Metal organic structure

By designing a metal-organic structure with a cyclic or cage-like structure and utilizing the bonding of alkali metal ions and cyclodextrin-based organic ligands, the problem of insufficient gas adsorption capacity in the existing technology has been solved, and the adsorption of nitrogen, CO2 and Efficient adsorption of monocyclic compounds.

CN118765288APending Publication Date: 2024-10-11TOYO SEIKAN GRP HLDG LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023693.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-26
Filing Date
2023-02-15
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing metal-organic structures have deficiencies in gas adsorption capacity and are difficult to effectively adsorb substances other than organic gases such as butane and carbon dioxide.

Method used

By designing metal-organic structures with cyclic or cage structures, and utilizing the bonding of alkali metal ions such as potassium ions with cyclodextrin-based organic ligands, materials with excellent adsorption properties are formed. The specific process includes the preparation of materials containing metal ions and An aqueous solution of organic ligands, to which an organic solvent is added to form a metal-organic structure.

Benefits of technology

It achieves efficient adsorption of nitrogen and carbon dioxide gas. The nitrogen adsorption capacity reaches more than 220cm3/g, and the CO2 gas adsorption capacity reaches more than 10cm3/g. It can also adsorb monocyclic compounds such as cyclopentane, etc., which significantly improves the gas adsorption performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005010165680000181
    Figure BDA0005010165680000181
Patent Text Reader

Abstract

The purpose of the present invention is to provide a metal organic structure having excellent gas adsorption ability. The present invention provides a metal-organic structure which is provided with a metal ion and an organic ligand coordinated to the metal ion, has a ring structure or a cage structure, and has the metal ion bonded in an amount of 7.40 mol or less per 1 mol of the organic ligand.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a metal organic structure. Background Art

[0002] Metal-organic frameworks (MOFs) are materials formed by the coordination bonding of metals and organic ligands. As such metal-organic frameworks, porous materials with a ring structure that can adsorb guest molecules are known. Compared with porous materials such as zeolites and activated carbon, such metal-organic frameworks have advantages such as easy control of pore size, and are expected to be put into practical use in various applications such as gas adsorbents.

[0003] Regarding metal organic structures having a ring structure, a method for producing a metal organic structure using γ-cyclodextrin is disclosed in non-patent document 1 (Yaghi, OM, Angew. Chem. Int. Ed. Engl. 2010, 49, 8630-8634). Non-patent document 1 records the following content: 1.0 equivalent of γ-cyclodextrin and 8 equivalents of KOH are mixed in an aqueous solution, and then methanol is subjected to "vapor diffusion" (vapor diffusion) of the aqueous solution for 2 to 7 days to obtain a metal organic structure.

[0004] In addition, Patent Document 1 (Japanese Patent Application Laid-Open No. 2021-54490) proposes a gas absorption film comprising a thermoplastic resin and a gas absorbent, wherein the gas absorbent includes a gas physical absorbent and / or a gas chemical absorbent, and the gas physical absorbent has a BET specific surface area of ​​50 m 2 / g~4000m 2 / g, the content of the gas absorbent in the layer containing the gas absorbent is 0.5 mass % to 30 mass %, and it is described that a metal organic structure can be used as one of the gas physical absorbents in the gas absorption film.

[0005] Patent Document 1 describes that organic gases such as butane, carbon dioxide, aldehydes, and acetic acid can be adsorbed using a specific metal organic structure such as 2-methylimidazole zinc.

[0006] The pore size and structure shape of the metal-organic structure vary depending on the type, combination, or mixing ratio of the metal ions and organic ligands that constitute it, and the substances that can be adsorbed are also different. Therefore, it is expected to use new adsorbents with metal-organic structures that can adsorb substances other than the above-mentioned organic gases.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2021-54490

[0010] Non-patent literature

[0011] Non-patent document 1: Yaghi, OM, Angew. Chem. Int. Ed. Engl. 2010, 49, 8630-8634 Summary of the invention

[0012] As a metal organic structure, it is advantageous to obtain a substance having a better adsorption capacity. Therefore, an object of the present invention is to provide a metal organic structure having a better adsorption capacity.

[0013] The present inventors have conducted intensive studies and have found that the above-mentioned problems can be solved by the following means.

[0014] [1] A metal-organic structure comprising a metal and an organic ligand coordinated to the metal, the metal-organic structure having a ring structure or a cage structure, wherein the metal ion is bonded in an amount of 7.40 mol or less per mol of the organic ligand.

[0015] [2] The metal-organic structure according to [1], wherein the nitrogen adsorption capacity is 220 cm 3 / g or above.

[0016] [3] The metal-organic structure according to [1] or [2], wherein CO 2 Gas adsorption capacity is 10cm 3 / g or above.

[0017] [4] The organometallic structure according to any one of [1] to [3], wherein the metal is an alkali metal.

[0018] [5] The organometallic structure according to [4], wherein the alkali metal is potassium.

[0019] [6] The organometallic structure according to any one of [1] to [5], wherein the organic ligand is cyclodextrin.

[0020] [7] The organometallic structure according to [6], wherein the cyclodextrin is γ-cyclodextrin.

[0021] [8] A gas adsorbent comprising the organometallic structure according to any one of [1] to [7].

[0022] [9] An adsorbent characterized in that it can adsorb at least monocyclic compounds, the adsorbent containing a metal organic structure, the metal organic structure having a ring structure or a cage structure and composed of at least one organic ligand coordinated to at least one metal ion, the organic ligand being a cyclic organic compound.

[0023]

[10] The adsorbent according to [9], wherein the metal ions are alkali metal ions.

[0024]

[11] The adsorbent according to

[10] , wherein the alkali metal is potassium.

[0025]

[12] The adsorbent according to any one of [9] to

[12] , wherein the cyclic organic compound is a cyclodextrin compound.

[0026]

[13] The adsorbent according to

[12] , wherein the cyclodextrin compound is α-cyclodextrin or γ-cyclodextrin.

[0027]

[14] The adsorbent according to any one of [9] to

[14] , wherein, in the metal-organic structure, the organic ligand is cyclodextrin, and the metal ion is a potassium ion.

[0028]

[15] The adsorbent according to any one of [9] to

[14] , wherein the metal organic structure has a two-dimensional sheet-like layer structure.

[0029]

[16] The adsorbent according to any one of [9] to

[15] , wherein the monocyclic compound is a cyclopentane derivative.

[0030]

[17] The adsorbent according to any one of [9] to

[16] , wherein the metal ion is bonded in an amount of 7.40 mol or less per mol of the organic ligand.

[0031]

[18] A resin composition, characterized in that the adsorbent according to any one of [9] to

[17] is contained in the resin.

[0032]

[19] A method for producing a metal organic structure having a ring structure, comprising: a step of preparing an aqueous solution containing a metal ion and an organic ligand that can coordinate to the metal ion as a first solution; and a step of directly adding a second solution containing an organic solvent to the first solution to generate a metal organic structure in which the organic ligand is coordinated to the metal ion.

[0033]

[20] The production method according to

[19] , wherein the metal ion is bonded in an amount of 7.40 mol or less per mol of the organic ligand.

[0034]

[21] The production method according to

[19] or

[20] , wherein the metal ion is an alkali metal ion.

[0035]

[22] The production method according to

[21] , wherein the metal ion is a potassium ion.

[0036]

[23] The production method according to any one of

[19] to

[22] , wherein the organic ligand comprises a cyclodextrin compound.

[0037]

[24] The production method according to

[23] , wherein the cyclodextrin compound contains γ-cyclodextrin.

[0038]

[25] The production method according to any one of

[19] to

[24] , wherein the metal ion is a zinc ion and the organic ligand is a compound having an imidazole skeleton.

[0039]

[26] The production method according to

[25] , wherein the compound having an imidazole skeleton is 2-methylimidazole.

[0040]

[27] The production method according to any one of

[19] to

[26] , wherein the metal ion is an iron ion, and the organic ligand is a compound having a monocyclic or polycyclic skeleton.

[0041]

[28] The production method according to

[27] , wherein the compound having a monocyclic or polycyclic skeleton is trimesic acid.

[0042]

[29] The production method according to claim 19, wherein the organic ligand is used in an amount of 0.05 to 50 mol per 1 mol of the metal ion in the first solution.

[0043]

[30] The production method according to any one of

[19] to

[29] , wherein the second solution is a solution that changes the pH of the first solution.

[0044]

[31] The production method according to

[30] , wherein the second solution is a solution for lowering the pH of the first solution, and the second solution is added in an amount to lower the pH of the first solution by 0.01 to 0.20.

[0045]

[32] The production method according to any one of

[19] to

[31] , wherein the second solution contains at least one solvent selected from an alcohol solvent, a ketone solvent, and an aprotic solvent.

[0046]

[33] The production method according to any one of

[19] to

[32] , wherein, in the step of generating the metal organic structure, the second solution is added to the first solution while the first solution is sheared.

[0047]

[34] The production method according to any one of

[19] to

[33] , further comprising a step of separating the metal-organic structure after the step of generating the metal-organic structure.

[0048]

[35] The production method according to

[34] , wherein the separation step includes a step of filtering the mixed solution of the first solution and the second solution.

[0049]

[36] The production method according to

[35] , wherein the separation step includes a step of washing or drying the metal organic structure after the filtering step.

[0050] According to the present invention, a metal-organic structure having excellent gas adsorption capacity is provided. DETAILED DESCRIPTION

[0051] Hereinafter, embodiments of the present invention will be described.

[0052] 1: Metal-organic structures

[0053] The metal organic structure of the present embodiment is a structure containing a metal ion and an organic ligand coordinated to the metal ion. The metal organic structure has a ring structure or a cage structure. In addition, the metal ion is bonded in an amount of 7.40 moles or less relative to 1 mole of the organic ligand. According to the view of the inventors, a metal organic structure with excellent adsorption capacity is obtained by having such a structure.

[0054] Specifically, the "ring structure or cage structure" refers to a ring structure or cage structure having a space capable of enclosing a guest molecule. By having such a structure, the guest molecule can be adsorbed on the metal organic structure.

[0055] The ring structure is preferably a structure formed by bonding a metal ion and an organic ligand.

[0056] The cage structure refers to a cubic crystal structure obtained by further crystallization of a metal organic structure having a ring structure formed by bonding metal ions and organic ligands.

[0057] The presence of the ring structure or the cage structure can give the metal organic structure the function of adsorbing guest molecules. Utilizing this function, the metal organic structure can be used for applications that require the function of adsorbing substances (such as gas adsorbents).

[0058] The number of moles of the metal ion per 1 mol of the organic ligand may be 7.40 mol or less, and is preferably 3.50 to 7.40 mol, more preferably 5.00 to 7.35 mol, and even more preferably 6.00 to 7.30 mol.

[0059] The metal ion can be used as long as it can form a coordination bond with the organic ligand. As the metal ion, for example, at least one metal ion selected from Li, Na, K, Rb, Be, Mg, Ca, Sr, Ba, Sc, Y, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Re, Fe, Ru, Os, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zn, Cd, Hg, Al, Ga, In, Tl, Si, Ge, Sn, Pb, As, Sb and Bi can be cited. Among them, alkali metal ions, Zn ions and Fe ions are preferred. As alkali metal ions, potassium ions and sodium ions are more preferred. As alkali metal ions, potassium ions are most preferred.

[0060] As the organic ligand, any ligand that forms a coordination bond with the metal ion can be used. As the organic ligand, a compound having a functional group that forms a coordination bond with the metal ion can be used. As such a functional group, for example, a hydroxyl, an imidazole radical, a pyridyl radical, a carboxyl group, a sulfonic acid group, and an amide group can be cited.

[0061] In one embodiment, as an organic ligand, a compound having a structure that can enclose a guest molecule can be used. Examples of such compounds include cyclodextrin compounds and crown ethers. In addition, crown ethers are cyclic oligomers of ethylene glycol containing carbon, hydrogen, and oxygen, and oxygen atoms are respectively bonded to two carbon atoms to form a crown ring. As organic ligands, cyclodextrin compounds are preferred, and examples include α-cyclodextrin, β-cyclodextrin, and γ-cyclodextrin. When γ-cyclodextrin is used, nitrogen adsorption and carbon dioxide (CO 2 ) absorption can be achieved. 2 ) A metal organic structure having excellent gas adsorption. In addition, the metal organic structure using α-cyclodextrin as an organic ligand has a two-dimensional sheet-like layered structure. The results of the examples described below also show that the metal organic structure using γ-cyclodextrin as an organic ligand in a cage-like structure also has adsorption properties for heptane, octane, etc., which cannot be adsorbed except for monocyclic compounds.

[0062] The metal organic structure used in the present invention has an organic ligand of a cyclodextrin compound. When the metal ion is a potassium ion, the metal organic structure is preferably a metal organic structure in which the cyclodextrin compound is bonded to 1 mole of potassium ion in a range of 0.05 to 0.8 moles in order to exhibit excellent adsorption performance.

[0063] That is, the results of the examples described later also show that, between the adsorbent using γ-CD-MOF in which 0.125 mol of γ-cyclodextrin and 1 mol of potassium ions are mixed (Example 1) and the adsorbent using γ-cyclodextrin (Comparative Example 2), the adsorption performance of the adsorbent of Example 1 is significantly improved.

[0064] On the other hand, the organic ligand does not necessarily need to have the function of encapsulating guest molecules. It is sufficient that the organic ligand has the function of encapsulating guest molecules as a whole metal organic structure. As such organic ligands, for example, compounds having an imidazole skeleton (for example, imidazole, 2-methylimidazole, 2-formylimidazole, etc.), compounds having a monocyclic or polycyclic skeleton (for example, terephthalic acid, trimesic acid, etc.), etc. can be cited.

[0065] According to this embodiment, a metal organic structure having excellent adsorption of guest molecules can be realized. According to this embodiment, a nitrogen adsorption amount of, for example, 220 cm 3 / g or more metal organic structure. Such a metal organic structure is useful as an adsorbent for adsorbing nitrogen. In a preferred embodiment, a nitrogen adsorption capacity of 250cm 3 In a further preferred embodiment, the nitrogen adsorption capacity can reach 280 cm 3 The nitrogen adsorption amount can be measured by the method described in the examples described later.

[0066] In addition, according to this embodiment, CO 2 The gas adsorption capacity is, for example, 10 cm 3 / g or more metal organic structure. Such a metal organic structure is used for adsorbing CO 2 Gas adsorbents are useful. In a preferred embodiment, CO 2 Gas adsorption capacity is 20cm 3 / g or more metal organic structure. In a further preferred embodiment, CO 2 Gas adsorption capacity is 40cm 3 / g or more metal organic structure. 2 The gas adsorption amount can be measured by the method described in Examples below.

[0067] The pore size of the metal-organic structure is related to CO 2 The molecular diameter of the gas is more than the same as that of CO 2In addition, especially when polar groups such as hydroxyl, carboxyl, and amino groups exist in the organic ligands constituting the metal organic structure, the interaction between the pore wall of the metal organic structure and carbon dioxide occurs, and CO 2 The gas adsorption performance is improved. For example, when cyclodextrin is used as an organic ligand, the primary alcohol of glucose constituting cyclodextrin reacts with CO 2 Gas interaction, adsorption of CO in the form of carboxylic acids 2 gas. Therefore, CO 2 The maximum gas adsorption amount depends on the pore specific surface area of ​​the metal organic structure and / or the amount of free polar groups that do not participate in the structural composition of the organic ligands constituting the metal organic structure.

[0068] The pore specific surface area of ​​the metal organic structure is, for example, 700 to 1400 m 2 / g, preferably 800 to 1300 m 2 / g, more preferably 900 to 1200 m 2 The pore specific surface area can be measured by the method described in the examples described later.

[0069] The pore volume of the metal organic structure is, for example, 0.300 to 0.600 cm 3 / g, preferably 0.350 to 0.500 cm 3 The pore volume can be measured by the method described in the examples described later.

[0070] The pore diameter of the metal organic structure is, for example, 1.300 to 1.600 nm, and preferably 1.400 to 1.500 nm. The pore diameter can be measured by the method described in Examples below.

[0071] 2: Methods for manufacturing metal-organic structures

[0072] The metal organic structure having the above-described structure can be produced, for example, by using a specific production method described below.

[0073] That is, the manufacturing method of this embodiment includes: a step of preparing an aqueous solution containing metal ions and an organic ligand that can be coordinated to the above-mentioned metal ions as a first solution (step S1), and a step of directly adding a second solution containing an organic solvent to the first solution to generate a metal organic structure in which the organic ligand is coordinated to the metal ions (step S2). Below, each step is described in detail.

[0074] (Step S1: Preparation of the first solution)

[0075] First, as the first solution, an aqueous solution containing metal ions and organic ligands is prepared. Specifically, a metal compound and an organic ligand are added to water and dissolved. Thus, the first solution can be obtained. The first solution can be prepared at room temperature (1 to 30° C.).

[0076] The metal compound used as the metal ion supply source is not particularly limited, and for example, inorganic halide salts such as metal hydroxides and chloride salts, and inorganic acid salts such as nitrates and acetates can be used.

[0077] When the metal ion is an alkali metal ion, it is preferable to use an alkali metal hydroxide as the metal compound.

[0078] When the metal ion is a Zn ion or a Fe ion, it is preferable to use an inorganic acid salt as the metal compound.

[0079] The pH of the first solution may be any pH at which the metal in the metal compound exists in the form of ions.

[0080] For example, when an alkali metal ion is used as the metal ion, the first solution is alkaline. In this case, the pH of the first solution is, for example, 8 or more, preferably 10 to 14, and more preferably 13 to 14.

[0081] When Zn is used as the metal ion, the appropriate pH depends on the type of zinc compound as the ion supply source, and when zinc acetate is used as the supply source, the appropriate pH is, for example, 6 to 13, preferably 7 to 12, and more preferably 9 to 10.

[0082] When Fe ions are used as metal ions, the appropriate pH also depends on the type of iron compound as the ion supply source. When iron (III) nitrate is used, the appropriate pH is, for example, 1 to 6, preferably 1 to 4, and more preferably 2 to 3.

[0083] In the first solution, the amount of the organic ligand is, for example, 0.05 to 50 mol, preferably 0.1 to 40 mol, and more preferably 0.125 to 30 mol, relative to 1 mol of the metal ion.

[0084] When the metal ion is an alkali metal ion, the amount of the organic ligand is preferably 0.05 to 8 mol, more preferably 0.125 to 8 mol, and even more preferably 0.125 to 0.8 mol, based on 1 mol of the metal ion.

[0085] When the metal ion is a potassium ion and the organic ligand is a cyclodextrin compound, as described above, it is preferably in the range of 0.05 to 0.8, particularly when the organic ligand is α-cyclodextrin, it is preferably in the range of 0.125 to 0.375, and when the organic ligand is γ-cyclodextrin, it is preferably in the range of 0.125 to 0.750.

[0086] When the metal ion is a Zn ion, the amount of the organic ligand is preferably 0.5 to 50 mol, more preferably 15 to 40 mol, based on 1 mol of the metal ion.

[0087] When the metal ion is an Fe ion, the amount of the organic ligand is preferably 0.05 to 5 mol, more preferably 0.1 to 1 mol, based on 1 mol of the metal ion.

[0088] When the content is within the above range, a metal organic structure having excellent adsorption properties for guest molecules such as nitrogen can be obtained.

[0089] The amount of water is, for example, 10 to 5000 mol, or preferably 50 to 5000 mol, relative to 1 mol of the metal ions.

[0090] When an alkali metal ion is used as the metal ion, the amount of water is preferably 50 to 200 mol, more preferably 80 to 200 mol, and further preferably 100 to 150 mol, based on 1 mol of the metal ion.

[0091] When Zn ions are used as metal ions, the amount of water is preferably 500 to 5000 mol, more preferably 1000 to 3500 mol, based on 1 mol of the metal ions.

[0092] When Fe ions are used as metal ions, the amount of water is preferably 200 to 3000 mol, more preferably 500 to 2000 mol, based on 1 mol of the metal ions.

[0093] The molar ratio of the organic ligand to water (organic ligand: water) is, for example, 1:10 to 1:2000, preferably 1:50 to 1:2000, more preferably 1:50 to 1:1500, further preferably 1:80 to 1:1500, and most preferably 1:100 to 1:1300. When the organic ligand is a cyclodextrin compound, the molar ratio is preferably in the range of 1:100 to 1:1300.

[0094] (Step S2: Addition of the Second Solution)

[0095] Next, the second solution is added directly to the first solution. Here, "directly" adding means that the second solution is added to the first solution while being kept in a liquid state.

[0096] The second solution contains an organic solvent. The second solution is preferably a solution that changes the pH of the first solution.

[0097] More preferably, the second solution is a solution that lowers the pH of the first solution.

[0098] As such an organic solvent, there can be mentioned a solvent that deprotonates the coordination bonding site in the organic ligand. As an organic solvent, for example, there can be mentioned at least one solvent selected from alcoholic solvents, ketone solvents and aprotic solvents. By adding such an organic solvent, the organic ligand is deprotonated, and as a result, a coordination bond is formed between the metal ion and the organic ligand, thereby forming a metal organic structure.

[0099] In this case, the second solution is preferably added in such an amount that the pH of the first solution is reduced by, for example, 0.01 to 0.20, preferably 0.05 to 0.15.

[0100] Examples of the alcohol solvent include methanol, ethanol, 1-propanol, and 1-butanol.

[0101] Examples of the ketone solvent include acetone and the like.

[0102] Examples of the aprotic solvent include N,N-dimethylformamide and the like.

[0103] A preferred organic solvent is an alcohol solvent, and methanol is more preferred.

[0104] The second solution is preferably added to the first solution while applying shear to the first solution. More preferably, the second solution is added to the first solution while stirring the first solution. The second solution may be added to the first solution at room temperature.

[0105] The second solution is preferably added to the first solution over, for example, 1 to 20 minutes, preferably 10 to 15 minutes.

[0106] If the second solution is added all at once, it may become cloudy and the desired metal structure organism may not be obtained. In contrast, by adding over 1 to 20 minutes, crystal nuclei can be formed to grow a crystal structure, and the desired metal structure organism can be easily obtained.

[0107] Examples of the method for adding the second solution include a method of adding at a constant speed using a dropping funnel, a method of adding a constant amount at a constant time interval, and a method of adding while gradually changing the amount added.

[0108] After the second solution is added, the mixed solution of the first solution and the second solution is preferably further stirred. After the second solution is added, the mixed solution is stirred at room temperature for, for example, 5 to 50 hours, preferably 10 to 30 hours. If stirring is not performed, a two-layer separation state with a turbid lower layer and a transparent upper layer may be formed, and the two-layer separation state may not be eliminated.

[0109] The amount of the organic solvent added is, for example, 3 to 1000 mol, or preferably 5 to 500 mol, relative to 1 mol of the metal ions.

[0110] When the metal ion is an alkali metal ion and the organic ligand is γ-cyclodextrin, the amount of the organic solvent added is preferably 3 to 100 mol, preferably 5 to 50 mol, and more preferably 10 to 30 mol per 1 mol of the metal ion.

[0111] When the metal ion is a potassium ion and the organic ligand is α-cyclodextrin, the organic solvent is preferably added in an amount in the range of 10 to 400 mol, preferably 50 to 300 mol, and more preferably 100 to 200 mol, relative to 1 mol of the potassium ion. When the organic ligand is γ-cyclodextrin, the organic solvent is preferably added in an amount in the range of 3 to 100 mol, preferably 5 to 50 mol, and more preferably 10 to 30 mol, relative to 1 mol of the potassium ion.

[0112] When the metal ion is a Zn ion, the amount of the organic solvent added is preferably 50 to 500 mol, more preferably 75 to 200 mol, based on 1 mol of the metal ion.

[0113] When the metal ion is an Fe ion, the amount of the organic solvent added is preferably 100 to 800 mol, more preferably 250 to 500 mol, based on 1 mol of the metal ion.

[0114] The metal organic structure can be generated by the method described above. The metal organic structure is generated in the form of a solid product. Therefore, the metal organic structure can be separated by filtering the mixed solution, for example. After filtering, the separated metal organic structure can be further washed with an organic solvent such as methanol. In addition, the separated metal organic structure can also be dried.

[0115] According to the method of the present embodiment described above, a metal organic structure having excellent adsorption properties for guest molecules can be synthesized in a short time.

[0116] (Adsorbent)

[0117] The adsorbent of the present invention contains a metal organic structure having a ring structure or a cage structure, wherein the metal organic structure is composed of at least one organic ligand coordinated to at least one metal ion and the organic ligand is a cyclic organic compound, thereby providing an adsorbent having excellent adsorption performance.

[0118] The adsorbent of the present invention can efficiently adsorb monocyclic compounds, especially cyclopentane derivatives.

[0119] Furthermore, the adsorbent of the present invention can exhibit excellent adsorption performance even when blended with a resin.

[0120] The metal organic structure constituting the adsorbent of the present invention has a ring-shaped or cage-shaped porous crystal structure formed by at least one organic ligand coordinated to at least one metal ion. Since the spatial structure inside the crystal is uniform, it can efficiently enclose guest molecules and can show excellent performance as an adsorbent.

[0121] In addition, among the metal organic structures used in the present invention, metal organic structures using cyclic organic compounds as organic ligands are also important. That is, the metal organic structures used in the present invention do not use cyclic organic compounds such as aromatic organic compounds and heterocyclic organic compounds as organic ligands like the metal organic structures used in the above-mentioned Patent Document 1, but refer to organic compounds having a cyclic structure such as cyclodextrin compounds. Since cyclodextrin compounds have a structure that can enclose guest molecules, the adsorption performance can be further improved, and since they are compounds of natural origin, they are also excellent in environmental friendliness.

[0122] The adsorbent of the present invention can be used alone as an adsorbent as long as it contains at least the metal organic structure of the ring structure or cage structure, but it does not exclude the inclusion of other components. For example, it can also contain other well-known metal organic structures, zeolite and other porous substances together with the metal organic structure as needed.

[0123] The adsorbent may be in the form of a powder, granule, or pellet of the metal organic structure described above, or may be formed into a pellet, fiber, film, or thin film in the form of a resin composition as described below.

[0124] The adsorbent of the present invention can be used by known methods, and can be directly added to a target substance, molded into granules or pellets and packed in a column, or molded into a membrane or film and used as a filter.

[0125] The adsorbent of the present invention can adsorb at least a monocyclic compound. Examples of such a monocyclic compound include cyclopentane derivatives and cyclohexane derivatives.

[0126] Examples of the cyclopentane derivative include methylcyclopentane, cyclopentene, cyclopentadiene, and cyclopentanol, and examples of the cyclohexane derivative include methylcyclohexane, cyclohexanedicarboxylic acid, and cyclohexanedimethanol.

[0127] In addition, in the case of a metal organic structure composed of potassium ions as metal ions and α-cyclodextrin or γ-cyclodextrin as organic ligands (hereinafter, sometimes referred to as "α-CD-MOF" or "γ-CD-MOF", respectively), in addition to the above-mentioned monocyclic compounds, it is also possible to exhibit adsorption performance for butyraldehyde, ethyl acetate, hexane and its derivatives, formic acid, etc. In addition, in the case of α-CD-MOF, in addition to the above, it is also possible to exhibit adsorption performance for octane and its derivatives, octene and its derivatives, and in the case of γ-CD-MOF, in addition to the above, it is also possible to exhibit adsorption performance for heptene derivatives.

[0128] (Resin composition)

[0129] The resin composition of the present invention contains the above-mentioned adsorbent in a resin.

[0130] As the resin containing the adsorbent, a conventionally known resin can be used, and examples thereof include low-, medium-, and high-density polyethylene, linear low-density polyethylene, linear ultra-low-density polyethylene, isotactic polypropylene, syndiotactic polypropylene, propylene-ethylene copolymer, polybutene-1, ethylene-butene-1 copolymer, propylene-butene-1 copolymer, ethylene-propylene-butene-1 copolymer and other olefin resins, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate and other polyester resins, nylon 6, nylon 6,6, nylon 6,10 and other polyamide resins, polycarbonate resins and other thermoplastic resins, phenolic resins, epoxy resins, polyurethane resins, melamine resins, urea-formaldehyde resins, alkyd resins, unsaturated polyester resins, silicone resins and other thermosetting resins, or photocurable acrylic resins, but are not limited thereto.

[0131] In the resin composition of the present invention, in order for the adsorbent in the resin composition to efficiently exhibit adsorption performance, the resin used as the matrix is ​​preferably a resin having excellent air permeability. Therefore, low-density polyethylene can be particularly preferably used among the above-mentioned resins.

[0132] The content of the adsorbent in the resin composition varies depending on the type of resin, application, etc., and cannot be generalized. It is preferably contained in an amount of 0.01 to 50 parts by mass, particularly 5 to 20 parts by mass, relative to 100 parts by mass of the resin. When the amount of the adsorbent is less than the above range, the desired adsorbability may not be obtained. On the other hand, when the amount of the adsorbent is more than the above range, the moldability when the resin composition is molded into a desired form may be impaired.

[0133] The resin composition may contain a dispersant, an antioxidant, a filler, and conventionally known additives for resins in addition to the above-mentioned adsorbent.

[0134] The preparation of the resin composition can be carried out by a conventionally known method, but is not limited thereto, and examples thereof include a method of dry mixing the adsorbent and the resin, a method of adding the adsorbent to the resin in a molten state and blending them, a method of preparing a dispersion in which the adsorbent is dispersed in an organic solvent and adding the dispersion to the resin in a molten state and melt-kneading the mixture, etc.

[0135] The resin composition of the present invention can be molded into various forms depending on its application, and can be molded into forms such as cups, trays, bottles, and tubes in addition to pellets, films, and sheets.

[0136] Example

[0137] Hereinafter, in order to explain the present invention in more detail, examples performed by the present inventors will be described.

[0138] (Measurement method)

[0139] [Thermogravimetric analysis evaluation]

[0140] The combustion behavior and potassium residue of the metal organic structure were measured by thermogravimetric analysis using TG / DTA7220 manufactured by Hitachi, Ltd. at a heating rate of 3°C / min and a measurement temperature of 30°C to 500°C.

[0141] [Molecular structure evaluation]

[0142] The molecular structure of the combustion residue of the metal organic structure generated by the thermogravimetric analysis was measured by Raman spectroscopy using a DXR Raman Microscope optical system manufactured by Thermo Scientific with a laser wavelength of 532 nm, a laser output of 5.0 mW, an exposure time of 6.00 seconds, and 10 exposure times.

[0143] [Composition molar ratio]

[0144] The above thermogravimetric analysis results show that the combustion residue is potassium bicarbonate, so the amount of potassium in the combustion residue is calculated. Based on the calculated potassium amount, the γ-cyclodextrin in the metal organic structure is calculated, and the molar ratio of γ-cyclodextrin to potassium in the metal organic structure is determined.

[0145] [Specific surface area·Pore volume·Pore diameter·Adsorption amount]

[0146] The nitrogen adsorption isotherm was measured at liquid nitrogen temperature by the multipoint method using BELSORP MAX II manufactured by Microtrac BEL, and the specific surface area, pore volume, pore diameter, and maximum nitrogen adsorption amount of the metal organic structure were calculated by MP calculation.

[0147] In addition, for CO 2 The gas adsorption was measured by the multi-point method at 298 K in the range of 0 to 100 kPa using a BELSORP MAX II manufactured by Microtrac BEL. 2 Gas adsorption isotherm, calculate CO 2 Maximum gas adsorption capacity.

[0148] [Crystal Structure]

[0149] The crystal structure of the obtained metal organic structure was evaluated by powder X-ray diffraction (PXRD) using SmartLab manufactured by Rigaku Corporation.

[0150] [Adsorption test using adsorbent in powder form]

[0151] The adsorption sample was prepared by filling the collection bottle with 0.2g of each adsorbent to collect various odor components. The reduction rate was compared and evaluated using the total area value of TIC (total ion chromatogram) of hydrocarbon compounds, monocyclic compounds, and alcohol compounds detected between retention times of 12.5 minutes and 22.5 minutes by GC / MS (GC-2010 manufactured by Shimadzu Corporation).

[0152] Analysis conditions: column DB-624 (60m×0.25mm×1.4μm); column temperature: initially maintained at 40°C for 10 minutes, then heated at 10°C / min. After reaching the final temperature of 250°C, maintained for 5 minutes; column flow rate: 1.88ml / min; carrier gas: helium; ionization method: EI; ion source temperature: 200°C; detection: MS scan (m / z 26.0-550)

[0153] The adsorbed gas is determined by the spectrum obtained under the above analysis conditions.

[0154] [Adsorption test of resin composition containing adsorbent]

[0155] 2 g of the resin composition was filled into a flask filled with 480 ppm of hexane, 500 ppm of octane or 2 ppm of acetic acid to prepare an adsorption sample. The gas component concentration after 1 hour of filling the adsorption sample was measured using the following detector tube.

[0156] Hexane concentration: Detector tube (GASTEC, No.105)

[0157] Octane concentration: Detector tube (GASTEC, No.105)

[0158] Acetic acid concentration: Detection tube (GASTEC, No.81L)

[0159] (Example 1)

[0160] After adding pure water to a 150 ml container (mayonnaise bottle), potassium hydroxide is added to the container and dissolved at room temperature. Furthermore, γ-cyclodextrin is added and dissolved at room temperature. The pH of the obtained solution is 13.50. Next, methanol is added dropwise over about 15 minutes while stirring the solution with a stirrer. After the addition, the solution is stirred for 24 hours to obtain a suspension containing a solid product. The pH of the solution after the addition of methanol is 13.40. The solid product is filtered out from the obtained suspension, and the separated solid product is washed with methanol. After washing, the solid product is dried at 50°C for one night to obtain the metal organic structure A of Example 1.

[0161] The molar ratio of the components was potassium ion:γ-cyclodextrin:water:methanol=1:0.125:137.5:20.

[0162] By using Raman spectroscopy on the combustion residue obtained by TG measurement of the obtained metal organic structure A, it can be found that the -1 A C-C peak was observed at , which confirmed that the combustion residue was potassium carbonate.

[0163] Based on the above measurement results, when the composition molar ratio of the obtained metal organic structure A was calculated, γ-cyclodextrin:potassium ion=1:6.70.

[0164] The pore specific surface area is 1327.1m 2 / g. The pore volume is 0.483cm 3 / g. The pore diameter is 1.457nm. The maximum adsorption capacity of nitrogen is 312cm 3 / g,CO 2 The maximum gas adsorption capacity is 57cm 3 / g.

[0165] The adsorption sample was prepared by filling the collection bottle with various odor components with 0.2g of metal organic structure A. The total area value of TIC (total ion chromatogram) of hydrocarbon compounds, monocyclic compounds, and alcohol compounds detected by GC / MS (Shimadzu, GC-2010) between retention time 10.0 minutes and 30.0 minutes was used for comparative evaluation. The total area value reduction rate of TIC was 86.3%.

[0166] According to the GC / MS measurement results, hydrocarbons, butyraldehyde, ethyl acetate, hexane, hexane derivatives, heptane, heptane derivatives, cyclopentane derivatives, formic acid, octane, octane derivatives, octene, and octene derivatives are particularly adsorbed.

[0167] (Example 2)

[0168] Metal-organic structure B was obtained in the same manner as in Example 1 except that the molar ratio of the components used was potassium ion:γ-cyclodextrin:water:methanol=1:0.25:137.5:20.

[0169] The composition molar ratio of the obtained metal organic structure B was calculated in the same manner as in Example 1, and was γ-cyclodextrin:potassium ion=1:7.03.

[0170] The pore specific surface area is 1329.0m 2 / g. The pore volume is 0.483cm 3 / g. The pore diameter is 1.454nm. The maximum adsorption capacity of nitrogen is 312cm 3 / g,CO 2 The maximum gas adsorption capacity is 63cm 3 / g.

[0171] The TIC total area value reduction rate was 90.3%. The TIC total area value reduction rate of Example 2 was calculated in the same manner as in Example 1.

[0172] According to the GC / MS measurement results, hydrocarbons, butyraldehyde, ethyl acetate, hexane, hexane derivatives, heptane, heptane derivatives, cyclopentane derivatives, formic acid, octane, octane derivatives, octene, and octene derivatives are particularly adsorbed.

[0173] (Example 3)

[0174] Metal-organic structure C was obtained in the same manner as in Example 1 except that the molar ratio of the components used was potassium ion:γ-cyclodextrin:water:methanol=1:0.375:137.5:20.

[0175] The composition molar ratio of the obtained metal organic structure C was calculated in the same manner as in Example 1, and was γ-cyclodextrin:potassium ion=1:7.09.

[0176] The pore specific surface area is 1243.8m 2 / g. The pore volume is 0.452cm 3 / g. The pore diameter is 1.453nm. The maximum adsorption capacity of nitrogen is 291cm 3 / g,CO 2 The maximum gas adsorption capacity is 54cm 3 / g.

[0177] The TIC total area value reduction rate was 94.6%. The TIC total area value reduction rate of Example 3 was calculated in the same manner as in Example 1.

[0178] According to the GC / MS measurement results, hydrocarbons, butyraldehyde, ethyl acetate, hexane, hexane derivatives, heptane, heptane derivatives, cyclopentane derivatives, formic acid, octane, octane derivatives, octene, and octene derivatives are particularly adsorbed.

[0179] (Example 4)

[0180] Metal-organic structure D was obtained in the same manner as in Example 1 except that the molar ratio of the components used was potassium ion:γ-cyclodextrin:water:methanol=1:0.5:137.5:20.

[0181] The composition molar ratio of the obtained metal organic structure D was calculated in the same manner as in Example 1, and was γ-cyclodextrin:potassium ion=1:7.29.

[0182] The pore specific surface area is 1263.3m 2 / g. The pore volume is 0.457cm 3 / g. The pore diameter is 1.448nm. The maximum adsorption capacity of nitrogen is 297cm 3 / g,CO 2 The maximum gas adsorption capacity is 12cm 3 / g.

[0183] The TIC total area value reduction rate was 92.5%. The TIC total area value reduction rate of Example 4 was calculated in the same manner as in Example 1.

[0184] According to the GC / MS measurement results, hydrocarbons, butyraldehyde, ethyl acetate, hexane, hexane derivatives, heptane, heptane derivatives, cyclopentane derivatives, formic acid, octane, octane derivatives, octene, and octene derivatives are particularly adsorbed.

[0185] (Comparative Example 1)

[0186] The metal organic structure H was synthesized according to the method described in Non-Patent Document 1. Specifically, pure water was added to a 30cc container (screw-cap bottle), potassium hydroxide (metal component) was added to the container, and dissolved at room temperature. Furthermore, γ-cyclodextrin (ligand component) was added and dissolved at room temperature. The molar ratio of each component at this time was potassium ion: γ-cyclodextrin: water = 1: 0.125: 137.5.

[0187] Next, the container was placed in a 450 ml mayonnaise bottle filled with methanol, sealed, and left to stand for 7 days to obtain a suspension containing a solid product by a synthesis reaction at the liquid-liquid interface based on methanol vapor.

[0188] Furthermore, a solid product was collected by filtration from the obtained suspension, washed, and then dried overnight at 50° C. Thus, the metal-organic structure H of Comparative Example 1 was obtained.

[0189] The composition molar ratio of the obtained metal organic structure H was calculated in the same manner as in Example 1, and was γ-cyclodextrin:potassium ion=1:7.43.

[0190] The pore specific surface area is 853.3m 2 / g. The pore volume is 0.31cm 3 / g. The pore diameter is 1.451nm. The maximum adsorption capacity is 200cm 3 / g.

[0191] (result)

[0192] The results are shown in Table 1. As shown in Table 1, the composition molar ratio (organic ligand: metal) of the metal organic structure of Comparative Example 1 is 1:7.43, and the maximum nitrogen adsorption amount is 200 cm 3 In contrast, in Examples 1 to 4, it was confirmed that the alkali metal (potassium) was bonded in an amount of 7.40 mol or less per mol of the organic ligand, and the maximum nitrogen adsorption amount was 220 cm 3 / g or more, and the nitrogen adsorption is more excellent than that of Comparative Example 1. In addition, in Examples 1 to 4, it was confirmed that CO 2 Gas adsorption capacity is 10cm 3 / g or more, with excellent CO 2 Gas adsorption capacity.

[0193]

[0194] (Example 5)

[0195] Metal-organic structure E was obtained in the same manner as in Example 1 except that the molar ratio of the components used was potassium ion:γ-cyclodextrin:water:methanol=1:0.625:137.5:20.

[0196] The pore specific surface area is 1091.0m 2 / g. The pore volume is 0.395cm 3 / g. The pore diameter is 1.450nm. The maximum adsorption capacity is 258cm 3 / g.

[0197] The TIC total area value reduction rate was 87.6%. The TIC total area value reduction rate of Example 5 was calculated in the same manner as in Example 1.

[0198] According to the GC / MS measurement results, hydrocarbons, butyraldehyde, ethyl acetate, hexane, hexane derivatives, heptane, heptane derivatives, cyclopentane derivatives, formic acid, octane, octane derivatives, octene, and octene derivatives are particularly adsorbed.

[0199] (Example 6)

[0200] Metal-organic structure F was obtained in the same manner as in Example 1 except that the molar ratio of the components used was potassium ion:γ-cyclodextrin:water:methanol=1:0.75:137.5:20.

[0201] The pore specific surface area is 651.4m 2 / g. The pore volume is 0.236cm 3 / g. The pore diameter is 1.449nm. The maximum adsorption capacity is 157cm 3 / g.

[0202] The TIC total area value reduction rate was 87.1%. The TIC total area value reduction rate of Example 6 was calculated in the same manner as in Example 1.

[0203] According to the GC / MS measurement results, hydrocarbons, butyraldehyde, ethyl acetate, hexane, hexane derivatives, heptane, heptane derivatives, cyclopentane derivatives, formic acid, octane, octane derivatives, octene, and octene derivatives are particularly adsorbed.

[0204] (Example 7)

[0205] A metal-organic structure G was obtained in the same manner as in Example 1 except that the metal component was changed to sodium hydroxide.

[0206] The pore specific surface area is 945.5m 2 / g. The pore volume is 0.345cm 3 / g. The pore diameter is 1.461nm. The maximum adsorption capacity is 226cm 3 / g.

[0207] (Examination of Examples 1 to 7 and Comparative Example 1)

[0208] Examples 1 to 7 have the same pore specific surface area, pore volume, pore diameter and maximum adsorption amount as those of Comparative Example 1. In Comparative Example 1, in order to obtain the metal organic structure, no crystal formation was observed within 1 day, and at least 7 days were required, whereas in Examples 1 to 7, the metal organic structure could be obtained within 1 day.

[0209] (Example 8)

[0210] The metal organic structure I was obtained in the same manner as in Example 1 except that the organic ligand was α-cyclodextrin and the molar ratio of the components was potassium ion:α-cyclodextrin:water:methanol=1:0.125:137.5:184.

[0211] The obtained metal organic structure I was confirmed to have a crystal structure by PXRD.

[0212] The composition molar ratio of the obtained metal organic structure I was calculated in the same manner as in Example 1, and was α-cyclodextrin:potassium ion=1:3.78.

[0213] The TIC total area value reduction rate was 97.9%. The TIC total area value reduction rate of Example 8 was calculated in the same manner as in Example 1.

[0214] According to the GC / MS measurement results, hydrocarbons, butyraldehyde, ethyl acetate, hexane, hexane derivatives, heptane, heptane derivatives, cyclopentane derivatives, formic acid, octane, octane derivatives, octene, and octene derivatives are particularly adsorbed.

[0215] (Example 9)

[0216] Metal-organic structure J was obtained in the same manner as in Example 1 except that β-cyclodextrin was used as the organic ligand and the molar ratio of the components used was potassium ion:β-cyclodextrin:water:methanol=1:0.125:137.5:104.

[0217] The obtained metal organic structure J was confirmed to have a crystal structure by PXRD.

[0218] (Comparative Example 2)

[0219] The total TIC area value was used for comparison and evaluation based on the reduction rate using GC / MS (Shimadzu Corporation, GC-2010) in the same manner as in Example 1 except that the inside of the collection bottle was filled with γ-cyclodextrin. The total TIC area value reduction rate was 5.6%. It should be noted that the total TIC area value reduction rate of Comparative Example 2 was calculated based on the total TIC area value in the same manner as in Example 1 except that the adsorbent was not dispersed in the inside of the collection bottle where various odor components were captured.

[0220] (Comparative Example 3)

[0221] The total TIC area value was used for comparison and evaluation based on the reduction rate using GC / MS (Shimadzu Corporation, GC-2010) in the same manner as in Example 1 except that α-cyclodextrin was filled inside the collection bottle. The total TIC area value reduction rate was 18.4%. It should be noted that the total TIC area value reduction rate of Comparative Example 3 was calculated based on the total TIC area value in the same manner as in Example 1 except that the adsorbent was not dispersed inside the collection bottle where various odor components were collected.

[0222] (Example 10)

[0223] After adding pure water to a 150 ml container (mayonnaise bottle), add 2-methylimidazole to the container and dissolve it at room temperature (the pH of the solution at this time is 9.64), and then add an aqueous solution of zinc acetate dihydrate (zinc acetate dihydrate: pure water = 0.27 g: 5 g). The pH of the resulting solution is 7.48. Next, while stirring the solution with a stirrer, methanol is added dropwise. After the addition, the solution is stirred for 1 hour to obtain a suspension containing a solid product. The pH of the solution after the addition of methanol is 7.38. The solid product is filtered out from the resulting suspension, and the separated solid product is washed with methanol. After washing, the solid product is dried overnight at 50°C to obtain the metal organic structure K of Example 1.

[0224] The molar ratio of the components was zinc ion: 2-methylimidazole: water: methanol = 1: 2: 220: 125.

[0225] The pore specific surface area is 69.9m 2 / g. The pore volume is 0.015cm 3 / g. The pore diameter is 0.879nm. The maximum adsorption capacity is 65cm 3 / g.

[0226] (Example 11)

[0227] A metal organic structure L was obtained in the same manner as in Example 10 except that the molar ratio of the components used was zinc ion:2-methylimidazole:water:methanol=1:18:2220:125.

[0228] The pore specific surface area is 1610.5m 2 / g. The pore volume is 0.563cm 3 / g. The pore diameter is 1.398nm. The maximum adsorption capacity is 351cm 3 / g.

[0229] (Example 12)

[0230] A metal organic structure M was obtained in the same manner as in Example 10 except that the molar ratio of the components used was zinc ion:2-methylimidazole:water:methanol=1:30:2220:125.

[0231] The pore specific surface area is 1674.0m 2 / g. The pore volume is 0.583cm 3 / g. The pore diameter is 1.394nm. The maximum adsorption capacity is 367cm 3 / g.

[0232] (Example 13)

[0233] After pure water was added to a 150 ml container (mayonnaise bottle), trimesic acid and iron (III) nitrate nonahydrate were added to the container. The pH of the obtained solution was 2.11.

[0234] Next, methanol was added dropwise while stirring the solution with a stirrer. After addition, the solution was stirred for 48 hours to obtain a suspension containing a solid product. The pH of the solution after the addition of methanol was 2.03. The solid product was filtered from the obtained suspension, and the separated solid product was washed with methanol. After washing, the solid product was dried at 50° C. overnight, thereby obtaining the metal organic structure N of Example 1.

[0235] It should be noted that the molar ratio of each component is iron ion: trimesic acid: water: methanol = 1:0.25:1247:352.

[0236] The pore specific surface area is 1068.6m 2 / g. The pore volume is 0.42cm 3 / g. The pore diameter is 1.579nm. The maximum adsorption capacity is 277cm 3 / g.

[0237] (Example 14)

[0238] A metal organic structure L was obtained in the same manner as in Example 13 except that the molar ratio of the components used was iron ion: trimesic acid: water: methanol = 1:0.5:1247:352.

[0239] The pore specific surface area is 806.9m 2 / g. The pore volume is 0.298cm 3 / g. The pore diameter is 1.476nm. The maximum adsorption capacity is 284cm 3 / g.

[0240] (Example 15)

[0241] A metal organic structure O was obtained in the same manner as in Example 13 except that the molar ratio of the components used was iron ion: trimesic acid: water: methanol = 1:0.67:1247:352.

[0242] The pore specific surface area is 145.7m 2 / g. The pore volume is 0.051cm 3 / g. The pore diameter is 0.700nm. The maximum adsorption capacity is 39cm 3 / g.

[0243] (Inspection of Examples 8 to 15)

[0244] As shown in Examples 8 to 15, when metal ions other than alkali metal ions are used as metal ions and a substance different from γ-cyclodextrin is used as an organic ligand, an organometallic structure can be obtained in a short time as in Examples 1 to 7.

[0245] (Example 16)

[0246] The following raw materials were mixed to obtain an adsorbent-containing resin composition.

[0247] LDPE (Novatec LC600A): 90 parts

[0248] Metal organic structure A: 10 parts

[0249] Next, 2 g of the resin composition prepared above was formed into a film having an average film thickness of 0.2 mm using a punch press.

[0250] After drying the prepared film at 140°C for 3 hours, 2 g of the film was filled in a flask filled with 480 ppm of hexane, 500 ppm of octane, or 2 ppm of acetic acid to prepare an adsorption sample. The gas component concentration after 1 hour of filling the adsorption sample was measured using a detector tube. The adsorption test showed that the film formed of the resin composition containing the gas adsorbent adsorbed 96 ppm of hexane, 150 ppm of octane, and 2 ppm of acetic acid.

[0251] (Comparative Example 4)

[0252] The following materials were mixed to obtain a resin composition.

[0253] LDPE (Novatec LC600A): 100 parts

[0254] Next, 2 g of the resin composition prepared above was formed into a film having an average film thickness of 0.2 mm using a punch press.

[0255] The adsorption measurement test was carried out in the same manner as in Example 3. The membrane adsorbed 16 ppm of hexane, 100 ppm of octane, and 0.2 ppm of acetic acid.

Claims

1. A metal-organic structure comprising a metal and an organic ligand coordinated to the metal, The metal organic structure has a ring structure or a cage structure. The metal ion is bonded in an amount of 7.40 mol or less relative to 1 mol of the organic ligand.

2. The metal organic structure according to claim 1, in, Nitrogen adsorption capacity is 220cm 3 / g or above.

3. The metal organic structure according to claim 1, in, CO 2 Gas adsorption capacity is 10cm 3 / g or above.

4. The organometallic structure according to claim 1, in, The metal is an alkali metal.

5. The organometallic structure according to claim 4, in, The alkali metal is potassium.

6. The organometallic structure according to claim 1, in, The organic ligand is cyclodextrin.

7. The organometallic structure according to claim 6, in, The cyclodextrin is γ-cyclodextrin. 8 . An adsorbent comprising the organometallic structure according to claim 1 .

9. An adsorbent, It is characterized in that At least it can adsorb monocyclic compounds. The adsorbent contains a metal organic structure, which is composed of at least one organic ligand coordinated to at least one metal ion and has a ring structure or a cage structure, and the organic ligand is a cyclic organic compound.

10. The adsorbent according to claim 9, in, The metal ions are alkali metal ions.

11. The adsorbent according to claim 10, in, The alkali metal is potassium.

12. The adsorbent according to claim 9, in, The cyclic organic compound is a cyclodextrin compound.

13. The adsorbent according to claim 12, in, The cyclodextrin compound is α-cyclodextrin or γ-cyclodextrin.

14. The adsorbent according to claim 9, in, For the metal-organic structure, the organic ligand is cyclodextrin, and the metal ion is potassium ion.

15. The adsorbent according to claim 9, in, The metal organic structure has a two-dimensional sheet-like layered structure. The adsorbent according to claim 9 , wherein the monocyclic compound is a cyclopentane derivative.

17. The adsorbent according to claim 9, in, The metal ion is bonded in an amount of 7.40 mol or less relative to 1 mol of the organic ligand.

18. A resin composition, It is characterized in that The adsorbent according to claim 9 is contained in the resin.

19. A method for producing a metal organic structure having a ring structure, include: a step of preparing an aqueous solution containing a metal ion and an organic ligand capable of coordinating to the metal ion as a first solution, and A step of directly adding a second solution containing an organic solvent to the first solution to generate a metal-organic structure in which the organic ligand is coordinated to the metal ion.

20. The manufacturing method according to claim 19, in, The metal ion is bonded in an amount of 7.40 mol or less relative to 1 mol of the organic ligand.

21. The manufacturing method according to claim 19, in, The metal ions are alkali metal ions.

22. The manufacturing method according to claim 21, in, The metal ion is a potassium ion.

23. The manufacturing method according to claim 19, in, The organic ligand comprises a cyclodextrin compound.

24. The manufacturing method according to claim 23, in, The cyclodextrin compound includes γ-cyclodextrin.

25. The manufacturing method according to claim 19, in, The metal ion is a zinc ion, The organic ligand is a compound having an imidazole skeleton.

26. The manufacturing method according to claim 25, in, The compound having an imidazole skeleton is 2-methylimidazole.

27. The manufacturing method according to claim 19, in, The metal ion is an iron ion, The organic ligand is a compound having a monocyclic or polycyclic skeleton.

28. The manufacturing method according to claim 27, in, The compound having a monocyclic or polycyclic skeleton is trimesic acid.

29. The manufacturing method according to claim 19, in, In the first solution, the organic ligand is used in an amount of 0.05 to 50 mol relative to 1 mol of the metal ion.

30. The manufacturing method according to claim 19, in, The second solution is a solution for changing the pH of the first solution.

31. The manufacturing method according to claim 30, in, The second solution is a solution for lowering the pH of the first solution, The second solution is added in an amount that reduces the pH of the first solution by 0.01 to 0.

20.

32. The manufacturing method according to claim 19, in, The second solution contains at least one solvent selected from the group consisting of an alcohol solvent, a ketone solvent, and an aprotic solvent.

33. The manufacturing method according to claim 19, in, In the step of producing the metal organic structure, the second solution is added to the first solution while the first solution is sheared.

34. The production method according to any one of claims 19 to 33, in, The method further includes the step of separating the metal-organic structure after the step of generating the metal-organic structure.

35. The manufacturing method according to claim 34, in, The separation step includes a step of filtering a mixed solution of the first solution and the second solution.

36. The manufacturing method according to claim 35, in, The separation step includes a step of washing or drying the metal-organic structure after the filtering step.