the adjacent a layer or c layer, the repetition of the regular arrangement leads to a reduction in the resulting reflection characteristics. Thus, for example, when the reflection band is set to the entire visible light band, since a specific hue cannot be fully reflected (the so-called color leakage state), the laminated film is not a metallic tone but has a color ring-like appearance. It should be noted that even in the case of a main reflection band in the heat ray region exceeding a wavelength of 800nm, a 1 / 2 band or a 1 / 3 band corresponding to its higher-order reflection band is sometimes repeated in the visible light band. Even in such a case, if the regular arrangement showing the above-mentioned thickness ratio is less than 90%, the uneven reflectivity in the higher-order reflection band also significantly occurs, so there is also a problem of poor hue due to color leakage. Therefore, in order to reduce the uneven reflectivity based on wavelength in a specific band, the regular arrangement showing the above-mentioned thickness ratio must exist for more than 90%. From the above viewpoint, it is more preferred that the regular arrangement showing the above-mentioned thickness ratio exists for more than 95%. It should be noted that the upper limit of the regular arrangement showing the above-mentioned thickness ratio is theoretically 100%.

[0100] This condition is highly dependent on the layer thickness distribution design of the laminating device. When the layer thickness distribution in the laminating device body is highly uneven, the discharge ratio of the three extruders can be adjusted to allow the regular arrangement satisfying the above layer thickness ratio to be above 90%.

[0101] It is further important that the second laminated film of the present invention has a reflection band that continuously shows a reflectivity of 20% or more in a range of continuous wavelengths of more than 100 nm within a wavelength range of 300 to 2600 nm. The second laminated film of the present invention achieves high reflectivity by making the thickness of the b layer, which shows the second highest refractive index value among the three thermoplastic resins, thin to a degree that has no effect on the reflection characteristics. As a prerequisite, it is necessary to design the thickness of the regularly arranged layer and the thickness of the b layer relative to it (thickness ratio) in accordance with the interference reflection theory formula (1) in consideration of the wavelength to be reflected. In addition, the reflection band present in the visible light region can be the main reflection band of the laminated film (the widest reflection band observed on the longest wavelength side, equivalent to the reflection band Π described later), or it can be a high-order reflection band observed in the 1 / n band (n is called the order, a natural number) when there is a main reflection band at a longer wavelength position. On the other hand, when the b layer is a thin film to the extent that the above-mentioned thickness ratio requirement is satisfied, in the wavelength band of the reflected light, it shows the same degree of reflectivity as the alternating laminated film of the a layer and the c layer without the b layer. In the case of alternately laminated films, the 1 / 2 band of the main reflection band can be designed to reflect or suppress according to the thickness ratio, but the 1 / 3 band of the main reflection band cannot be suppressed according to the interference reflection theory. Therefore, for example, in order to highly reflect light in the visible light region, it is necessary to have a reflection band that continuously shows a reflectivity of 20% or more in a range of continuous wavelengths of 100 nm or more, from a wavelength of 300 nm or more to 2400 nm, which is three times the wavelength of 800 nm at the long wavelength end of the visible light reflection region.

[0102] It should be noted that in formula (1), k represents a natural number, λ represents a wavelength, Nx, Ny, and Nz represent the refractive index in the x layer, y layer, and z layer, respectively, and dx, dy, and dz represent the layer thickness in the x layer, y layer, and z layer, respectively.

[0103] [Number 1]

[0104] kλ=2(n X d X +n Y d Y +n Z d Z ) (1)

[0105] (where k is a natural number)

[0106] The thickness ratio and the reflection band design can be designed by the layer thickness distribution design of the lamination device and the thickness of the laminated film. The thickness of the laminated film can be adjusted according to the production method of the laminated film described later by the traction speed of the casting, the discharge amount of the extruder, the stretching ratio, etc. according to the appropriate purpose.

[0107] The third laminated film of the present invention needs to have a reflection band that continuously displays a reflectivity of 75% or more in a range of more than 100 nm in a wavelength range of 400 to 800 nm. In order to present an appearance with a specific strong color tone, it is important for the third laminated film of the present invention to display a high reflectivity in the visible light region. Therefore, it is necessary to continuously display a high reflectivity of 75% or more in a range of more than 100 nm in a wavelength range of 400 to 800 nm, preferably more than 80%. It is more preferable to continuously display a reflectivity of more than 80% throughout the entire region of 400 to 800 nm in wavelength. For example, by having less uneven reflectivity and displaying high reflectivity in the range of 400 to 800 nm in wavelength, the resulting laminated film displays a metallic appearance. As an indicator of uneven reflectivity, for example, the standard deviation σ / R of the reflectivity at each wavelength in the reflection band relative to the average reflectivity of the reflection band (range of wavelength 400 to 800 nm) can be cited. The smaller the value, the smaller the reflectivity unevenness. In order to achieve the above-mentioned reflection characteristics, it is effective to increase the number of regular arrangements to increase the number of layers that reflect the target wavelength band, to soften the inclination of the layer thickness distribution, to select a combination of thermoplastic resins that constitute the regular arrangement so that the refractive index difference between the thermoplastic resin layer showing the highest refractive index and the thermoplastic resin layer showing the lowest refractive index is high, etc. These methods can be appropriately combined.

[0108] Furthermore, in the third laminated film of the present invention, it is necessary that 30% or more and 80% or less of the total number of layers constituting the regularly arranged thermoplastic resin layers are thermoplastic resin layers having a layer thickness of 1 nm or more and 25 nm or less. Here, "30% or more and 80% or less of the total number of layers constituting the regularly arranged thermoplastic resin layers having a layer thickness of 1 nm or more and 25 nm or less" means that when the total number of regularly arranged layers constituting the laminated film is set to n, 0.3×n or more and 0.8×n or less of the layers have a layer thickness of 1 nm or more and 25 nm or less. Compared with the conventional laminated film having an alternating laminated structure as the basic structure, the third laminated film of the present invention uses three different thermoplastic resin layers in order to have both the adhesion suitable for long-term use and the high reflectivity characteristics, and it is important to make the thickness of the intermediate thermoplastic resin layer (for example, the layer with the second highest refractive index value, etc.) that may hinder the high reflectivity of the laminated film as thin as possible. As a specific example of such a scheme, for example, when three thermoplastic resin layers are set as α layer, β layer, and γ layer, and the layer structure is set as (αβγβ)x, the thickness of the β layer is made thin. It should be noted that the thin layer is sometimes referred to as a film layer below.

[0109] In particular, when the third laminated film of the present invention is made to reflect light of a specific wavelength, it is important to design the thin film layer to have an optical thickness (refractive index × layer thickness) of 1 / 10 or less of the wavelength so that the thin film layer is not recognized as an interface (in other words, has no influence on the reflection characteristics). Since the third laminated film of the present invention has a reflection band in the wavelength range of 400 to 800 nm (so-called visible light region), if the layer thickness that satisfies the optical thickness of 1 / 10 or less is sufficiently contained at a wavelength of 400 nm, which is the lowest wavelength that can become the short-wavelength end of the reflection band, the laminated film structure that obtains the target high reflectivity can be obtained when the long-wavelength end of the reflection band is located at any position above the wavelength of 400 nm. In addition, although the refractive index varies depending on the thermoplastic resin used, if the refractive index of the thermoplastic resin is taken into consideration, the third laminated film of the present invention can fully satisfy the target high reflection characteristics as long as the thickness of the thin film layer is designed to be 25 nm or less. The lower limit of the thickness of the thermoplastic resin layer (in other words, the thickness of the film layer) constituting 30% or more and 80% or less of the total number of layers of the regularly arranged thermoplastic resin layer is 1 nm. If the lower limit is made thinner than this, the flow of the film layer is easily compressed by the polymer flowability of the layers other than the film layer in the lamination process, and the laminated film of the desired structure cannot be stably obtained. From the viewpoint of the desired reflection characteristics and film forming stability, the thermoplastic resin layer with a layer thickness of 1 nm or more and 25 nm or less needs to be 30% or more and 80% or less, more preferably 40% or more and 80% or less, and further preferably 40% or more and 60% or less. As means for achieving the above range, the adjustment of the layer thickness distribution design of the lamination device, the adjustment of the discharge balance of the three extruders, etc. can be cited, and they can be used in combination as appropriate.

[0110] The third laminated film of the present invention preferably has a regular arrangement in which the thickness ratio α / β of the α layer to the β layer and the thickness ratio γ / β of the γ layer to the β layer show a value of 1.40 or more in 90% or more when the α layer, β layer, and γ layer are arranged in descending order of dielectric constant (refractive index). Here, "the regular arrangement in which the thickness ratio α / β of the α layer to the β layer and the thickness ratio γ / β of the γ layer to the β layer show a value of 1.40 or more in 90% or more" means that when the number of regular arrangements constituting the laminated film is set to n, 0.9n or more regular arrangements show the above thickness ratio. By satisfying this requirement, the third laminated film of the present invention also becomes a laminated film that suppresses uneven reflectance and shows high reflectance over a wide band, as described for the second laminated film of the present invention. From the above viewpoint, it is more preferable that the number of regular arrangements showing the above thickness ratio is 95% or more.

[0111] In the first laminated film of the present invention, preferably, 30% or more and 80% or less of the total number of regularly arranged thermoplastic resin layers are thermoplastic resin layers having a layer thickness of 1 nm or more and 25 nm or less. The reasons for the preference, the preferred range, and the means for achieving such a scheme are as described in the third laminated film of the present invention.

[0112] As the reflective characteristics shown by the laminated film of the present invention, the average reflectivity at a wavelength of 400nm to 800nm ​​is preferably 50% or more and 100% or less. The so-called average reflectivity described here is measured by setting the sampling interval to 1nm according to the "reflection spectral measurement" in the measurement method described later, and the reflectivity at the wavelength of 400nm to 800nm ​​at this time is averaged to obtain the value. By making the reflectivity high throughout the entire visible light region, a laminated film with a more metallic appearance is obtained. From the above viewpoint, the average reflectivity is preferably 70% or more, more preferably 75% or more, further preferably 80% or more, and most preferably 90% or more.

[0113] In order to improve the average reflectivity, the number of regular arrangements can be set to 50 or more; in addition, a combination of a thermoplastic resin layer showing crystallinity and a thermoplastic resin layer formed of an amorphous resin as a thermoplastic resin layer with a high refractive index difference can be used (when selecting a thermoplastic resin, it is particularly effective to make the refractive index difference between the thermoplastic resin with the largest refractive index constituting the regular arrangement and the thermoplastic resin layer with the smallest refractive index large.). In addition, the average reflectivity can also be made high by controlling the thickness ratio of each layer to a required / preferred range in each invention. It should be noted that these methods can also be used in combination as appropriate.

[0114] Even when the maximum reflectivity and the average reflectivity are increased, in order to display a metallic tone, it is preferred that the reflectivity in the wavelength band be controlled to be uneven within a certain range over the entire visible light region. Specifically, when the average value of the reflectivity at a wavelength of 400nm to 800nm ​​is set to R[%] and the deviation of the reflectivity is set to σ[%], the percentage of σ / R is 10.0% or less, thereby eliminating coloration caused by reflection leakage and displaying a good metallic tone. From the above viewpoint, the percentage of σ / R is more preferably 5.0% or less. In order to suppress the uneven reflectivity in the visible light reflection region, the layer thickness distribution is designed in a smoothly inclined manner, the inclination of the layer thickness distribution shows a monotonically continuously increasing distribution, and the combination of thermoplastic resins that will become the main components of the layer with the highest refractive index (preferably A layer and α layer in the first and third laminated films of the present invention, and a layer in the second laminated film of the present invention) and the layer with the lowest refractive index (preferably C layer and γ layer in the first and third laminated films of the present invention, and c layer in the second laminated film of the present invention) is selected in a manner with a high refractive index difference (especially, showing a refractive index difference of more than 0.20) so as to be easily achieved. In addition, it is also effective to make the stacking ratio of each layer within the above range and increase the number of regular arrangements to make the layers that reflect light of the same wavelength more (these methods can be used in combination as appropriate.).

[0115] The laminated film of the present invention preferably has a peeling rate of 10% or less in a square in an adhesion test based on the cross-cut method specified in JIS K 5600-5-6: 1999. It should be noted that the "peeling rate of the square in the adhesion test based on the cross-cut method specified in JIS K 5600-5-6: 1999" is sometimes referred to as the peeling rate below. It is believed that the peeling of the laminated film occurs through both agglomeration / material failure in which the laminated film breaks and peels off, and interfacial failure in which the laminated film peels off at the interface between the thermoplastic resin layers. The peeling caused by these two factors can be grasped in the cross-cut test. Any destruction is a phenomenon that should not occur when the laminated film is used for a long time. A peeling rate of 10% or less in the cross-cut test indicates that the laminated film has the reliability to withstand long-term use.

[0116] The laminated film shows a peeling rate of less than 10%, so that the damage occurring from the laminated film interface during long-term use is reduced. For example, in the processing process, the floating caused by peeling at the interface during the film conveying with rollers and the cracking of the cross-section part in the cutting process are suppressed. As a result, for example, when a protective film is set at a position different from the laminated film, it is possible to suppress the peeling at the laminated film interface due to the peeling strength that is not equal to that during peeling. In particular, in applications such as repeated bending, floating at the interface is not easy to occur, and the original physical properties / optical properties of the laminated film are stably maintained, so it is suitable for long-term use. From the above viewpoints, the peeling rate is more preferably less than 5%, and more preferably 0%. It should be noted that if only the above viewpoints are considered, the smaller the peeling rate, the more preferred, and the most preferred scheme is the scheme with a peeling rate of 0%, but if you want to achieve a peeling rate of 0%, you need to form a regular arrangement of thermoplastic resin layers with similar chemical structures, so sometimes the reflection characteristics of the obtained laminated film may be poor. If this is taken into account, it is also preferred to set the lower limit of the peeling rate to 1%.

[0117] The following describes a preferred laminate structure, resin design, and process conditions for achieving such a low peeling rate.

[0118] As a preferred laminated structure for obtaining a low peeling rate of the laminated film of the present invention, if the first laminated film of the present invention is taken as an example, it has: a regular arrangement of (ABCB)x and (ABCBCB)x with a small number of interface types as described above. Since there are only two types of interfaces, the AB interface and the BC interface, it is sufficient to consider only the resin design of one of the A layer, the B layer, and the C layer and the other two adjacent layers, and it is easy to adopt the resin design described later that is not prone to interlayer peeling. It should be noted that, for example, by replacing the A layer, the B layer, and the C layer with the a layer, the b layer, and the c layer respectively, the second laminated film of the present invention can be explained in the same way, and by replacing them with the α layer, the β layer, and the γ layer respectively, the third laminated film of the present invention can be explained in the same way. The following description can also be explained by replacing the elements in the second and third laminated films of the present invention in the same way.

[0119] In the present invention, a preferred resin design for obtaining a low peeling rate is described. As the simplest method, it is considered to extrude the thermoplastic resins forming the two adjacent thermoplastic resin layers, but when thermoplastic resins with different skeleton structures are mixed with each other, it is technically very difficult to finely disperse and maintain the transparency of the laminated film. Therefore, it can be achieved by copolymerizing the components of the skeleton structure contained in the thermoplastic resin forming the thermoplastic resin layer forming the adjacent layer with respect to the adjacent thermoplastic resin layers forming the interface, or dispersing and containing them as low molecular weight components. As for the amount of common components for copolymerization and kneading, when the two thermoplastic resin layers are compared, it can be achieved by making the components having a common chemical structure be 60 mol% or more and 95 mol% or less when the amount of components constituting the thermoplastic resin is set to 100 mol%. The so-called component amount at this time, for example, in the case of polyethylene terephthalate, refers to 50 mol% of the total dicarboxylic acid component and 50 mol% of the total diol component, which is considered to be 100 mol%. Based on the composition of the thermoplastic resin constituting one thermoplastic resin layer, the total amount of different components in the thermoplastic resin constituting the adjacent thermoplastic resin layer is 5 mol% or more and 40 mol% or less.

[0120] When the amount of common components is less than 60 mol%, the molecules contained in the thermoplastic resin layers are not easy to form intermolecular interactions and lack compatibility. It should be noted that this method is the simplest resin design, but since it becomes a form in which components with different basic skeletons coexist in the main thermoplastic resin constituting the layer, depending on the dispersion mixing conditions, components with different basic skeletons sometimes exist as island structures (domains) in the main thermoplastic resin constituting the layer, and the white turbidity (haze) increases and impairs the transparency of the laminated film. Such domain problems can be overcome by increasing the dispersion of thermoplastic resins. Specifically, it can be achieved by using a mixing extruder with a screw having more than two axes, increasing the ratio of the screw speed to the discharge amount during the mixing of additives, or changing the configuration of the sections involved in the mixing of the screws to a form in which the screws are more deeply engaged with each other, and increasing the mixing degree. Alternatively, it is also preferred to include additives with a common skeleton that improve the interaction of thermoplastic resins.

[0121] In the laminated film of the present invention, as another resin design for achieving a low peeling rate, a prescription can also be used to make the thermoplastic resin layer on one side adjacent to the thermoplastic resin layer contain a terminal functional group component that reacts with the unreacted functional group component contained in the thermoplastic resin layer on the other side. Specifically, it is a method for improving the interaction by reacting the unreacted terminal group contained in the thermoplastic resin forming the thermoplastic resin layer on one side or the terminal group contained in the additive pre-added in the thermoplastic resin layer on one side with the reactive additive in advance, and applying a component having the same basic skeleton structure as the adjacent thermoplastic resin layer. As a functional group for achieving such a reaction, for example, in the case where the layer on one side contains a carboxyl terminal, it can be achieved by adding an additive containing a terminal group highly reactive with a carboxyl group, such as a phenolic group, an epoxy group, an amino group, etc. as a reactive additive. In addition, in the case where the layer on one side contains an alkoxysilyl terminal, it can be achieved by adding an additive containing an inorganic filler or a metal component as a reactive additive. In the case of the present method, similar to the case of copolymerizing, alloying, or blending thermoplastic resins, in addition to the problem of increased haze due to the dispersed state, there is sometimes a problem that unreacted additives further react when heated before the lamination process, causing rheological properties to change and causing lamination disturbance.

[0122] Therefore, as another scheme, a prescription can be cited in which the thermoplastic resin layer on one side adjacent to the other side contains an unreacted functional group that reacts with the unreacted functional group component contained in the thermoplastic resin layer on the other side. For this method, since the thermoplastic resin supplied from the separate extruder in the lamination process reacts only after contact in the lamination process in the lamination process in the lamination device, the rheological behavior of the thermoplastic resin constituting each layer will not change before the lamination process as in the previous method, and the occurrence of lamination disorder can be reduced to improve the adhesion, so it is preferred. For this method, compared with the design in which the terminal group contained in the above-mentioned added additive reacts with the reactive additive in advance, the haze increase is easy to become smaller. As a combination of functional groups to achieve such a reaction, the combination of the above-mentioned functional groups can be used.

[0123] As a control factor for improving the interaction between adjacent thermoplastic resin layers, the difference in compatibility parameters (SP values) of the thermoplastic resins constituting adjacent thermoplastic resin layers can be cited. The so-called compatibility parameters described here are parameters related to the energy inherent in thermoplastic resins. The closer these values ​​of thermoplastic resins are to each other, the more similar the skeleton structures are, the higher the affinity is, and the higher the adhesion at the interface. The compatibility parameters can be estimated by the calculation methods of Hansen, Hoy, and Fedors, but the compatibility parameters of thermoplastic resins as organic polymer materials use the Fedors calculation method that can be calculated based on the molecular structure of the resin. By using this method, the compatibility parameters of thermoplastic resins containing structural units derived from copolymer components can also be simply calculated according to the ratio of each structural unit. For the Fedors calculation method, the compatibility parameters are determined by the cohesive energy density and molar molecular volume of the molecules depending on the type and number of substituents, and the compatibility parameters are estimated according to formula (2). Here, E coh (cal / mol) represents the cohesive energy, V represents the molar molecular volume (cm 3 / mol).

[0124] [Number 2]

[0125]

[0126] The compatibility parameter in the laminated film of the present invention is a value obtained by rounding off the second decimal place of an estimated value calculated based on Fedor's formula. This method is described in F. Fedors, Polym. Eng. Sci., 14(2), 147 (1974).

[0127] In order for the adjacent thermoplastic resin layers to exhibit good adhesion, the compatibility parameters (SP values) of the adjacent thermoplastic resin layers are preferably designed to have a numerical difference of 1.0 or less. In order to reduce the numerical difference of the compatibility parameter, as described above, for example, the components contained in the thermoplastic resins of the adjacent thermoplastic resin layers forming the interface are often obtained by having the components contained in the thermoplastic resins in the range of 60 mol% or more and 95 mol% or less when the amount of the components constituting the thermoplastic resins is set to 100 mol%.

[0128] Next, the lamination process for achieving a low peeling rate is described. In the case of the stretching process described later as an example, the temperature in the heat treatment process in the tenter is preferably heat-treated at a temperature in the range of a temperature lower than the melting point of the thermoplastic resin layer showing the highest melting point among the thermoplastic resin layers constituting the laminated film, and above the melting point of the thermoplastic resin layer with the lowest melting point among the thermoplastic resin layers different from the above-mentioned thermoplastic resin layers. More preferably, the heat treatment is performed at a temperature higher than the melting point of the thermoplastic resin layer showing a high melting point that is lower than the thermoplastic resin layer corresponding to the outermost layer. By heat-treating in the above-mentioned temperature range, when the thermoplastic resin layer different from the crystalline thermoplastic resin layer in the laminated film shows crystallinity or semi-crystallinity, the crystals of the thermoplastic resin constituting the resin layer melt and become amorphous molecules, and the molecular motion is activated by heat, so that the polymers of the thermoplastic resins forming adjacent thermoplastic resin layers at the interface diffuse with each other and the molecules are entangled with each other, and the compatibility of the two is improved. Specifically, in the case of a combination of crystalline / semi-crystalline / amorphous thermoplastic resin layers as a preferred laminated structure of the present invention, it is preferably treated at a heat treatment temperature between the melting points of the crystalline thermoplastic resin layer and the semi-crystalline thermoplastic resin layer.

[0129] On the other hand, in the case where the layer other than the thermoplastic resin layer corresponding to the outermost surface of the laminated film is an amorphous thermoplastic resin layer that does not show a melting point, it is better to be heat-treated at a temperature lower than the melting point of the outermost thermoplastic resin layer and at a high temperature as close to the melting point as possible. That is, in the case of a combination of thermoplastic resin layers showing crystallinity / amorphousness / amorphousness as a preferred laminated structure of the present invention, it is preferably heat-treated at a temperature below the melting point of the crystalline thermoplastic resin layer, and specifically preferably at a temperature range of more than -30°C and less than -5°C of the melting point of the crystalline thermoplastic resin layer. It should be noted that in the case of a laminated film including a crystalline thermoplastic resin layer, the heat treatment temperature of the laminated film can be grasped by the crystallite melting temperature (Tmeta) when the thermal properties of the film are measured by a differential scanning calorimeter (DSC) in the measurement method described later.

[0130] In order to achieve a low peeling rate, it can be achieved by combining multiple elements among the above-mentioned resin composition, laminated structure, and process conditions. Based on the above, for example, the first laminated film of the present invention is a combination of thermoplastic resin layers having three different thermoplastic resin layers arranged in the order of layer A, layer B, layer C, and layer B, wherein layer A is a combination of thermoplastic resin layers having crystalline, layer B is a semi-crystalline or amorphous, and layer C is an amorphous thermoplastic resin as the main component, preferably, when the thermoplastic resin as the main component of layer A is set to A and the thermoplastic resin as the main component of layer C is set to thermoplastic resin C, layer B is a combination of thermoplastic resin obtained by alloying, blending or copolymerizing thermoplastic resin A and thermoplastic resin C as the main component, and the heat treatment temperature in the transverse stretching process is below the melting point of layer A and above the melting point of layer B. The so-called blended resin as the main component described here means that as a manufacturing method, the thermoplastic resin forming the adjacent thermoplastic resin layer, in this example, the thermoplastic resin A and the thermoplastic resin C are blended and supplied at a mass ratio of 5:95 to 95:5, and the thermoplastic resin is included in the components constituting the B layer in an amount of more than 50% by mass and less than 100% by mass. That is, when the entire B layer is set to 100% by mass, the B layer contains a total of more than 50% by mass and less than 100% by mass of the thermoplastic resin A and the thermoplastic resin C. It should be noted that, with respect to the second and third laminated films of the present invention, "A layer, B layer, C layer" can be replaced by "a layer, b layer, c layer", "α layer, β layer, γ layer" respectively and explained in the same way.

[0131] The laminated film with regular arrangement of the present invention can form each thermoplastic resin forming three different thermoplastic resin layers of regular arrangement using more than three extruders and respectively send out from different flow paths, and use a multi-manifold type feed block, a static mixer, etc. as a known lamination device to form a laminate. In particular, as in the present invention, in the case of a high-precision lamination requiring the reflection band to be controlled to a specific band, since the accuracy of the thickness control of each layer becomes very important, it is preferably a method using a feed block with a fine slit. In the case of forming a laminate using a slit-type feed block, the thickness of each layer and its distribution can be achieved by changing the length and width of the slit to tilt the pressure loss. The so-called slit length here is the length of the comb teeth portion of the flow path formed for flowing each thermoplastic resin layer in a certain regular arrangement in the slit plate. In addition, as a simple method for doubling the number of layers, a stacking process using a stacking device can be combined with a splitting / merging process using a square mixer, but in the process from splitting to merging, the cross-sectional area of ​​the flow path of the resin flow changes, and stacking disorder may occur. Therefore, it is preferred that a stacked body with a target number of layers can be constructed in a feed block having fine slits.

[0132] The laminated film of the present invention can be designed to have a layer thickness distribution in which the thickness of each layer of the different thermoplastic resin layers constituting the laminated film increases monotonically from one surface toward the opposite surface, a layer thickness distribution in which the layer thickness increases and then decreases from one side of the film toward the center of the film, a layer thickness distribution in which the layer thickness decreases and then increases from one side of the film toward the center of the film, etc. In addition, the inclination of the layer thickness distribution can be designed to have a continuous change such as a linear, geometric, or differential series, or a layer having approximately 10 to 50 layers having almost the same layer thickness and the layer thickness changes in a step-like manner.

[0133] Since the more layers with the same layer thickness exist, the more the reflectivity of the laminated film under a specific wavelength is improved, it is preferred that the layer thickness increases or decreases toward the center of the film, and the layer thickness distribution of multiple existences of the tilted distribution is distributed, but in the case of the same number of stacked layers and the same band as the target, the distribution of multiple existences of the tilted distribution needs to be designed with fewer stacked layers than the distribution showing a monotonically increased / decreased distribution, so the tilt of the layer thickness distribution becomes larger. Thus, by widening the end of the reflection band, the optical distance of light interference is generated between multiple tilted distributions, so that the size of the fluctuation of the baseline of the reflectivity becomes stronger, thereby sometimes generating the problem of uneven color when the laminated film is identified. In order not to produce the above-mentioned problems, the layer thickness of each thermoplastic resin layer constituting the laminated film preferably shows a monotonically increased layer thickness distribution. The monotonically increased layer thickness distribution can be achieved, for example, by the design of a stacking device such as a feed block (specifically, the adjustment of the slit length and width in the feed block).

[0134] The laminated film of the present invention preferably has a reflection bandwidth of the widest reflection band Π in which the reflectivity continuously shows more than 20% in a range of more than 100 nm in a wavelength range of 300 nm to 2600 nm, and the average reflectivity in the reflection band is set to R [%], and when the film thickness is set to t [μm], (λ·R) / t is greater than 820 and less than 1400. Here, in the reflection spectral spectrum measurement described below in the embodiment, the reflection spectral spectrum obtained by performing 10-point averaging processing on the reflection spectral spectrum obtained by measuring with a spectrophotometer at 1 nm intervals is used for judgment. As described in detail below, by obtaining reflectivity data of 295 nm to 2605 nm in the measurement using a spectrophotometer, the data of 10 consecutive points are averaged, so that the reflection spectral spectrum data of 300 nm to 2600 nm can be obtained.

[0135] use Figures 4 to 7 The widest reflection band Π in which the reflectivity continuously shows 20% or more over a range of 100 nm or more is described. Figures 4 to 7In the figure, symbols 6 to 10 represent the reflection spectrum, reflection band Π, reflection bandwidth λ, maximum reflectivity, and average reflectivity R, respectively. The reflection spectrum of symbol 6 is the spectrum obtained by averaging 10 points. Figure 4 , 5 As shown, for the spectral spectrum subjected to the above-mentioned averaging process, when there are multiple bands where the reflectivity continuously shows 20% or more over a continuous range of 100 nm or more in the band between 300 nm and 2600 nm, the band is located on the longest wavelength side. Figure 5 The diagram shows Figure 4 The average reflectivity and maximum reflectivity under different reflection band shapes. In addition, Figure 6 As shown in FIG. 1 , when the reflection band includes a region where the reflectivity is less than 20%, the long-wavelength band where the reflectivity is continuously 20% or more in the range of 100 nm is defined as the reflection band II, with the region as the boundary. Figure 7 As shown in FIG. 1 , when a band showing a reflectivity of 20% or more over 2600 nm exists on the long wavelength side, in a portion included in a band of 300 nm to 2600 nm, when a reflectivity of 20% or more is shown over a continuous range of 100 nm or more, the band is determined as a reflection band II. It should be noted that, as a means for making the laminated film of the present invention have a reflection band II, after selecting the thermoplastic resin of each layer in a regular arrangement so that the difference between the refractive index of the thermoplastic resin layer with the largest refractive index and the refractive index of the thermoplastic resin layer with the smallest refractive index is 0.09 or more (more preferably 0.16 or more, further preferably 0.18 or more, and particularly preferably 0.20 or more), it is effective to make the number of the regularly arranged layers included continuously 20 or more, more preferably 50 or more, and further preferably 100 or more.

[0136] The reflection bandwidth in the band π is represented by λ[nm], the average reflectivity in the reflection band is represented by R[%], and λ·R is expressed by Figures 4 to 7 The area of ​​the recorded oblique line area is indicated. The area of ​​this area substantially indicates the broadband / high reflectivity performance of the laminated film, but in the case of the laminated film of the present invention, even if the laminated film is produced through the same lamination process, the wavelength band shifts according to the thickness of the laminated film. Therefore, the high reflectivity / wide reflection band effect based on the composition of the laminated film, which is a characteristic of the laminated film of the present invention composed of three different thermoplastic resin layers (or three thermoplastic resin layers with different refractive indices), cannot be expressed only by the area λ·R. Therefore, in the present invention, by dividing the area of ​​the area by the thickness t, the influence of the change in wavelength bandwidth caused by the thickness of the laminated film is eliminated, and the high reflectivity / wide reflection band effect based on the composition of the laminated film is expressed.

[0137] Regarding the area of ​​the region, for example, in the case of a laminated film having a uniform 90% reflection band of 800 nm to 1200 nm, the area (λ·R) is shown as 36000 (1200-800) nm×90% by simple calculation, but if the laminated film is made half as thick, the band becomes 400 nm to 600 nm, so it becomes 18000 (600-400) nm×90%. Even for laminated films with the same laminated structure, the area changes, so the effect of wide reflection band / high reflectivity due to the laminated film structure cannot be expressed. Therefore, if the film thickness of the former is divided by tμm, and the latter is divided by half the thickness t / 2μm, both become (λ·R) / t=18000 / t, and even for laminated films reflecting different wavelengths, the effect of wide reflection band / high reflectivity due to the structure of the laminated film can be compared without depending on the thickness of the laminated film.

[0138] (λ·R) / t being greater than 820 and less than 1400 indicates a laminated film that has both high reflectivity and broadband reflection, although the number of layers is low (thin film), which cannot be achieved using the existing technology, especially the laminated film of (AB)m in which two thermoplastic resin layers are alternately laminated. (λ·R) / t showing greater than 820 indicates that the thickness of the laminated film or the number of layers used to obtain a certain high reflection / high reflection band is small, which is related to suppressing the large-scale manufacturing device or obtaining a laminated film that conforms to the recent trend of thin filmization, such as as an optical film for display. Furthermore, the small thickness of the laminated film improves the operability during post-processing and the processability of sputtering and evaporation. On the other hand, (λ·R) / t being less than 1400 means that considering the interlayer adhesion and the thickness of the laminated film, a high reflectivity / wide reflection band is achieved with a smaller number of layers than the previous alternating lamination technology. In order to achieve high reflectivity / wide reflection band with too few layers, it is necessary to increase the refractive index difference of the thermoplastic resin layer, so it becomes indispensable to laminate thermoplastic resin layers formed by thermoplastic resins with completely different skeleton structures. Therefore, sometimes the interlayer adhesion when a laminated film is made is poor. From the above viewpoints, the more preferred range of (λ·R) / t is 950 or more and 1400 or less, and more preferably 950 or more and 1200 or less.

[0139] In order to satisfy these relationships, it can be achieved by having a preferred laminated structure with the regular arrangement (layer arrangement in brackets) of (ABCB)x, and becoming a preferred resin composition for achieving a low peeling rate. In addition, it is also effective to make the B layer in the regular arrangement not a scheme in which the thermoplastic resin as the main component of the A layer and the thermoplastic resin as the main component of the C layer are mixed, but a scheme in which the main component is a thermoplastic resin different from the main components of the A layer and the C layer. This is because when thermoplastic resins with completely different skeleton structures are made compatible with each other through alloys and blends, it is difficult to evenly disperse the components unless appropriate compatibilizers are combined in appropriate mixing amounts. The mixed thermoplastic resins are prone to form an island structure in the layer, and the island structure sometimes causes a decrease in reflectivity caused by the formation of light diffusion. It should be noted that (ABCB)x can be replaced by (abcb)x in the second laminated film of the present invention, and can be replaced by (αβγβ)x in the third laminated film of the present invention.

[0140] The laminated film of the present invention preferably has a reflection brightness L*SCE (D65) of 0.1% or more and 30% or less. By making the reflection brightness L*SCE (D65) less than 30%, the diffuse light is reduced when the light incident on the laminated film is reflected, so the laminated film has a higher gloss. Laminated films with high gloss have a high-end feel and are suitable for use in various decorations. In addition, since such laminated films do not undergo processing such as vapor deposition and sputtering to provide a metal layer, they also have excellent electromagnetic wave transmittance and recyclability, so they can also be suitably used in applications that require both metallic design and electromagnetic wave transmittance. From the above viewpoints, the reflection brightness L* (SCE) of the laminated film is more preferably less than 20%, and further preferably less than 15%. It should be noted that the reflection brightness L*SCE (D65) can be measured by a spectrophotometer, which is described in detail below.

[0141] In order to make the reflection brightness L*SCE (D65) of the laminated film of the present invention 30% or less, a method of making all the thermoplastic resin layers constituting the regular array a layer containing a single thermoplastic resin or a layer mixed with thermoplastic resins showing good compatibility, a method of using a compatibility-friendly additive in the layer containing the thermoplastic resin, etc. (these methods may be used in combination as appropriate). The reason is that if the compatibility of the thermoplastic resins contained in the thermoplastic resin layer and the compatibility of the thermoplastic resin and the additive are good, the generation of voids during stretching can be suppressed, and the increase of L*SCE (D65) can be suppressed. It should be noted that from the perspective of the winding property of the laminated film, in order to prevent wrinkles and surface scratches when winding into a roll, it is necessary to give the surface layer of the laminated film easy slip, so in reality, L*SCE (D65) is shown to be 0.1% or more. It should be noted that the so-called SCE is an abbreviation of "Specular Component Exclude", which is a value of the brightness of only diffuse reflected light to remove regular reflected light. That is, L*SCE(D65) refers to the brightness of only diffuse reflected light of a D65 light source.

[0142] The laminated film of the present invention preferably has a bending rigidity of 0.5×10 -7 [N·m 2 ] and above and 5.2×10 -7 [N·m 2 ] or less. The so-called bending stiffness is an index indicating the strength of bending per unit length. The higher the value, the harder the film is and the easier it is to introduce wrinkles when bending. The bending stiffness per unit length is represented by E×I, where E represents the Young's modulus of the optical functional film in the bending direction [N / m 2 ], I represents the moment of inertia of the section per unit length, which is represented by formula (3). Since this parameter is particularly strongly affected by the thickness h of the laminated film, the thinner the film, the more resistant it is to bending. When the laminated film is produced by the manufacturing method described below, the bending rigidity is preferably calculated in the length direction and the width direction of the laminated film, and the higher value satisfies 0.5×10 -7 [N·m 2 ] and above and 5.2×10 -7 [N·m 2 From the above viewpoints, the more preferred range of flexural rigidity is 0.5×10 -7 [N·m 2 ] and above and 3.0×10 -7 [N·m 2 It should be noted that the flexural rigidity can be measured according to JIS K-7161 (2014) and JIS K-7127 (1999), which are described in detail below.

[0143] [Number 3]

[0144] EI=E×b×d 3 / 12 (3)

[0145] In addition, in Formula (3), b represents the film width [m] of the measurement object, and d represents the film thickness [m].

[0146] In order to make the bending rigidity of the laminated film of the present invention within the above-mentioned preferred range, it can be achieved by using a crystalline / semi-crystalline / amorphous, or crystalline / amorphous / amorphous resin combination to reduce the elastic modulus, and by designing the layer thickness distribution of the lamination device and optimizing the casting traction and stretching conditions to produce a laminated film having a film thickness of about 50 μm or less and having a reflection band in the visible light reflection region. It should be noted that these methods can be appropriately used in combination.

[0147] The laminated film of the present invention preferably has a peak generated on the highest temperature side in a measurement of dynamic viscoelasticity tan δ at 0° C. to 180° C. as P H , the peak generated on the lowest temperature side is set as P L , will represent P H The temperature on the high temperature side, which is the midpoint between the peak value and the high temperature side baseline, is set as T H [℃], will represent P L The low temperature side temperature of the midpoint between the peak value and the low temperature side baseline is set as T L [℃], T H -T L is greater than 60 and less than 120. For dynamic viscoelasticity measurement, by continuously applying a certain frequency of vibration while increasing the temperature, the softening behavior of the laminated film can be grasped. Since each thermoplastic resin constituting each thermoplastic resin layer of the laminated film of the present invention has a softening point, the response behavior of the loss tangent tanδ corresponding to the softening point is obtained. It should be noted that tanδ can be measured based on the tensile vibration-non-resonance method of JIS K7244-4 (1999) (set it as a dynamic viscoelastic method), which is described in detail below.

[0148] An example of a dynamic viscoelastic spectrum obtained by the laminated film of the present invention is shown in Figure 8 In. Figure 8 In the figure, reference numeral 11 indicates the loss tangent tanδ spectrum obtained by dynamic viscoelasticity measurement, and reference numeral 12 indicates the peak P generated on the lowest temperature side. L [°C], symbol 13 represents the peak P generated on the highest temperature side H [℃], symbol 14 represents the baseline on the low temperature side, symbol 15 represents the baseline on the high temperature side, and symbol 16 represents P LThe temperature T of the low temperature side is the midpoint between the peak value and the low temperature side baseline L [℃], symbol 17 indicates P H The temperature T of the high temperature side is the midpoint between the peak value and the high temperature side baseline H [℃]. Figure 8 , but in the case of a laminated film obtained by combining thermoplastic resins with similar softening points, the number of peaks may be two or one. In addition, when there is no tanδ value that forms a constant baseline and the inclination derived from the peak continues outside the measurement range, the upper limit of the measurement temperature range, 180°C, or the lower limit, 0°C, is used as T H , T L .

[0149] The T H -T L The temperature range in which the laminated film exhibits softening behavior is indicated. A wide range indicates that the laminated film has good temperature responsiveness over a wide temperature range. H -T L The laminate film has a temperature range of 60 to 120°C. When the laminate film is composed of the same thermoplastic resin, when it is used in a molded component having a metallic tone as described later, the molding followability at low temperature during shaping is also improved, and a more homogeneous molded product can be obtained. Since the ease of elongation during molding varies depending on the type of thermoplastic resin, the comparison of laminate films of different types of thermoplastic resins is not limited to this. In order to display such a wide temperature response range, it can be achieved by laminating three thermoplastic resins with different softening points. However, when the softening point temperatures are greatly different, roller adhesion and poor stretching may occur in the film making process depending on the combination of thermoplastic resins. Therefore, it is preferred to use a T H -T L The resin combination is 60% or more and 90% or less.

[0150] The laminated film of the present invention has excellent visible light reflection characteristics compared with conventional laminated films, so it can be preferably used as a decorative purpose such as displaying metallic tones and non-ferrous metal tones. For example, the trend of lightweighting of electric vehicles in automotive applications has accelerated, and the resinization of metal parts has been progressing so far. Therefore, it can be integrally molded with molding resin in front grilles, window seals, car logos, etc. to give metallic tones. In addition, it can also be used in interior components around panels for expressing a sense of luxury. In addition, it can also be used for back decoration of household appliances, electronic equipment, etc., semi-transparent mirror adjustment films, etc. In addition to decorative purposes, as a display application, it can also be used as a brightness enhancement film arranged just above the light guide plate of the backlight of a liquid crystal display, and in quantum dot displays using specific light-emitting elements, organic EL displays, etc., only specific wavelengths such as red and green are reflected without leaking light and utilized. Optical reflective film and utilization.

[0151] As a method of use, the laminate may be applied to a product, or may be used as a molded body by in-mold molding or insert molding. That is, the molded body of the present invention uses the laminated film of the present invention.

[0152] Specific preferred requirements when the laminated film of the present invention is used in a vehicle-mounted component for automobile use are described below. The vehicle-mounted component of the present invention is characterized by comprising a protective layer, a printed layer, an adhesive layer, and the laminated film of the present invention.

[0153] The so-called protective layer refers to a layer provided for the purpose of imparting weather resistance, light resistance, scratch resistance (impact resistance), etc. to the recognition surface. The method for forming the protective layer is not particularly limited as long as the effect of the present invention is not impaired, and a method of laminating resin sheets via an adhesive layer, a method of printing a printed coating, a method of applying a hard coating, a method of laminating a resin substrate via an adhesive, a bonding material, etc., a method of integrating the resin by insert molding, etc. can be used.

[0154] For example, when the laminated film itself is a thin film, it is also preferred to laminate a resin sheet as a protective layer on at least one side of the laminated film via an adhesive from the viewpoint of assisting the moldability of the laminated film and forming a protective layer. The reason is that when the laminated film itself is a thin film, the laminated film itself may have insufficient stiffness and may cause wrinkles during molding. This problem can be alleviated by laminating it with a resin sheet via an adhesive in advance.

[0155] The resin used as the protective layer is not particularly limited, and for example, polybutadiene resin, polystyrene resin, polypropylene resin, acrylic resin, polyacrylonitrile / styrene copolymer resin, polyacrylonitrile / butadiene / styrene copolymer resin, polycarbonate resin, polyacrylonitrile / ethylene propylene / styrene copolymer resin and the like can be used. In addition, the resin used for the resin substrate can contain colorants such as dyes, inorganic pigments, organic pigments, various additives such as antioxidants, antistatic agents, crystal nucleating agents, inorganic particles, organic particles, thinning agents, heat stabilizers, lubricants, infrared absorbers, ultraviolet absorbers, dopants for adjusting the refractive index, etc. In the case of automotive use, since impact resistance, hardness, and heat resistance are required, polycarbonate resins, acrylic resins, and their composites are preferably used.

[0156] In the vehicle-mounted component of the present invention, in order to fully obtain the strength of the molded body suitable for the vehicle-mounted component, the thickness of the protective layer is preferably 200 μm or more and 1 cm or less. On the other hand, from the perspective of the lightweight trend of the film as a vehicle-mounted component, the thickness of the protective layer is more preferably 200 μm or more and 5 mm or less, and further preferably 200 μm or more and 2 mm or less. It should be noted that the thickness of each layer and laminated film constituting the vehicle-mounted component can be measured by observing the cross-section when the vehicle-mounted component and the laminated film are cut parallel to the thickness direction (direction perpendicular to the film surface) with a digital microscope, which is described in detail below.

[0157] The so-called adhesive layer in the vehicle-mounted component of the present invention refers to a layer laminated to prevent peeling at the interface with the printed layer and the protective layer when the laminated film of the present invention is integrally molded. The adhesive layer is preferably provided on at least one side of the laminated film, and it can be bonded to the other component to form a vehicle-mounted component. The components constituting the adhesive layer are not particularly limited, but it is preferably provided with an adhesive layer formed of an acrylic / urethane copolymer resin and two or more cross-linking agents.

[0158] Examples of the acrylic / urethane copolymer resin that constitutes the adhesive layer preferably used in the vehicle-mounted member of the present invention include acrylic monomers such as alkyl acrylates (the alkyl group is methyl, ethyl, n-propyl, n-butyl, isobutyl, tert-butyl, 2-ethylhexyl, cyclohexyl, etc.), hydroxyl group-containing monomers such as 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, and 2-hydroxypropyl methacrylate, amino group-containing monomers such as acrylamide, methacrylamide, N-methylmethacrylamide, N-methylacrylamide, N-hydroxymethylacrylamide, N-hydroxymethylmethacrylamide, N,N-diethylaminoethyl acrylate, and N,N-diethylaminoethyl methacrylate, glycidyl group-containing monomers such as glycidyl acrylate and glycidyl methacrylate, and carboxyl group-containing monomers or salts thereof such as acrylic acid, methacrylic acid, and salts thereof (sodium salts, potassium salts, ammonium salts, etc.).

[0159] In addition, as the urethane component that can be used in the adhesive layer of the vehicle-mounted component of the present invention, a resin obtained by reacting a polyhydroxy compound with a polyisocyanate compound by a known polymerization method for urethane resins such as emulsion polymerization and suspension polymerization can be used. Examples of the polyhydroxy compound constituting the urethane component include polyethylene glycol, polypropylene glycol, polyethylene / polypropylene glycol polybutylene glycol, 1,6-hexanediol, 1,4-butanediol, 1,5-pentanediol, diethylene glycol, triethylene glycol, polycaprolactone, polyhexanediol adipate, polyhexanediol sebacate, polybutylene adipate, polybutylene sebacate, trimethylolpropane, trimethylolethane, pentaerythritol, polycarbonate diol, glycerol, and the like.

[0160] As the crosslinking agent for obtaining the adhesive layer in the present invention, it is preferable to copolymerize the crosslinking functional group, and for example, melamine crosslinking agents, isocyanate crosslinking agents, aziridine crosslinking agents, epoxy crosslinking agents, hydroxymethylated or alkylated urea crosslinking agents, acrylamide crosslinking agents, polyamide crosslinking agents, Oxazoline crosslinking agents, carbodiimide crosslinking agents, various silane coupling agents, various titanate coupling agents, etc.

[0161] In addition, since it is easy to be charged if it is only the component of the above-mentioned adhesive layer, as a result, foreign matter is sometimes mixed between the laminated film and the printed layer or the protective layer due to static electricity, causing a problem of appearance defects. Therefore, in the components of the adhesive layer, from the viewpoint of antistatic, it is preferred to include a conductive polymer. As conductive polymers, polypyrrole, polyaniline, polyacetylene, polythiophene / vinylene (ポリチオフェン·ビニレン), polyphenylene sulfide, poly-p-phenylene, polyheterocyclic / vinylene (ポリヘテロサイクル·ビニレン), etc. can be cited, and (3,4-ethylenedioxythiophene) (PEDOT) is particularly preferred.

[0162] From the viewpoint of making adhesion and film appearance both, the thickness of the adhesive layer of the present invention is preferably 0.5 μm or more and 30 μm or less. If the thickness of the adhesive layer of the present invention is less than 0.5 μm, the adhesion is sometimes impaired. On the other hand, if the thickness of the adhesive layer of the present invention exceeds 30 μm, the film appearance is sometimes impaired by the uneven thickness of the adhesive layer. The preferred range of the thickness of the adhesive layer of the present invention is 0.7 μm or more and 20 μm or less, more preferably 1 μm or more and 10 μm or less, and further preferably 2 μm or more and 5 μm or less.

[0163] In the vehicle-mounted member of the present invention, the thickness of the laminated film of the present invention is preferably 20 μm to 200 μm. Since the laminated film of the present invention is characterized by having a high reflectivity in a thinner film, it is more preferably 20 μm to 70 μm.

[0164] The so-called printing layer in the vehicle-mounted component of the present invention refers to a coloring layer provided on the opposite side of the recognition side of the molded body of the laminated film having visible light transmittance in order to express the desired color tone as an automobile interior material or exterior material. The printing layer is preferably formed of a single color of a standard product such as a standard color, a set color, or a universal color called a printing coating. By forming such a coloring layer, the above-mentioned printing coating is mixed with a colorless and transparent standard product such as a white pigment (medium) or Victoria oil (victoria) to adjust the color concentration, that is, a printing coating in which two or more colors of a standard product such as a standard color, a set color, or a universal color called a printing coating are mixed and toned to a specified color, and the finished product rate can be improved by reducing the working hours, and the printing coating can be formed cheaply.

[0165] The printing coating is not particularly limited as long as the effects of the present invention are not impaired, and examples thereof include those obtained by adding colorants such as dyes, inorganic pigments, and organic pigments to light-transmitting resins such as polyester resins, polyolefin resins, acrylic resins, urethane resins, fluorine resins, polyvinyl acetate resins, vinyl chloride-vinyl acetate copolymer resins, and ethylene-vinyl acetate copolymer resins.

[0166] As a method for forming the printed layer, there is no particular limitation as long as the effect of the present invention is not impaired, and for example, coating or printing can be used. For example, in addition to coating methods such as roller coating, gravure coating, and comma coating, printing methods such as gravure printing and screen printing can also be used. From the perspective of color retention and design after molding, the thickness of the printed layer formed by coating or printing is preferably 1 μm or more and 100 μm or less, more preferably 2 μm or more and 40 μm or less, and further preferably 2 μm or more and 20 μm or more. On the other hand, the higher the reflectivity of the laminated film of the present invention, the less the amount of transmitted light of the laminated film, so the coloring effect brought by the printed layer can be infinitely minimized, resulting in the advantage of being able to make the printed layer thin.

[0167] The laminated film of the present invention has the characteristic of being able to achieve broadband reflection / high reflectivity in the visible light region by using three different thermoplastic resins. According to the characteristic of broadband reflection, in the vehicle-mounted component of the present invention, the thickness ratio of the thickest part to the thinnest part of the laminated film of the present invention is preferably 1.2 times or more and 2.5 times or less, and more preferably 1.2 times or more and 1.5 times or less. Generally, when an optical reflective film having a laminated structure such as the present invention is used as a molded product, a portion of the laminated film is thinned by elongation during molding before and after molding. When a laminated film having a reflection band in the visible light region is used for this purpose, the reflection band moves to the short wavelength side and the coloring problem associated therewith occurs. Therefore, by applying a laminated film showing a wide reflection band, it is possible to maintain the average reflectivity in the visible light region even when the reflection band moves to the short wavelength side by thinning after molding, and the metallic appearance is not damaged.

[0168] It should be noted that in the vehicle-mounted component of the present invention, the thickness ratio of the thickest part to the thinnest part of the laminated film can be measured and calculated by the following steps. First, after cutting the vehicle-mounted component in parallel with the thickness direction of the laminated film (the direction perpendicular to the film surface) at any 10 points, a digital microscope is used to observe the laminated state in each position to measure the thickness of the laminated film in each position. Then, the value obtained by dividing the maximum value of the obtained value by the minimum value is obtained, and it is set as the thickness ratio of the thickest part to the thinnest part of the laminated film of the present invention in the vehicle-mounted component (the detailed measurement method is described below.). In order to make the vehicle-mounted component meet the thickness ratio, and the vehicle-mounted component as a whole has no coloring, etc. and has the same metallic appearance, it is preferred that the reflection band of the laminated film has a reflection band throughout the entire visible light band, and the long wavelength end of the reflection band is on the long wavelength side compared with 950nm, that is, the reflection band shows more than 550nm. Such a laminated film can be achieved by the design of a lamination device.

[0169] Since the laminated film of the present invention can achieve high reflectivity, the vehicle-mounted component of the present invention can be a vehicle-mounted component with a light-shielding area with a light transmittance of less than 20%. Since the laminated film of the present invention itself shows a high reflectivity, it is not necessary to set the printed layer for expressing the design thickly on the entire molded body as in the past, so it is possible to set a light-shielding area laminated with the laminated film as a vehicle-mounted component without implementing a printing screen processing step. Furthermore, depending on the design, it is sometimes required to have a vehicle-mounted component with both a light-shielding area and a light-transmitting area. By using the laminated film of the present invention, the printed layer is made as thin as possible, so that the loss of light transmittance caused by the light absorption of the printed layer does not occur, and it becomes easy to set a region with high light transmittance at the same time as a vehicle-mounted component in addition to the light-shielding area laminated with the laminated film. Specifically, by making the printed layer thin as described above, it is possible to suppress visible light absorption and become a vehicle-mounted component with a light-transmitting area with a light transmittance of more than 80%.

[0170] The following describes the preferred form of a vehicle using a vehicle-mounted component having the above-mentioned characteristics. The so-called vehicle described in the present invention refers to a car traveling on the road, a bicycle with a prime mover, a light vehicle, and a railway vehicle, an industrial vehicle used in a factory, etc. In particular, for automobiles, the installation of an advanced driver assistance system (ADAS) for the purpose of improving safety has been promoted, and as a transmitting device that performs this role, a radar using high-frequency electromagnetic waves, a LiDAR (Light Detection And Ranging) using near-infrared rays, etc. are installed. In the past, vehicle-mounted components formed of metal shells, metal vapor-deposited films, etc. were used, but due to the unique electromagnetic wave shielding / near-infrared reflectivity of metals, it was difficult to combine with these transmitting devices for ADAS.

[0171] Therefore, the vehicle-mounted component using the laminated film of the present invention has a metallic appearance showing reflection in the visible light region as a molded body, and further has excellent visible light reflection characteristics. On the other hand, considering that the reflection characteristics of the near-infrared reflection band can be controlled, it can be preferably used in combination with radars and LiDARs using high-frequency electromagnetic waves.

[0172] The vehicle of the present invention comprises the vehicle-mounted component of the present invention, and a millimeter-wave radar showing peak intensity at any frequency of 22 GHz to 26 GHz, 58 GHz to 62 GHz, and 76 to 80 GHz. Usually, in front of, on the side, and on the rear of the vehicle, a radar is used that uses electromagnetic waves of different frequency bands to be transmitted according to the distance from the surrounding vehicles, bicycles, people, and other moving bodies to be detected. However, if it is a vehicle-mounted component of the present invention, since it does not have shielding performance for any high-frequency electromagnetic waves, it can exhibit excellent electromagnetic wave transmittance in combination with any frequency band radar. Specifically, in the case of an automobile, the vehicle-mounted component of the present invention can be preferably used as an exterior component of the front grille, the vehicle logo portion, and the radar cover portion.

[0173] Furthermore, the vehicle of the present invention can also be a radar cover having infrared transmission, and the radar cover has the vehicle-mounted component of the present invention. By controlling the infrared reflection performance / reflection band of the laminated film by thickness and layer thickness distribution so as not to have reflection performance at the near-infrared wavelength used by LiDAR, it can also be applied to vehicles using LiDAR.

[0174] The image display device of the present invention is described below. The image display device of the present invention comprises a screen protection layer, a light source, a transistor, and the laminated film of the present invention. The so-called image display device refers to a device for displaying an image, and examples thereof include a liquid crystal image display device, an organic EL display, a quantum dot display, and the like.

[0175] The so-called protective layer in the image display device refers to a component used to protect the image display device from the influence of the external environment represented by temperature and humidity. As long as the components constituting the protective layer have the necessary weather resistance, transparency, strength, etc. for the image display device to be applied, the material and thickness are not particularly limited, but preferably optical grade glass materials or plastic materials. In addition, from the perspective of recognizability, the protective layer is preferably transparent. The thickness of the protective layer is generally as long as it is more than 0.2mm and less than 20mm, preferably more than 0.5mm and less than 5mm. The protective layer has a thickness of more than 0.2mm, so that the strength becomes sufficient and the occurrence of cracking is suppressed. On the other hand, the thickness of the protective layer is less than 20mm, so that it becomes an image display device that follows the trend of thinning in recent years. It should be noted that a processing layer with various functions such as anti-glare, oil repellency, antifouling, self-repairing, blue light cutoff, hard coating, etc. can be laminated on the upper side (recognition side) of the protective layer, or a surface treatment film having the processing. The surface treatment film may be a single film or a film having a laminated structure in which a plurality of resins are laminated.

[0176] The so-called light source in the screen display device, in the case of a liquid crystal image display device, refers to a direct backlight, a long-life and high-brightness edge backlight composed of LED lamps and light guide plates arranged in a column shape, etc. In addition, in the case of an organic EL display, it refers to a self-luminous display panel portion having a structure in which a layer composed of molecules that transport holes and electrons and light-emitting molecules that display three colors of red, green, and blue that display fluorescence or phosphorescence is sandwiched by an electrode layer. In the case of a quantum dot display, it refers to the part of the blue LED lamp arranged on the back of a quantum dot sheet containing semiconductor components that excite and emit light in red and green.

[0177] The so-called transistor in the image display device refers to a thin film transistor (TFT) that has been finely processed for applying voltage to the liquid crystal to orient it in the case of a liquid crystal image display device. In the case of an organic EL display, it refers to a transistor formed on a CMOS substrate using a single crystal silicon wafer. The transistor portion can be in the form of a transistor using amorphous silicon, LTPS using polycrystalline silicon, or IGZO using a four-element compound of indium / gallium / zinc / oxygen.

[0178] In the image display device of the present invention, the laminated film of the present invention is preferably used as a brightness increasing film that reflects the emitted light on the back side and reflects it backward toward the recognition side by being applied to the back side of the light source of the image display device. In recent years, with the purpose of expanding the application position of the display, the image display device is used not only in the use of TV, PC display, mobile phone, but also in vehicle-mounted equipment and industrial equipment. Further, as the use of the image display device, as a vehicle-mounted equipment, in addition to the previous navigation device, it is also expanded to the application of the speedometer, warning light, etc. assembled on the instrument panel as a metering instrument panel, and the rear monitor that displays the image behind the vehicle, etc. Among them, sometimes it is required to attach importance to the design of the display device, and the display area is not punched into the previous plane rectangle but punched into a rounded shape, a shape with a complex curved surface, or a shape with a hole in the central part. When punching into such a special shape, for the laminated film designed in a way of high reflectivity based on the previous alternating laminated structure, due to insufficient interlayer adhesion, there is a problem that the laminated film cannot withstand the punching process. Therefore, a laminated film that uses three different thermoplastic resins to achieve interlayer adhesion that can withstand only punching processing, as in the laminated film of the present invention, can be suitably used in a screen display device whose display area is a shape other than a rectangle. That is, the image display device of the present invention preferably has a display area in a shape other than a rectangle.

[0179] The lighting device of the present invention is described below. The lighting device of the present invention has the laminated film of the present invention on the back side of the light source. For the purpose of improving the illumination of LED lighting using light-emitting diodes, lighting using electric heat lamps, etc., by covering the inner surface of the frame covering the lamp with the laminated film of the present invention (in other words, arranging the laminated film on the back of the light source), the light irradiated from the lamp along the frame direction can be reflected to the front, thereby improving the illumination. The lamp frame is generally not on a plane, but often has a curved three-dimensional shape. Therefore, in the lighting device of the present invention, it is preferred that the laminated film of the present invention has a three-dimensional shape. The so-called three-dimensional shape described here means a state in which the length of the longest side of a rectangular parallelepiped formed in a manner of surrounding the formed laminated film is less than 0.9 times the length of the long side of the laminated film used.

[0180] The solar cell module of the present invention uses the laminated film of the present invention. Specifically, the laminated film of the present invention reflects the light of the sunlight that is not absorbed by the cell and is transmitted through the gap to the front so that it re-enters, thereby being used for purposes of increasing the light utilization efficiency of the visible light brought by the cell. Specifically, the laminated film of the present invention having the visible light reflection property can be applied to the upper surface of the back plate part of the solar cell module or the aluminum frame part of the side of the solar cell module.

[0181] Next, the preferred method for manufacturing the laminated film of the present invention is described below. Of course, the present invention is not limited to such an example and is explained. It should be noted that if the first, second, and third laminated films of the present invention are all combinations in which each thermoplastic resin layer satisfies the requirements of each laminated film, they can be manufactured by the same method.

[0182] The thermoplastic resins constituting each thermoplastic resin layer of the laminated film are prepared in the form of particles. After being dried in hot air or under vacuum as required, the particles are supplied to each extruder. When the thermoplastic resin contains additives, the additives of powder / particles / liquid can be mixed and dispersed in the process of this extrusion, or the master batch obtained by pre-dispersing the additives in the thermoplastic resin can be supplied. In the extruder, the extrusion amount of the resin is uniformed by a gear pump etc. of each thermoplastic resin heated and melted to above the melting point, and foreign matter, modified resin etc. are removed through a filter etc. After these thermoplastic resins are formed into the desired laminated body via a laminating device, they are discharged from the die head in a sheet shape. Then, the molten sheet discharged from the die head is extruded onto a cooling body such as a casting drum, and is cooled and solidified to become a cast sheet. At this time, it is preferred to use a filamentous, band-shaped, needle-shaped or knife-shaped electrode, so that it is closely fitted with a cooling body such as a casting drum and quenched and solidified by electrostatic force. In addition, it is also preferred to blow air from a slit-shaped, spot-shaped, or planar device to make it close to a cooling body such as a casting drum and quench and solidify, or to use a roller to make it close to a cooling body and quench and solidify. It is also possible to auxiliaryly apply liquid surfactant water, liquid paraffin, or other liquids with good wettability on the casting drum surface to impart adhesion.

[0183] The thermoplastic resins that form the three different thermoplastic resin layers constituting the laminated film (the case of the first and third laminated films of the present invention. In the case of the second laminated film of the present invention, "three thermoplastic resin layers with different refractive indices" are used instead) are fed out from different flow paths using three or more extruders, and are fed into a multilayer lamination device before being discharged in the form of sheets. As a multilayer lamination device, a multi-manifold die head, a feed block, a static mixer, etc. can be used. In particular, in order to efficiently obtain a multilayer lamination structure, it is preferred to use a feed block with fine slits. If such a feed block is used, the device will not be extremely large-scale, so the amount of foreign matter generated due to thermal degradation is small, and high-precision lamination can be performed even when the number of laminations is extremely large. In addition, the lamination accuracy in the width direction is also significantly improved compared to the prior art. In addition, for this device, since the thickness of each layer can be adjusted by the shape (length, width) of the slit, any layer thickness can be achieved. The molten multilayer laminated sheet having a desired layer structure thus formed is guided to the die to obtain a cast sheet as described above.

[0184] The resulting cast sheet is preferably then biaxially stretched along the length direction and the width direction. The stretching can be biaxially stretched successively or simultaneously. In addition, it can be further re-stretched along the length direction and / or the width direction. Here, the so-called length direction refers to the moving direction of the film, and the so-called width direction refers to the direction orthogonal to the length direction in the film surface.

[0185] The case of sequential biaxial stretching is first described. Here, the so-called stretching in the length direction refers to uniaxial stretching for giving the sheet molecular orientation in the length direction. It is usually implemented by the difference in the peripheral speed of the rollers. It can be carried out in one stage or in multiple stages using multiple roller pairs. The stretching ratio varies depending on the type of resin, but is usually preferably 2 to 10 times. For example, when polyethylene terephthalate or polyethylene naphthalate, which is a thermoplastic resin showing crystallinity and preferably used to form the laminated film of the present invention, is used, it is particularly preferably used 2 to 7 times. In addition, as the stretching temperature, it is preferably set in the range of the glass transition temperature of the thermoplastic resin layer with the highest glass transition temperature among the thermoplastic resin layers constituting the laminated film to the glass transition temperature + 100°C. When strong orientation is performed in the longitudinal stretching step, necking occurs in the film width direction, so that not only a sufficient film width cannot be obtained, but also the thickness unevenness and transmission spectrum unevenness in the longitudinal direction and / or width direction after width stretching may become large.

[0186] After the uniaxially stretched laminated sheet obtained in this way is subjected to surface treatment such as corona treatment, flame treatment, plasma treatment, etc. as required, an easy-adhesion layer having functions such as easy slip, easy adhesion, antistatic properties, etc. is applied by in-line coating. In the in-line coating process, the easy-adhesion layer can be coated on one side of the laminated film, or on both sides of the laminated film at the same time or one side at a time.

[0187] Next, the uniaxially stretched laminate is stretched in the width direction. The so-called width direction stretching refers to stretching for giving the sheet an orientation in the width direction. Usually, it is carried out using a tenter, while holding the two ends of the sheet in the width direction with clamps and conveying it. The stretching ratio varies depending on the type of resin, but is usually preferably 2 to 10 times. For example, when polyethylene terephthalate or polyethylene naphthalate, which is a thermoplastic resin preferably used to form the crystalline thermoplastic resin layer of the laminate film of the present invention, is used, it is particularly preferably used 2 to 7 times. In addition, as the stretching temperature, it is preferably the glass transition temperature of the resin with the highest glass transition temperature among the resins constituting the laminate film to the glass transition temperature + 120°C.

[0188] The biaxially stretched laminated film is subjected to heat treatment in a tenter at a temperature above the stretching temperature and below the melting point of the thermoplastic resin layer with the highest melting point among the thermoplastic resin layers constituting the laminated film, and after being uniformly and slowly cooled, it is cooled to room temperature and wound up. In addition, when slowly cooling from the heat treatment in order to impart thermal dimensional stability, relaxation treatment in the longitudinal direction and / or the width direction may be used in combination as needed.

[0189] Next, the case of simultaneous biaxial stretching is described. In the case of simultaneous biaxial stretching, the obtained cast sheet can be subjected to surface treatment such as corona treatment, flame treatment, plasma treatment, etc. as required, and then given functions such as slipperiness, adhesion, and antistatic properties by online coating. In the online coating process, the adhesive layer can be coated on one side of the laminated film, or on both sides of the laminated unit at the same time or one side at a time.

[0190] Next, the cast sheet is guided to a simultaneous biaxial tenter, and the two ends of the sheet in the width direction are held by a clamp while being transported, and stretched simultaneously and / or in stages in the length direction and the width direction. As a simultaneous biaxial stretching machine, there are a pantograph method, a screw method, a drive motor method, and a linear motor method, but it is preferably a drive motor method or a linear motor method that can arbitrarily change the stretching ratio and can be relaxed at any place. The stretching ratio varies depending on the type of resin, but usually, as an area ratio, it is preferably 6 to 50 times. In the case of using polyethylene terephthalate or polyethylene naphthalate, which is a thermoplastic resin preferably used to form a crystalline thermoplastic resin layer of the laminated film of the present invention, it is particularly preferably used as an area ratio of 8 to 30 times. The stretching speed can be the same speed, or it can be stretched in the length direction and the width direction at different speeds. In addition, as a stretching temperature, it is preferably the glass transition temperature of the thermoplastic resin layer with the highest glass transition temperature among the thermoplastic resin layers constituting the laminated film ~ glass transition temperature + 120°C.

[0191] In order to give planarity, dimensional stability, the sheet of biaxial stretching is preferably then stretched in a tenter frame at a temperature above and below the melting point in order to suppress the distribution of the main orientation axis in the width direction. In the heat treatment, preferably before and / or after entering the heat treatment zone, the sheet is relaxed along the length direction. After heat treatment, the sheet is cooled evenly and slowly, and then the sheet is cooled and wound up until the room temperature. In addition, as required, the sheet can be relaxed along the length direction and / or the width direction when slowly cooled from the heat treatment. In addition, the sheet can be relaxed along the length direction before and / or after entering the heat treatment zone.

[0192] The laminated film obtained as described above is cut to a necessary width by a winding device, and is wound in a roll state so as not to introduce winding wrinkles. It should be noted that both ends of the film may be embossed to improve the winding state during winding.

[0193] The thickness of the laminated film of the present invention is not particularly limited, but is preferably 20 μm or more and 100 μm or less. If the thin film tendency of various functional films is taken into account, it is preferably 70 μm or less, and more preferably 50 μm or less. Although there is no lower limit, in order to stabilize the winding property and form the film without cracking, a thickness of 20 μm or more is preferred in reality.

[0194] The thickness adjustment method of the laminated film is not particularly limited, but preferably the thickness is adjusted without changing the stretching ratio in the conveying direction and the width direction, preferably by the increase or decrease of the traction speed of the cooling body such as the casting drum. In order to suppress the film width contraction that occurs at this time, it is preferred to also appropriately adjust the gap between the die head and the above-mentioned cooling body. In the case where the film width cannot be made constant, for example, the stretching ratio in the width direction can be made constant by adjusting the distance between the clamps in the tenter.

[0195] In addition, on the outermost surface of the laminated film of the present invention, a hard coating layer composed of a curable resin as the main component can be laminated in order to add functions such as scratch resistance, dimensional stability, and adhesion / adhesion. When the laminated film is transported roll to roll in order to install the laminated film on the product, scratches on the surface of the laminated film due to friction between the roll and the film can be prevented. Further, even if the resin oligomer component in the laminated film and the various additives that can be added to the laminated film have the possibility of seeping out during high-temperature heat treatment, by setting the hard coating layer on the outermost surface, the hard coating layer with a high cross-linking density can also show a precipitation inhibition effect. In addition, the dimensional change of the film caused by the heat treatment can also be suppressed by laminating the curable resin layer, and the increase in film thickness caused by heat shrinkage and the changes in optical properties such as the transmission spectrum of the laminated film accompanied therewith can be suppressed. On the other hand, by setting a thermosetting resin layer that shows a low refractive index compared to the refractive index of the thermoplastic resin layer showing crystallinity on the surface of the laminated film optically, the refractive index difference with the air interface becomes smaller, so that surface reflection can be suppressed, and the reflectivity of the laminated film as a whole is improved, so it is preferred.

[0196] In addition to the hard coat layer, as a layer showing functionality, an abrasion resistant layer, an antireflection layer, a color correction layer, an ultraviolet absorption layer, an adhesive layer, a gas barrier layer to which a metal oxide or the like is added, a printed layer, etc. may be formed. These layers may be a single layer or multiple layers, and a single layer may have multiple functions.

[0197] Example

[0198] Hereinafter, the present invention will be described based on examples, but the present invention is not limited to these examples. Each property was measured by the following method.

[0199] (Methods for measuring properties and evaluating effects)

[0200] The method for measuring the characteristics and the method for evaluating the effects in the present invention are as follows.

[0201] (1) Differential Scanning Calorimetry (DSC)

[0202] A differential scanning calorimeter EXSTAR DSC6220 manufactured by Hitachi HiTech Nologis Co., Ltd. was used. The measurement and temperature reading were carried out in accordance with JIS-K-7122 (1987). Specifically, about 5 mg of the sample was placed on an aluminum tray and heated from 25°C to 300°C at a rate of 10°C / min. At a temperature higher than the glass transition temperature Tg (°C) at the intersection of the tangent of the baseline and the inflection point of the step transition portion when the temperature was increased from room temperature, the crystallite melting temperature Tmeta (°C) showing a tiny endothermic peak different from the melting point was read. Furthermore, after the temperature was increased, liquid nitrogen was used for rapid cooling, and the temperature was further increased under the same conditions, and the melting enthalpy Tm (J / g) corresponding to the area of ​​the endothermic peak (melting point) confirmed on the highest temperature side at this time was read.

[0203] (2) Layer composition

[0204] The layer thickness distribution of the laminated film was obtained by observing the sample thinned by an ultra-thin slicer using a transmission electron microscope (TEM). Specifically, a transmission electron microscope JEM-1400Plus (manufactured by JEOL Ltd.) was used to observe the cross section of the laminated film (thickness direction, i.e., the cross section perpendicular to the film surface) under an accelerating voltage of 100 kV, and a cross-sectional image was obtained to determine the layer structure (number of layers, regular arrangement, layer thickness distribution) and the thickness of each layer. It should be noted that in order to obtain the contrast difference between each layer, a staining technique using an electron stain (RuO4, etc.) was used. In addition, according to the thickness of each layer, when the thickness of the thin film layer is less than 100 nm, it is directly observed at a magnification of 40,000 times, when the thickness of the thin film layer is greater than 100 nm and less than 500 nm, it is directly observed at a magnification of 20,000 times, and when it is greater than 500 nm, it is observed at 1,000 to 10,000 times according to the thickness, and the layer thickness distribution is analyzed. Based on the contrast difference of the obtained image, the number of stacked layers, regular arrangement, layer thickness of each layer, and layer thickness distribution were determined.

[0205] (3) Layer interface (poor contrast)

[0206] The cross-sectional image obtained in the transmission electron microscope observation of (2) was converted into a compressed image file (JPEG) format, and the position-brightness data was obtained by the spectrum profile along the thickness direction of the laminate film using ImagePro-10 manufactured by MediaCybernetics. Then, using spreadsheet software (Microsoft "Excel" (registered trademark) 2016), the relationship between position and brightness was plotted, and a 5-point moving average was applied to the obtained spectrum. The average processing was performed by averaging the brightness of 5 consecutive measurement positions, changing the position one point at a time and continuously processing the same calculation, and an averaged position-brightness spectrum was obtained. In the obtained averaged position-brightness spectrum, the position surrounded by the inflection point where the slope changes from positive to negative, or from negative to positive, is judged as one layer. For each layer obtained by this method, the position-brightness data was then obtained for the plane direction of the laminate film (the direction perpendicular to the thickness direction). After calculating the average value and standard deviation of the brightness obtained for each layer, if the difference between the average values ​​of the brightness of two adjacent layers is greater than any one of the standard deviations of the brightness of the adjacent thermoplastic resin layers, it is determined that these two adjacent layers are different. In addition, the difference (distance) between the positions of the inflection points is calculated as the layer thickness of each layer.

[0207] (4) Thickness ratio

[0208] The thickness ratio of each regular arrangement constituting the laminated film is calculated using the layer thickness calculated by the method described in (2) and (3). Specifically, focusing on the regular arrangement of the portion other than the outermost layer of the laminated film, the thickness ratio A / B and the thickness ratio C / B are calculated from the total value of the layer thickness of all A layers and all C layers contained in the regular arrangement, taking the total value of the layer thickness of all B layers contained in the regular arrangement as a reference. After the thickness ratios of each regular arrangement contained in the laminated film are calculated as described above, their average values ​​are set as the final thickness ratio A / B and thickness ratio C / B.

[0209] (5) Reflection spectroscopic measurement

[0210] The sample was cut out from the center of the laminate film in the width direction with a 4 cm square, and a black paint spray was used on one side of the laminate film to implement a back black treatment. For the back black treatment, three repeated coatings were applied to achieve a completely non-transmissive state. Using the spectrophotometer U-4100 manufactured by Hitachi HiTech Science, an alumina plate was fixed as a reflective member at the opening on the back of the integrating sphere. In addition, as an absolute reflectivity measurement unit using specular reflection, the attached 12° regular reflection attachment (P / N134-0104) was set just in front of the integrating sphere, and the untreated side of the sample with back black treatment was facing the unit side to make it firmly close, and the reflection spectroscopic spectrum in the wavelength range of 295nm to 2605nm was continuously measured, and the continuous 10-point data was averaged to obtain the reflection spectrum data of 300nm to 2600nm. During the measurement, the scanning speed was set to 600nm / minute and the sampling interval was set to 1nm. Based on the obtained reflection spectroscopic spectrum, the widest reflection band in which the reflectivity continuously shows more than 20% in a range of more than 100nm is set as Π, the reflection bandwidth of this band Π is set as λ, and the average reflectivity of the reflection band is set as R and read. In addition, the maximum reflectivity and average reflectivity at a wavelength of 400 to 800nm, the reflection band (and its presence or absence) that continuously shows a reflectivity of more than 20% in a range of more than 100nm in a range of 300 to 2600nm, and the reflection band (and its presence or absence) that continuously shows a reflectivity of more than 75% in a range of more than 100nm in a range of 400 to 800nm ​​are also read from the obtained reflection spectroscopic spectrum, and whether the reflectivity of more than 80% is continuously displayed in the entire region of 400 to 800nm ​​is also implemented by the spectrum. Further, the standard deviation σ of the reflectivity in the reflection band is calculated, and the reflectivity unevenness in the reflection band is set to σ / R×100 and calculated as a percentage.

[0211] (6) Cross-cut peeling rate

[0212] The evaluation was conducted according to the adhesion (cross-cut) test method specified in JIS K 5600-5-6 (1999). Using a cross-cut guide CCJ-1 with a spacing of 1 mm manufactured by COTEC, 11 orthogonal cuts were introduced in the vertical and horizontal directions at an angle of 20 to 30 degrees using an NT cutter to produce 100 squares. A 24 mm wide "Selotime" (registered trademark) manufactured by Nichiban was pasted on the squares, and the tape was quickly peeled off at an angle of about 60 degrees, and the number of completely peeled squares was read. This operation was repeated 10 times, and the average number of peeled squares was calculated to calculate the peeling rate.

[0213] (7) Haze

[0214] A haze meter (HGM-2DP) manufactured by Suga Testing Instruments Co., Ltd. was used. The sample was cut into 10 cm × 10 cm pieces from the center of the film width direction, and the total light transmittance and haze value were measured according to the old JIS-K-7105 (1994). Three points were measured at equal intervals in the film width direction, and the average value was used as the measurement result.

[0215] (8) Electron Energy Loss Spectroscopy (EELS)

[0216] Before the measurement, the main orientation axis direction of the laminated film of the object to be measured was determined using a phase difference measuring device (KOBRA-WPR) manufactured by Prince Instruments Co., Ltd. The in-plane phase difference measurement using this phase difference measuring device was performed, and the direction consistent with the numerical value of the orientation angle obtained was judged as the main orientation axis direction. With respect to the main orientation axis direction, a cross-section (thickness direction cross-section) cutting sample of the object to be measured was prepared by an ultra-thin sectioning method using an ultra-thin slicer. The dielectric constant of the prepared cross-section cutting sample was measured using an atomic resolution analysis electron microscope ARM200F manufactured by JEOL. Specifically, after obtaining a HAADF-STEM (High Angle Annular Dark-Field Scanning Transmission Electron Microscopy) image with an acceleration voltage of 80 kV and a beam spot size of 0.2 mmφ, a multi-point analysis (60×60 pixels, 20 nm / pixel) was performed on the layer of the object to be measured at 50 msec, and data on energy loss and electron beam intensity were obtained. The same operation was performed on each of the same thermoplastic resins in the laminate film at 3 points each, and data with improved S / N ratio were obtained. From the obtained spectrum, background correction due to elastic scattering and removal of multiple scattering effects were performed, and then the dielectric function of each layer was calculated by Kramers-Kronig transformation shown in formula (4). The integration range during Kramers-Kronig transformation was set to 0 to 200 eV. Based on the dielectric function of formula (4), the real part and imaginary part of the dielectric constant were calculated from formulas (5) and (6), respectively, and then the dielectric constant was calculated from the square root of the sum of their squares by formula (7). After the dielectric constant of each thermoplastic resin layer at a loss energy of 2.5 eV was calculated by the above method, the dielectric constant ratio was found from the ratio of the largest dielectric constant to the smallest dielectric constant.

[0217] It should be noted that in equations (4) to (7), Re represents the real part, Im represents the imaginary part, ε represents the dielectric constant (average value), ε(ω) represents the dielectric function, ε1 represents the real part of the dielectric constant, ε2 represents the imaginary part of the dielectric constant, and ω and ω' represent angular frequencies.

[0218] [Number 4]

[0219]

[0220] [Number 5]

[0221]

[0222] [Number 6]

[0223]

[0224] [Number 7]

[0225]

[0226] (9) Reflection brightness L*(SCE)

[0227] The sample was cut out from the center of the laminate film in the width direction with a 4 cm square, and a black paint spray was used on one side of the laminate film to implement a back black treatment. For the back black treatment, the coating was repeated 3 times to achieve a state of non-transmitting light. The spectrophotometer CM3600d manufactured by Conika Minolta Sensing was used, and the lightness L*(SCE) of the reflected hue of the sample obtained by the back black treatment was measured after calibration using the attached white calibration plate and zero calibration box. Specifically, an MVD accessory with a measurement diameter of 8 mm was installed, the light source was a D65 light source, and the incident surface of the light was the back non-treated surface, and the lightness L*(SCE) at this time was read. The same measurement was performed at 3 randomly selected points within the 4 cm square laminate sample surface, and the average value was set as the L*SCE(D65) of the laminate film to be measured.

[0228] (10) Flexural rigidity

[0229] According to JIS K-7161 (2014) and JIS K-7127 (1999), the measurement was carried out under the following conditions. The laminated film was cut into a rectangular shape of 10 mm × 200 mm with the length direction as the long side, and set as a sample. Next, the sample was stretched at room temperature of 23°C, 5 cm between chucks, and a stretching speed of 300 mm / min using the automatic film strength and elongation measuring device "Tensilon" (registered trademark) AMF / RTA-100 produced by Olientech (KK), and the Young's modulus in the length direction was measured. Similarly, the sample with the width direction as the long side was also measured, and the Young's modulus in the width direction was set. The above measurement was performed 5 times in the length direction and the width direction of each laminated film, and the higher side of the average value of the obtained values ​​was set as the Young's modulus E of the laminated film. The flexural rigidity of the laminated film is represented by the product EI of the Young's modulus E and the moment of inertia I of the section. That is, the flexural rigidity EI of the laminated film is represented by the following formula (3), where b is the width of the measurement sample and d is the film thickness. The value calculated by substituting the Young's modulus E measured by the above method into the following formula is taken as the flexural rigidity.

[0230] [Number 8]

[0231] EI=E×b×d 3 / 12 (3)

[0232] In addition, in Formula (3), b represents the film width [m] of the measurement object, and d represents the film thickness [m].

[0233] (11) Dynamic viscoelasticity tanδ measurement

[0234] The loss tangent spectrum was obtained using a dynamic viscoelasticity measuring apparatus DMS6100 manufactured by Seiko Instruments Co., Ltd. in accordance with the tensile vibration-non-resonance method (referred to as a dynamic viscoelasticity method) of JIS K7244-4 (1999). The detailed measurement conditions are as follows.

[0235] Measurement mode "tensile", distance between chucks "20 mm", width of test piece "10 mm", frequency "10 Hz", strain amplitude "10 μm", minimum tension "20 mN", initial value of force amplitude "40 mN", measurement temperature "250°C to 180°C", heating rate "2°C / min".

[0236] (12) Long-term reliability test

[0237] A constant temperature and humidity machine (LHL-114) manufactured by Espec Co., Ltd. was used. A 10 cm square sample was cut out from the obtained laminated film, and the sample was placed in the constant temperature and humidity machine while being sandwiched between two sheets of ordinary paper. After 500 hours of standing treatment, the cross-cut peeling rate described in (6) and the change in haze value (Δ haze) described in (7) were evaluated and judged as A to D as follows.

[0238] A: The change in the peeling rate was 1% or less, and the Δ haze was 0.1% or less.

[0239] B: Not equivalent to A, the change in peeling rate is 5% or less, and the Δ haze is 0.5% or less.

[0240] C: Neither A nor B is equivalent, the change in the peeling rate is 10% or less, and the Δ haze is 1.0% or less.

[0241] D: None of A to C is equivalent.

[0242] (13) Electromagnetic wave transmittance

[0243] On the entire surface of one side of the laminated film, a solvent-based ink "UPX" black (480) made by Minogrup Co., Ltd. and "UPX standard dilution solvent" made by Minogrup Co., Ltd. were mixed and diluted at a ratio of 100:20 (mass ratio), and a 4μm thick printing layer was set using a 250-mesh screen by a screen printer. Then, a high-pressure molding machine was used to heat to 180°C and a pressure of 100 bar to form a three-dimensional convex shape (100mm×100mm) on the printing layer side, and then the unnecessary parts were removed. Next, the laminated body, which has been partially shaped and the unnecessary parts removed, is placed in the mold of an injection molding machine, and a molten polycarbonate resin (301-22 manufactured by Sumika Polycarbonate Body Co., Ltd.) is injected on the opposite side of the printed layer, and the molded product (equivalent to a vehicle-mounted component. Hereinafter, simply referred to as a molded product) is obtained by welding and integration. The thickness of the polycarbonate resin layer at this time is set to about 1 mm. A 76GHz MIMO radar module T18PE_01120112_2R5D_76G manufactured by Esta Kaya is placed on the back of the molded product, and the relative intensity [dB] of the electromagnetic wave that passes through the molded body and is reflected and bounced back from the wall surface at a distance of 3m in a straight line is measured, and the determination is made as described below based on the measurement results with and without the molded body. It should be noted that the evaluation result is that A is the most excellent.

[0244] A: The relative intensity of electromagnetic waves is less than 10dB.

[0245] B: The change in relative intensity of electromagnetic waves is greater than 10 dB.

[0246] (14) Near infrared radar transmittance

[0247] In the method for manufacturing a molded product described in item (13), a printed layer of a laminated film is not provided, and a molded body is produced by the same method. The obtained molded body is subjected to a spectrophotometer U-4100 manufactured by Hitachi HiTech Science, and an attached relative transmission unit is installed, and an alumina plate is fixed as a reflective member in the opening on the back of the integrating sphere. The molded body is fixed to the front of the integrating sphere in close contact, and the average transmittance at a wavelength of 900nm to 1600nm is measured, thereby simulating and verifying the radar transmittance of the molded body as described below. It should be noted that the evaluation result is that A is the most excellent, and C is treated as a characteristic that is difficult to apply to a radar cover of LiDAR.

[0248] A: The average transmittance was 80% or more.

[0249] B: The average transmittance is 30% or more and less than 80%.

[0250] C: The average transmittance showed less than 30%.

[0251] (15) Determination of light transmittance of molded products

[0252] The average transmittance of the planar portion of the convex portion of the molded article produced in item (13) at a wavelength of 400 nm to 800 nm was measured using a spectrophotometer U-4100 manufactured by Hitachi High-Tech Science and Technology Co., Ltd., to evaluate the light transmittance of the molded article at the position where the laminate film was molded.

[0253] (16) Thickness of each layer constituting the molded product

[0254] The thickness of each layer and laminated film constituting the molded product produced in item (13) was measured by observing the laminated state using a digital microscope VHX-5000 manufactured by Keyence Corporation when the cross section when the molded product was cut parallel to the thickness direction of the laminated film (direction perpendicular to the film surface). A high-magnification lens capable of observation at a maximum magnification of 5000 times was installed, and observation was performed at an observation magnification of 1000 times when the layer thickness was 10 μm or more, and at an observation magnification of 5000 times when the layer thickness was less than 10 μm.

[0255] (17) Thickness ratio of the thickest part to the thinnest part of the laminate film in the molded product (an indicator of molding followability)

[0256] In the molded product produced in item (13), the thickness ratio of the thickest part to the thinnest part of the laminated film is measured and calculated by the following steps. First, after cutting the molded product parallel to the thickness direction of the laminated film (the direction perpendicular to the film surface) at any 10 points, the digital microscope VHX-5000 of Keyence Company was used to observe the laminated state at each position to measure the thickness of the laminated film at each position. The value obtained by dividing the maximum value obtained by the minimum value is set as the thickness ratio of the thickest part to the thinnest part of the laminated film in the molded product. It should be noted that the observation magnification using the digital microscope is as described in item (16). In addition, when selecting any 10 points for cross-sectional observation, in order to correctly grasp the thickness ratio, at least 3 places are selected from parts with strong elongation such as the ends of the molded product, and at least 3 places are selected from positions with weak elongation while maintaining flatness.

[0257] (18) Measurement of front brightness of display

[0258] As a display for evaluation, a light source unit of Sony KD-65X9500B was used. The display for evaluation was made by arranging a laminated film just below the backlight attached to the light source unit and assembling the display again. A colorimeter BM-7 manufactured by Topcontec Nohaus was used to evaluate the brightness at a total of five points, including the center (symbol 19) of the light source unit (symbol 18), a point on a straight line passing through the center of the light source unit and parallel to the long side of the light source unit and located in the middle of the end and center of the light source unit (point 2, symbol 20), and a point on a straight line passing through the center of the light source unit and parallel to the short side of the light source unit and located in the middle of the end and center of the light source unit (point 2, symbol 21), and the average value was used as the brightness data. Furthermore, the brightness before inserting the laminated film was set to 100%, the relative brightness value was calculated, and the front brightness was evaluated based on the following criteria.

[0259] A: A relative brightness value exceeding 110% was obtained.

[0260] B: A relative brightness value exceeding 105% and not more than 110% was obtained.

[0261] C: A relative brightness value exceeding 102.5% and 105% or less was obtained.

[0262] D: A relative brightness value of 102.5% or less was obtained.

[0263] The following describes the thermoplastic resin, additives, and water-based coating material X used in the examples of the present invention. The copolymerization component amount of the polyester resin described here indicates the copolymerization amount relative to 100 mol % of the acid component and 100 mol % of the diol component.

[0264] <Thermoplastic resin>

[0265] Resin 1: a crystalline homopolyethylene terephthalate resin (refractive index: 1.66) having a glass transition temperature of 78°C, a melting point of 254°C, and a melting enthalpy of 40 J / g

[0266] Resin 2: A crystalline polyethylene terephthalate resin (refractive index: 1.63) copolymerized with 10 mol% of isophthalic acid, showing a glass transition temperature of 79°C, a melting point of 230°C, and a melting enthalpy of 12 J / g.

[0267] Resin 3: Semi-crystalline polyethylene terephthalate resin (refractive index: 1.61) copolymerized with 15 mol% of isophthalic acid, showing a glass transition temperature of 77°C, a melting point of 217°C, and a melting enthalpy of 2 J / g

[0268] Resin 4: a crystalline polyethylene naphthalate resin (refractive index: 1.73) copolymerized with 5 mol% of polyethylene glycol having a molecular weight of 400, showing a glass transition temperature of 97°C, a melting point of 254°C, and a melting enthalpy of 33 J / g.

[0269] Resin 5: Amorphous polyethylene terephthalate resin (refractive index: 1.57) copolymerized with 33 mol % of cyclohexanedimethanol and having a glass transition temperature of 80°C

[0270] Resin 6: Amorphous polyethylene terephthalate resin (refractive index: 1.55) copolymerized with 20 mol % of spiroglycol and having a glass transition temperature of 77°C

[0271] Resin 7: A crystalline acid-modified ethylene-propylene copolymer resin having a melting point of 133° C. (refractive index: 1.53)

[0272] Resin 8: Amorphous homo / polymethylene methacrylate resin (refractive index: 1.49) having a glass transition temperature of 101°C

[0273] Resin 9: a crystalline poly(m-xylylene adipamide) resin (refractive index: 1.52) having a glass transition temperature of 86°C and a melting point of 237°C.

[0274] Resin 10: An amorphous thermoplastic resin (refractive index: 1.61) having a glass transition temperature of 99° C. obtained by alloying resin 4 and resin 8 at a volume concentration ratio of 50:50.

[0275] Resin 11: A crystalline polyethylene terephthalate resin (refractive index: 1.63) copolymerized with 8 mol % of dimethyl 5-sulfoisophthalate, having a glass transition temperature of 78° C. and a melting point of 253° C.

[0276] The refractive index referred to here is the in-plane refractive index measured by the following steps. First, with respect to a thermoplastic resin showing a melting point, a biaxially stretched monofilm having a thickness of 25 μm produced by the manufacturing method described in Example 1 using the thermoplastic resin was obtained (wherein, in the manufacture of the biaxially stretched monofilm, the stretching temperature was set to the glass transition temperature of each thermoplastic resin + 10°C (80°C for resin 7 that does not show a glass transition temperature). In addition, the thickness was adjusted by the pulling speed of the casting drum.). Then, the obtained biaxially stretched monofilm was subjected to in-plane phase difference measurement using a phase difference measuring device (KOBRA-WPR) manufactured by Oji Instruments Co., Ltd., and the direction consistent with the numerical value of the obtained orientation angle was set as the main orientation axis direction. Next, a laser beam with a wavelength of 632.8 nm was irradiated in each of the main orientation axis direction and the direction orthogonal to the main orientation axis in the film plane using a prism coupler SPA-4000 manufactured by Sairon Technology, and the refractive index at this time was read, and the average value thereof was adopted as the refractive index of each thermoplastic resin, which was regarded as the refractive index of each thermoplastic resin layer. In addition, regarding the amorphous resin, the same measurement as above was performed on the cast sheet produced by the manufacturing method described in Example 1, and the refractive index of each thermoplastic resin (each thermoplastic resin layer) was set.

[0277] <Additives>

[0278] An acrylic polymer having an epoxy value of 1.4 meq / g and an average molecular weight of 2900 g / mol.

[0279] <Water-based coating agent X>

[0280] To a material obtained by mixing the following polyester resin 1 (100 parts by mass), reactive compound 1 (30 parts by mass), and reactive compound 2 (30 parts by mass), 0.5 parts by mass of silica colloidal particles having a particle size of 100 nm were added relative to 100 parts by mass of a binder resin corresponding to a mixture of the above resins and compounds, and after adjusting the solid content concentration to 5 parts by mass using water as a solvent, 0.03 parts by mass of a surfactant was added relative to a total of 100 parts by mass of water and mixed to prepare a coating composition.

[0281] Polyester resin 1:

[0282] The following steps were performed to obtain an aqueous dispersion of a polyester resin composed of the following copolymer composition. The following copolymer components and 0.1 parts of potassium titanium oxalate as a catalyst were added to a reactor, and the mixture was heated to 200°C under normal pressure and nitrogen atmosphere while being stirred and mixed. Next, the reaction temperature was slowly raised to 250°C over 4 hours to complete the transesterification reaction. 15 parts by mass of the polyester resin and 85 parts by mass of water were added to a dissolving tank and dispersed at a temperature of 80 to 95°C for 2 hours under stirring to obtain a 15% aqueous dispersion of the polyester resin.

[0283] (Copolymer composition)

[0284] ·Dicarboxylic acid component

[0285] Dimethyl 2,6-naphthalene dicarboxylate: 88 mol%

[0286] Sodium 5-sulfoisophthalate dimethyl ester: 12 mol%

[0287] Diol component

[0288] Compound containing 2 mol of ethylene oxide added to 1 mol of bisphenol S: 86 mol%

[0289] 1,3-Propanediol: 14 mol%

[0290] Reactive compound 1:

[0291] Carbodiimide water-based crosslinking agent (Nisshinbo Chemical Co., Ltd. "Carbodiimide" (registered trademark) V-04)

[0292] Reactive compound 2:

[0293] contain Aqueous dispersion of oxazoline polymer ("Epocros" (registered trademark) WS-500 manufactured by Nippon Shokubai Co., Ltd.).

[0294] (Example 1)

[0295] As the thermoplastic resins constituting the thermoplastic resin layers A, B, and C, resin 1, resin 2, and resin 5 were used in order. The prepared thermoplastic resins were respectively put into three twin-screw extruders in the form of pellets, melted and kneaded at 270°C, 270°C, and 280°C, respectively. The kneading conditions were set so that the screw speed relative to the discharge amount was 0.7. Then, after passing through 7 FSS-type leaf disk filters, they were metered by a gear pump and merged by a feed block with 601 slits and a temperature adjusted to 270°C, forming a thickness ratio A / B showing 0.98, a thickness ratio C / B showing 1.02, and being stacked in a regular arrangement of A layer / B layer / C layer / B layer in the thickness direction, and the two surface layers became a 601-layer stacked body like the A layer. Here, the length and width of the slit in the feed block are designed so that the layer thickness increases monotonically from the outermost surface on one side toward the outermost surface on the opposite side, except for the two outermost layers. Then, the laminated body that has passed through the feed block is supplied to a T-die, formed into a sheet, and then rapidly cooled and solidified on a casting drum whose surface temperature is maintained at 25°C while applying an 8kV electrostatic voltage with a wire to obtain an unstretched laminated cast sheet. The obtained laminated cast sheet is heated with a roller set at 70 to 80°C, and then stretched 3.3 times in the longitudinal direction while being rapidly heated from both sides of the film by a radiation heater in a stretching section of 100 mm, and then temporarily cooled. Next, after the two sides of the obtained laminated uniaxially stretched film were subjected to corona discharge treatment in air so that the wetting tension of the base film was 55mN / m, a water-based coating agent X (hereinafter referred to as coating) as a slippery layer was applied to the treated surfaces of both sides of the film using a #4 scraper bar to form a transparent / slippery / easy-adhesive layer. Further, the uniaxially laminated film was guided to a tenter, preheated with hot air at 85°C, and stretched 3.6 times in the film width direction at a temperature of 90°C. The biaxially stretched film was heat-set with hot air at 200°C immediately after the transverse stretching, and was subjected to a 5% relaxation treatment in the width direction just before the tenter exit and then wound up. The obtained laminated film was further used to produce a molded product by the method described in item (13) of "Method for measuring characteristics and method for evaluating effects". The evaluation results of the obtained laminated film and molded body are shown in Table 1-2.

[0296] (Examples 2 to 16, Examples 19 to 25, Examples 27, 28, 31, 32, Comparative Examples 1, 2, 4)

[0297] The resin, additives, number of layers of the feed block, the discharge rate of the extruder (thickness ratio in a regular arrangement), the film-making conditions, and the film thickness of each layer were changed as described in Tables 1-1, 2-1, and 3-1. A laminated film and a molded body were obtained in the same manner as in Example 1. The evaluation results of the obtained laminated film and molded body are shown in Tables 1-2, 2-2, and 3-2. It should be noted that the thickness of the laminated film was adjusted by the drawing speed of the casting drum.

[0298] (Examples 17 and 18)

[0299] A laminated film was obtained in the same manner as in Example 16 except that the epoxy terminal modifier for improving adhesion was pre-compounded in a predetermined addition concentration in the thermoplastic resin listed in Table 2-1 and used as the thermoplastic resin constituting the thermoplastic resin layer. The evaluation results of the obtained laminated film are shown in Table 2-2.

[0300] (Example 26)

[0301] In Example 20, as a feed block, a slit plate having two pieces with 301 slits was used, and the length and width of the slits in the feed block were designed so that the layer thickness monotonically increased from the outermost surface of one side toward the middle layer (301 layer) except for the two outermost layers and the middle layer (301st layer), and the layer thickness monotonically decreased from the middle layer toward the outermost layer on the opposite side. A laminated film was obtained by the same operation as the manufacturing method described in Example 20. It was confirmed by transmission electron microscope observation that the two surface layers and the middle layer showed a thick film layer of 5 μm. The evaluation results of the obtained laminated film are shown in Table 3-2.

[0302] (Examples 29 and 30)

[0303] In Example 1, the thermoplastic resins constituting the thermoplastic resin layers A, B, and C were the resins listed in Table 3-1. Furthermore, as a laminating device, a feed block having three slit plates with the number of slits listed in Table 3-1 was used, which was designed to be laminated in a regular arrangement of A layer / B layer / C layer in the thickness direction and to show a layer thickness distribution in which the layer thickness monotonically increases from the outermost layer on one side toward the outermost layer on the opposite side. In addition, the extruder discharge (thickness ratio in the regular arrangement) and the film-making conditions (stretching ratio, stretching temperature, heat treatment conditions) were changed as described in Table 3-1, and a laminated film was obtained in the same manner as in Example 1. The evaluation results of the obtained laminated film are shown in Table 3-2.

[0304] (Comparative Example 3)

[0305] As the thermoplastic resins constituting the thermoplastic resin layer A layer and the thermoplastic resin layer B layer, resin 4 and resin 8 were used in order, respectively. In addition, a feed block with 301 slits and a temperature adjustment of 270°C was used to merge them, forming a 301-layer laminated body with a thickness ratio A / B showing 0.86, which was stacked in an alternating regular arrangement along the thickness direction, and the two surface layers became the A layer. Here, the slit length and width in the feed block are designed in a manner that the layer thickness increases monotonically from the outermost surface of one side toward the outermost surface of the opposite side, except for the two outermost layers. The film-making conditions other than these were changed as described in Table 1-1, and the laminated film was obtained by operating in the same manner as in Example 1. The evaluation results of the obtained laminated film are shown in Table 1-2.

[0306] (Example 33, Comparative Example 5)

[0307] The laminated film described in Example 21 and the laminated film described in Comparative Example 4 were bonded with an optical adhesive film TD06-A25 manufactured by Tomogawa Paper Co., Ltd. to form laminated films with adhesive layers. The laminated film with an adhesive layer was bonded to the inner surface of a lampshade of Standlight B096K1YZB9 manufactured by GOLWIS without wrinkles, and lighting devices for evaluation were prepared respectively. The light source used was an LED lamp LDA3N-G-3T3 with a color temperature of 5000K (day white) manufactured by Iris Oyama. The illumination of the lamps before and after the laminated film was measured with a spectral radiometer CL-500A manufactured by Conika Minolta at a distance of 1m from the lamp, and the illumination was read. Compared with the case where the laminated film of Comparative Example 4 was used (Comparative Example 5), the illuminance was improved by 10% by using the laminated film of Example 21 (Example 31), and the illuminance improvement effect due to the increase in reflectivity was confirmed.

[0308] [Table 1-1]

[0309]

[0310] [Table 1-2]

[0311]

[0312] In the table, the bending rigidity is represented by E. For example, 1.3E-07 in Example 1 means 1.3×10 -7 The same explanation applies to other embodiments and comparative examples in the following Tables 1-2, 2-2, and 3-2.

[0313] [Table 2-1]

[0314]

[0315] [Table 2-2]

[0316]

[0317] [Table 3-1]

[0318]

[0319] [Table 3-2]

[0320]

[0321] Industrial Availability

[0322] The laminated film of the present invention has a regular arrangement of three different thermoplastic resin layers, so that the third thermoplastic resin layer, which plays the role of a buffer layer, can laminate thermoplastic resin layers with completely different skeleton structures, such that the refractive index difference becomes large, without interlayer delamination. Therefore, compared with the prior art that can only laminate thermoplastic resins with the same skeleton structure, it can be expected to expand the scope of new functional addition beyond the limitation of the trade-off between optical characteristics of high reflectivity / broadband and interlayer delamination. Furthermore, by making interlayer delamination less likely to occur, an optical film suitable for long-term practical use can be obtained, and it can be used for a long time in applications such as decorative molding films for automobiles, home appliances, etc., optical films for displays, etc., without damaging the original optical characteristics.

[0323] Explanation of symbols

[0324] 1: Spectrum showing the relationship between depth in the thickness direction and contrast (grayscale) change of a laminated film with ABCB regular arrangement

[0325] 2: Layer thickness of layer A

[0326] 3: Layer thickness of B layer

[0327] 4: Layer thickness of C layer

[0328] 5: Layer thickness of the interfacial layer of the laminated film with AB alternating stacking arrangement

[0329] 6: Reflection spectroscopy

[0330] 7: Reflection band Π

[0331] 8: Wavelength bandwidth λ of reflection band Π

[0332] 9: Maximum reflectivity of reflection band Π

[0333] 10: Average reflectivity R of reflection band Π

[0334] 11: Loss tangent tanδ spectrum in dynamic viscoelasticity measurement

[0335] 12: Peak P generated on the lowest temperature side L

[0336] 13: Peak P generated on the highest temperature side H

[0337] 14: Baseline on the low temperature side

[0338] 15: Baseline on the high temperature side

[0339] 16: indicates P L The temperature T of the low temperature side is the midpoint between the peak value and the low temperature side baseline L

[0340] 17: indicates P H The temperature T of the high temperature side is the midpoint between the peak value and the high temperature side baseline H

[0341] 18: Light source unit

[0342] 19: Center of light source unit

[0343] 20: A point on a straight line that passes through the center of the light source unit and is parallel to the long side of the light source unit and is located halfway between the end and the center of the light source unit

[0344] 21: A point on a straight line that passes through the center of the light source unit and is parallel to the short side of the light source unit and is located halfway between the end and the center of the light source unit.

Claims

1. A laminated film, characterized in that: The invention has three or more layers of three different thermoplastic resins arranged in a regular pattern and satisfies the following conditions X and Y at the same time. Condition X: When three different thermoplastic resin layers are set as A layer, B layer, and C layer, a thickness ratio A / B of the A layer to the B layer in the regular arrangement is 0.60 or more and 5.00 or less, and a thickness ratio C / B of the C layer to the B layer in the regular arrangement is 0.70 or more and 5.00 or less; Condition Y: The maximum reflectance at a wavelength of 400 to 800 nm is 35% or more and 100% or less.

2. A laminated film, characterized in that: A regular arrangement having three or more layers of three thermoplastic resins having different refractive indices, wherein when the three thermoplastic resin layers are arranged as layer a, layer b, and layer c in descending order of refractive index, the thickness ratio a / b of the layer a to the layer b and the thickness ratio c / b of the layer c to the layer b in the regular arrangement are greater than 1.40 in more than 90% of the cases, and, in the wavelength range of 300 to 2600 nm, there is a reflection band which continuously shows a reflectivity of greater than 20% in a range of more than 100 nm.

3. A laminated film, characterized in that: A regularly arranged layer having three or more layers of three different thermoplastic resins, and having a reflection band that continuously shows a reflectivity of 75% or more over a range of more than 100 nm in the wavelength range of 400 to 800 nm, wherein more than 30% and less than 80% of the total number of layers of the regularly arranged thermoplastic resin layers are thermoplastic resin layers with a layer thickness of more than 1 nm and less than 25 nm.

4. The laminated film according to claim 1, characterized in that A thickness ratio A / C of the A layer to the C layer in the regular array is greater than or equal to 0.70 and less than or equal to 1.

40. The laminated film according to claim 2 , wherein the layer b exists every other layer in the thickness direction.

6. The laminated film according to claim 1 or 4, characterized in that: The dielectric constant at a loss energy of 2.5 eV obtained by electron energy loss spectroscopy (EELS) measurement is larger in the order of the A layer, the B layer, and the C layer.

7. The laminated film according to claim 3, characterized in that: When the three thermoplastic resin layers are configured as an α layer, a β layer, and a γ layer, the dielectric constant at a loss energy of 2.5 eV obtained by electron energy loss spectroscopy (EELS) measurement is large in descending order of the α layer, the β layer, and the γ layer.

8. The laminated film according to claim 3 or 7, characterized in that: In the regular arrangement, 90% or more of the regular arrangement exists in which the thickness ratio α / β of the α layer to the β layer and the thickness ratio γ / β of the γ layer to the β layer are 1.40 or more.

9. The laminated film according to any one of claims 1 to 8, characterized in that The peeling rate of the cross-cut in the adhesion test based on the cross-cut method specified in JIS K 5600-5-6:1999 is 10% or less.

10. The laminated film according to any one of claims 1 to 9, characterized in that The average reflectivity at a wavelength of 400 nm to 800 nm is 50% or more and 100% or less.

11. The laminated film according to any one of claims 1 to 10, characterized in that Let the reflection bandwidth of the widest reflection band Π in which the reflectivity continuously shows more than 20% in a range of more than 100 nm within the wavelength range of 300 to 2600 nm be λ, let the average reflectivity in the reflection band be R, and when the film thickness is t, (λ·R) / t is greater than 820 and less than 1400, the unit of λ is nm, the unit of R is %, and the unit of t is μm.

12. The laminated film according to any one of claims 1, 4, 6, 9 to 11, characterized in that The regular arrangement is an arrangement in which the A layer, the B layer, the C layer, and the B layer exist in sequence.

13. The laminated film according to any one of claims 1, 2, 4 to 6, and 9 to 12, characterized in that: 30% or more and 80% or less of the total number of layers constituting the regularly arranged thermoplastic resin layers are thermoplastic resin layers having a layer thickness of 1 nm or more and 25 nm or less.

14. The laminated film according to any one of claims 1 to 13, characterized in that The dielectric constant ratio of the thermoplastic resin layer having the highest refractive index to the thermoplastic resin layer having the lowest refractive index at a loss energy of 2.5 eV obtained by electron energy loss spectroscopy (EELS) measurement is 1.10 or more and 1.60 or less.

15. The laminated film according to any one of claims 1 to 14, characterized in that The transmission lightness L*SCE (D65) is 0.1% or more and 30% or less.

16. The laminated film according to any one of claims 1 to 15, characterized in that The thickness of each layer included in the regular arrangement shows a distribution that increases monotonically from one surface toward the opposite surface.

17. The laminated film according to any one of claims 1 to 16, characterized in that At least one of the three different thermoplastic resin layers is a thermoplastic resin layer showing crystallinity.

18. The laminated film according to claim 17, characterized in that The thermoplastic resin as a main component of the thermoplastic resin layer showing crystallinity is polyethylene terephthalate or polyethylene naphthalate.

19. The laminated film according to any one of claims 1 to 18, characterized in that The three different thermoplastic resin layers are a combination of thermoplastic resin layers showing crystalline / semi-crystalline / amorphous properties, or crystalline / amorphous / amorphous properties.

20. The laminated film according to claim 19, characterized in that The amorphous thermoplastic resin layer contains, as a main component, any one of acrylic resin and polyester having an alicyclic structure.

21. The laminated film according to any one of claims 1 to 20, characterized in that The bending stiffness is 0.5×10 -7 [N·m 2 ] and above and 5.2×10 -7 [N·m 2 ]the following.

22. The laminated film according to any one of claims 1 to 21, characterized in that In the measurement of dynamic viscoelasticity tanδ at 0°C or higher and 180°C or lower, the peak generated on the highest temperature side is defined as P H , the peak generated on the lowest temperature side is set as P L , will represent the P H The temperature on the high temperature side, which is the midpoint between the peak value and the high temperature side baseline, is set as T H , will represent the P L The low temperature side temperature of the midpoint between the peak value and the low temperature side baseline is set as T L When T H -T L is 60 or more and 120 or less, the T H and T L The unit is ℃.

23. A vehicle-mounted component, characterized in that: A laminated film comprising a protective layer, a printing layer, an adhesive layer, and the laminated film according to any one of claims 1 to 22.

24. The vehicle-mounted component according to claim 23, characterized in that: The thickness of the laminated film is greater than or equal to 20 μm and less than or equal to 200 μm, and the thickness of the protective layer is greater than or equal to 200 μm and less than or equal to 1 cm.

25. The vehicle-mounted component according to claim 23 or 24, characterized in that: The thickness ratio of the thickest portion to the thinnest portion of the laminated film is 1.2 times or more and 2.5 times or less.

26. The vehicle-mounted component according to any one of claims 23 to 25, characterized in that: A light shielding region having a light transmittance of 20% or less is provided.

27. The vehicle-mounted component according to any one of claims 23 to 26, characterized in that: It has a light-transmitting area with a light transmittance of 80% or more.

28. A vehicle, characterized in that: A vehicle-mounted component according to any one of claims 23 to 27, and a millimeter wave radar showing a peak intensity at any frequency of 22 GHz to 26 GHz, 58 GHz to 62 GHz, and 76 GHz to 80 GHz.

29. A vehicle, characterized in that: A radome that transmits infrared rays is provided, wherein the radome includes the vehicle-mounted component according to any one of claims 23 to 27.

30. An image display device, characterized in that: The invention comprises a screen protection layer, a light source, a transistor, and the laminated film according to any one of claims 1 to 22.

31. The image display device according to claim 30, characterized in that: The display area is a shape other than a rectangle.

32. A lighting device, characterized in that: The laminated film according to any one of claims 1 to 22 is provided on the back side of the light source.

33. The lighting device according to claim 32, characterized in that: The laminated film has a three-dimensional shape.

34. A solar cell module, characterized in that: The laminated film according to any one of claims 1 to 22 is used.

Citation Information

Patent Citations

  • Infrared reflective laminate

    CN101896339A

  • Layered film

    CN108136745A

  • Multilayer laminated film

    CN111741845A

  • Laminated film

    JP2004314570A

  • Laminated polyester film

    JP2006327157A