Polyimide resin composition and molded article
By combining polyimide structural units and organic flame retardants in a specific ratio, the flame retardancy and appearance problems of polyimide resin when the thickness is thin are solved, and a polyimide with high flame retardancy and good appearance is realized. Imine resin composition, suitable for a variety of high frequency and communication equipment.
Patent Information
- Application Number
- CN202380023794.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-01
- Filing Date
- 2023-02-14
- Publication Date
- 2024-10-11
AI Technical Summary
It is difficult for existing polyimide resins to have high flame retardancy and good appearance when the thickness is thin. Especially in applications such as flexible printed circuit boards, it is difficult to maintain flame retardancy and appearance quality after the thickness of the molded body is reduced. .
Polyimide structural units and organic flame retardants with specific structures are used in a specific ratio to form a polyimide resin composition to improve its flame retardancy and appearance quality in thin layers.
Even when the thickness is thin, the polyimide resin composition can maintain high flame retardancy and good appearance, is suitable for high-frequency circuits, communication equipment and other fields, and has high heat resistance and low dielectric properties.
Smart Images

Figure CN118765307A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polyimide resin composition and a molded body. Background Art
[0002] Polyimide resin is a useful engineering plastic having high thermal stability, high strength, and high solvent resistance due to the rigidity of the molecular chain, resonance stabilization, and strong chemical bonding, and is used in a wide range of fields.
[0003] Although polyimide resins have high heat resistance, they do not exhibit thermoplasticity and have a problem of low molding processability. In recent years, polyimide resins having thermoplasticity have also been reported. In addition to the heat resistance inherent in polyimide resins, thermoplastic polyimide resins also have excellent molding processability. Therefore, thermoplastic polyimide resins can also be applied to molded bodies that can be used in harsh environments that nylon and polyester, which are general thermoplastic resins, cannot be used.
[0004] As one of the molecular designs for imparting thermoplasticity to polyimide resins, generally speaking, there is a method of introducing a soft structure such as an aliphatic structure into the main chain. The aliphatic structure has the following advantages: it is easier to impart thermoplasticity to polyimide and it is easy to exhibit low dielectric properties due to its large size. On the other hand, compared with the aromatic structure, its oxidation resistance is poor, resulting in the problem of reducing the high flame retardancy of the original polyimide.
[0005] In order to apply such thermoplastic polyimide resins to applications requiring high flame retardancy, studies have also been conducted on improving flame retardancy by adding flame retardants. For example, Patent Document 1 discloses a polyimide resin composition containing a polyimide resin of a specific structure and a phosphinate metal salt-based flame retardant, which has excellent molding processability and can have both high flame retardancy and good appearance.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: International Publication No. 2019 / 220968 Summary of the invention
[0009] Problem that the invention aims to solve
[0010] Among polyimide resins, especially semi-aromatic polyimide resins, fully aliphatic polyimide resins or polyimide resins with large substituents such as fluorine, in addition to the high heat resistance and dimensional stability originally possessed by polyimide resins, extremely low dielectric properties (low dielectric constant and low dielectric loss tangent) as resin materials can also be achieved. Therefore, polyimide resins are also attracting attention in the application of related components (flexible printed substrates, antennas, etc.) and other electrical / electronic components for the 5th generation mobile communication system (5G) requiring low dielectric properties. In these uses, in addition to low dielectric properties, similarly to the technology disclosed in patent document 1, it is also required to have high flame retardancy, even if flame retardants are added, no good appearance such as exudation will be produced.
[0011] However, when the thickness of the molded body is thin, such as a flexible printed circuit board, for example, when the thickness of the molded body is reduced to less than 500 μm, less than 200 μm, or further less than 100 μm, it becomes extremely difficult to achieve high flame retardancy and good appearance. The technology disclosed in Patent Document 1 still has room for improvement in this regard.
[0012] An object of the present invention is to provide a polyimide resin composition that can produce a molded product having both high flame retardancy and good appearance even when the thickness is thin (for example, 500 μm or less).
[0013] Solutions for solving problems
[0014] The present inventors have found that a polyimide resin composition containing a polyimide resin in which specific different polyimide structural units are combined at a specific ratio and an organic flame retardant having a specific structure can solve the above-mentioned problems.
[0015] That is, the present invention relates to the following contents.
[0016] [1] A polyimide resin composition comprising a polyimide resin (A) and a compound (B) represented by the following formula (5), wherein the polyimide resin (A) comprises a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), and the content ratio of the repeating structural unit of the formula (1) is 20 to 70 mol% relative to the total of the repeating structural unit of the formula (1) and the repeating structural unit of the formula (2).
[0017]
[0018] (R1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. X1 and X2 are each independently a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.)
[0019]
[0020] (R 51 R is an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms. 52 ~R 53 and R 61 ~R 66 Each independently represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. 51 is an integer from 0 to 6, p 52 and p 53 are each independently an integer from 0 to 4, p 63 and p 66 Each independently represents an integer from 0 to 3. 51 ~p 53 、p 63 or p 66 When it is 2 or more, multiple R 51 ~R 53 , R 63 or R 66 They are optionally the same or different from each other. n is an integer of 1 to 10.
[0021] Effects of the Invention
[0022] According to the polyimide resin composition of the present invention, a molded body having both high flame retardancy and good appearance can be made even in the case of thin thickness (e.g., less than 500 μm). Furthermore, the polyimide resin composition and the molded body containing it have high heat resistance (high glass transition temperature) and low dielectric properties. Therefore, the polyimide resin composition and the molded body of the present invention can be applied to applications requiring high flame retardancy and low dielectric constant and low dielectric loss tangent, such as: 5G, or the 6th generation mobile communication system (6G) related components using a frequency band of 70G to 300GHz, various antennas, various antenna substrates, wire coating materials, bonding sheets, insulating films, raw materials for carbon fiber reinforced plastics (CFRP), high-frequency circuit substrates, printed wiring substrates, chip-on-film (COF) flexible substrates, multi-layer laminates, LED mounting substrates, industrial robot substrates , communication substrates for household robots, semiconductor component materials, wafers for high-frequency devices, Wi-fi chips, wireless communication equipment, transmission lines, bearing coatings, heat-insulating shafts, trays, various belts, heat-resistant low-dielectric belts, heat-resistant low-dielectric tubes, various sensors, various radars, antenna covers (radomes), optical communication modules (TOSA / ROSA), 8k-TV wired mobile devices or digital home appliances, base stations, drones, surveillance cameras, indoor or outdoor servers, artificial satellites, communication equipment for space stations, etc. DETAILED DESCRIPTION
[0023] [Polyimide resin composition]
[0024] The polyimide resin composition of the present invention contains a polyimide resin (A) and a compound (B) represented by the following formula (5), wherein the polyimide resin (A) contains a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), and the content ratio of the repeating structural unit of the formula (1) is 20 to 70 mol% relative to the total of the repeating structural unit of the formula (1) and the repeating structural unit of the formula (2).
[0025]
[0026] (R1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. X1 and X2 are each independently a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.)
[0027]
[0028] (R 51 R is an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms. 52 ~R 53 and R 61 ~R 66 Each independently represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. 51 is an integer from 0 to 6, p 52 and p 53 are each independently an integer from 0 to 4, p 63 and p 66 Each independently represents an integer from 0 to 3. 51 ~p 53 、p 63 or p 66 When it is 2 or more, multiple R 51 ~R 53 , R 63 or R 66 They are optionally the same or different from each other. n is an integer of 1 to 10.
[0029] The polyimide resin composition of the present invention, by containing a polyimide resin (A) formed by combining specific different polyimide structural units in the above-mentioned specific ratio, becomes a resin composition that can better show thermoplasticity and excellent molding processability. In addition, by combining the polyimide resin (A) with a specific compound (B), even in the case of a thin thickness (e.g., less than 500 μm), a molded body that can have both high flame retardancy and good appearance can be produced.
[0030] In the present invention, the reason for obtaining the above-mentioned effect is not clear, but it is considered as follows. In aromatic condensed phosphate flame retardants, compound (B) has high heat resistance. On the other hand, since it is an organic flame retardant with a melting point, it is different from granular flame retardants without a melting point such as phosphinate metal salt flame retardants, and it is believed that the compatibility with polyimide resin (A) during thermal molding is higher. Therefore, it is believed that the polyimide resin composition according to the present invention can still show high flame retardancy even when making a molded body with a thin thickness, and it is not easy to cause precipitation, thermal decomposition, exudation, etc. of compound (B) in the molded body, and a good appearance can be maintained.
[0031] Polyimide resin (A) is a thermoplastic resin with high crystallinity. If a granular flame retardant without a melting point such as a phosphinate metal salt flame retardant is added thereto, the flame retardant will act as a crystal nucleating agent and have a tendency to promote crystallization. Generally speaking, if the crystallization of a crystalline thermoplastic resin is too fast, there is a situation where the extrudability is reduced during the crystallization and the melt mixing is cooled. However, compound (B) has the effect of delaying the crystallization of polyimide resin (A), that is, reducing the curing rate, and also has the effect of improving the extrudability of the obtained polyimide resin composition.
[0032] Furthermore, the polyimide resin composition containing the compound (B) can maintain or improve the low dielectric properties derived from the polyimide resin (A), and thus can achieve extremely low dielectric constant and dielectric loss tangent as a resin material.
[0033] <Polyimide resin (A)>
[0034] The polyimide resin (A) used in the present invention comprises a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), wherein the content ratio of the repeating structural unit of the formula (1) is 20 to 70 mol % relative to the total of the repeating structural unit of the formula (1) and the repeating structural unit of the formula (2).
[0035]
[0036] (R1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. X1 and X2 are each independently a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.)
[0037] The polyimide resin (A) used in the present invention is a thermoplastic resin, and its form is preferably powder or pellets. Thermoplastic polyimide resins are different from polyimide resins that do not have a glass transition temperature (Tg) and are formed by, for example, closing the imide ring after molding in the state of a polyimide precursor such as polyamic acid, or polyimide resins that decompose at a temperature below the glass transition temperature.
[0038] The repeating structural unit of formula (1) is described in detail below.
[0039] R1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. Here, the alicyclic hydrocarbon structure refers to a ring derived from an alicyclic hydrocarbon compound, and the alicyclic hydrocarbon compound may be saturated or unsaturated and may be monocyclic or polycyclic.
[0040] Examples of the alicyclic hydrocarbon structure include, but are not limited to, cycloalkane rings such as cyclohexane rings, cycloalkene rings such as cyclohexene, bicycloalkane rings such as norbornane rings, and bicycloalkene rings such as norbornene. Among these, cycloalkane rings are preferred, cycloalkane rings having 4 to 7 carbon atoms are more preferred, and cyclohexane rings are still more preferred.
[0041] The carbon number of R1 is 6-22, preferably 8-17.
[0042] R1 contains at least one alicyclic hydrocarbon structure, and preferably contains 1 to 3 alicyclic hydrocarbon structures.
[0043] R1 is preferably a divalent group represented by the following formula (R1-1) or (R1-2).
[0044]
[0045] (m 11 and m 12 Each independently represents an integer of 0 to 2, and is preferably 0 or 1. 13 ~m 15 Each independently represents an integer from 0 to 2, preferably 0 or 1.)
[0046] R1 is particularly preferably a divalent group represented by the following formula (R1-3).
[0047]
[0048] In addition, in the divalent group represented by the above formula (R1-3), the positional relationship of the two methylene groups with respect to the cyclohexane ring may be cis or trans, and the ratio of cis to trans may be any value.
[0049] X1 is a tetravalent group having 6 to 22 carbon atoms and including at least one aromatic ring. The aromatic ring may be a monocyclic ring or a condensed ring, and examples thereof include, but are not limited to, a benzene ring, a naphthalene ring, an anthracene ring, and a tetracene ring. Among these, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred.
[0050] X1 has 6 to 22 carbon atoms, preferably 6 to 18 carbon atoms.
[0051] X1 contains at least one aromatic ring, and preferably contains 1 to 3 aromatic rings.
[0052] X1 is preferably a tetravalent group represented by any of the following formulae (X-1) to (X-4).
[0053]
[0054] (R 11 ~R 18 Each is independently an alkyl group having 1 to 4 carbon atoms. 11 ~p 13 Each independently represents an integer of 0 to 2, and is preferably 0. 14 、p 15 、p 16 and p 18 Each independently represents an integer of 0 to 3, and is preferably 0. 17 is an integer of 0 to 4, preferably 0. 11 ~L 13 Each is independently a single bond, an ether group, a carbonyl group or an alkylene group having 1 to 4 carbon atoms.)
[0055] It should be noted that X1 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring, so R in formula (X-2) 12 , R 13 、p 12 and p 13 The tetravalent group represented by the formula (X-2) is selected so that the number of carbon atoms in the tetravalent group falls within the range of 10 to 22.
[0056] Similarly, L in formula (X-3) 11 , R 14 , R 15 、p 14 and p 15 The tetravalent group represented by formula (X-3) is selected so that the number of carbon atoms in the tetravalent group falls within the range of 12 to 22. 12 , L 13 , R 16 , R 17 , R 18 、p 16 、p 17 and p 18The tetravalent group represented by the formula (X-4) is selected so that the number of carbon atoms in the tetravalent group falls within the range of 18 to 22.
[0057] X1 is particularly preferably a tetravalent group represented by the following formula (X-5) or (X-6).
[0058]
[0059] Next, the repeating structural unit of formula (2) is described in detail below.
[0060] R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms, preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and further preferably 8 to 10 carbon atoms. Here, the chain aliphatic group refers to a group derived from a chain aliphatic compound, and the chain aliphatic compound may be saturated or unsaturated, may be straight chain or branched, and may contain heteroatoms such as oxygen atoms.
[0061] R2 is preferably an alkylene group having 5 to 16 carbon atoms, more preferably an alkylene group having 6 to 14 carbon atoms, further preferably an alkylene group having 7 to 12 carbon atoms, and particularly preferably an alkylene group having 8 to 10 carbon atoms. The alkylene group may be a linear or branched chain group, and is preferably a linear chain group.
[0062] R2 is preferably at least one selected from the group consisting of an octamethylene group and a decamethylene group, and is particularly preferably an octamethylene group.
[0063] In addition, other suitable embodiments of R2 include a divalent chain aliphatic group having 5 to 16 carbon atoms and containing an ether group. The carbon number is preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and further preferably 8 to 10 carbon atoms. Among them, a divalent group represented by the following formula (R2-1) or (R2-2) is preferred.
[0064]
[0065] (m 21 and m 22 Each independently represents an integer of 1 to 15, preferably 1 to 13, more preferably 1 to 11, and further preferably 1 to 9. 23 ~m 25 Each independently represents an integer of 1 to 14, preferably 1 to 12, more preferably 1 to 10, and even more preferably 1 to 8.)
[0066] It should be noted that R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and further preferably 8 to 10 carbon atoms). Therefore, m in formula (R2-1) is 21 and m 22The divalent group represented by formula (R2-1) is selected so that the number of carbon atoms in the group falls within the range of 5 to 16 (preferably 6 to 14, more preferably 7 to 12, and even more preferably 8 to 10). 21 +m 22 It is 5 to 16 (preferably 6 to 14, more preferably 7 to 12, and further preferably 8 to 10).
[0067] Similarly, m in formula (R2-2) 23 ~m 25 The divalent group represented by formula (R2-2) is selected so that the number of carbon atoms in the group falls within the range of 5 to 16 (preferably 6 to 14, more preferably 7 to 12, and even more preferably 8 to 10). 23 +m 24 +m 25 The carbon number is 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and still more preferably 8 to 10 carbon atoms).
[0068] X2 is defined similarly to X1 in formula (1), and preferred aspects are also the same.
[0069] The content ratio of the repeating structural unit of formula (1) is 20 to 70 mol% relative to the total of the repeating structural unit of formula (1) and the repeating structural unit of formula (2). When the content ratio of the repeating structural unit of formula (1) is within the above range, the polyimide resin can be fully crystallized even in a general injection molding cycle. If the content ratio is less than 20 mol%, the molding processability is reduced, and if it exceeds 70 mol%, the crystallinity is reduced, so the heat resistance is reduced.
[0070] From the viewpoint of expressing high crystallinity, the content ratio of the repeating structural unit of formula (1) relative to the total of the repeating structural unit of formula (1) and the repeating structural unit of formula (2) is preferably 65 mol% or less, more preferably 60 mol% or less, and further preferably 50 mol% or less.
[0071] The content ratio of the repeating structural unit of formula (1) relative to the total of the repeating structural unit of formula (1) and the repeating structural unit of formula (2) is preferably 20 mol% or more and less than 40 mol%. Within this range, the crystallinity of the polyimide resin (A) is improved, and a resin composition with better heat resistance can be obtained.
[0072] From the viewpoint of molding processability, the content ratio is preferably 25 mol % or more, more preferably 30 mol % or more, further preferably 32 mol % or more, and from the viewpoint of expressing high crystallinity, further preferably 35 mol % or less.
[0073] The total content ratio of the repeating structural units of the formula (1) and the repeating structural units of the formula (2) is preferably 50 to 100 mol %, more preferably 75 to 100 mol %, further preferably 80 to 100 mol %, and further preferably 85 to 100 mol % relative to all repeating structural units constituting the polyimide resin (A).
[0074] The polyimide resin (A) may further contain a repeating structural unit of the following formula (3). In this case, the repeating structural unit of formula (3) is preferably contained in an amount of 25 mol% or less relative to the total of the repeating structural unit of formula (1) and the repeating structural unit of formula (2). On the other hand, the lower limit is not particularly limited and may be greater than 0 mol%.
[0075] From the viewpoint of improving heat resistance, the content ratio is preferably 5 mol % or more, more preferably 10 mol % or more, while from the viewpoint of maintaining crystallinity, it is preferably 20 mol % or less, more preferably 15 mol % or less.
[0076]
[0077] (R3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. X3 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.)
[0078] R3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. The aromatic ring may be a monocyclic ring or a condensed ring, and examples thereof include, but are not limited to, a benzene ring, a naphthalene ring, an anthracene ring, and a tetracene ring. Among these, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred.
[0079] The carbon number of R3 is 6-22, preferably 6-18.
[0080] R3 contains at least one aromatic ring, preferably 1 to 3 aromatic rings.
[0081] In addition, the aromatic ring may also be bonded with a monovalent or divalent electron-withdrawing group. Examples of the monovalent electron-withdrawing group include a nitro group, a cyano group, a p-toluenesulfonyl group, a halogen group, a haloalkyl group, a phenyl group, an acyl group, and the like. Examples of the divalent electron-withdrawing group include a fluorinated alkylene group (e.g., -C(CF3)2-, -(CF2) p -(herein, p is an integer of 1 to 10)) such a halogenated alkylene group, in addition to -CO-, -SO2-, -SO-, -CONH-, -COO-, etc. can be mentioned.
[0082] R3 is preferably a divalent group represented by the following formula (R3-1) or (R3-2).
[0083]
[0084] (m 31 and m 32 Each independently represents an integer of 0 to 2, and is preferably 0 or 1. 33 and m 34 Each independently represents an integer of 0 to 2, and is preferably 0 or 1. 21 , R 22 and R 23 Each is independently an alkyl group having 1 to 4 carbon atoms, an alkenyl group having 2 to 4 carbon atoms, or an alkynyl group having 2 to 4 carbon atoms. 21 、p 22 and p 23 is an integer of 0 to 4, preferably 0. 21 is a single bond, an ether group, a carbonyl group, or an alkylene group having 1 to 4 carbon atoms.)
[0085] It should be noted that R3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring, so m in formula (R3-1) is 31 、m 32 , R 21 and p 21 The divalent group represented by the formula (R3-1) is selected so that the number of carbon atoms in the divalent group falls within the range of 6 to 22.
[0086] Similarly, L in formula (R3-2) 21 、m 33 、m 34 , R 22 , R 23 、p 22 and p 23 The divalent group represented by the formula (R3-2) is selected so that the number of carbon atoms in the divalent group falls within the range of 12 to 22.
[0087] X3 is defined similarly to X1 in formula (1), and preferred aspects are also the same.
[0088] The polyimide resin (A) may further contain a repeating structural unit represented by the following formula (4).
[0089]
[0090] (R4 is -SO2- or -Si(R x )(R y )O- divalent group, R x and R y Each independently represents a chain aliphatic group having 1 to 3 carbon atoms or a phenyl group. X4 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.
[0091] X4 is defined similarly to X1 in formula (1), and preferred aspects are also the same.
[0092] The terminal structure of the polyimide resin (A) is not particularly limited, but it is preferred that the terminal has a chain aliphatic group having 5 to 14 carbon atoms.
[0093] The chain aliphatic group may be saturated or unsaturated, and may be linear or branched. When the polyimide resin (A) has the above-mentioned specific group at the terminal, a resin composition having excellent heat aging resistance can be obtained.
[0094] Examples of the saturated chain aliphatic group having 5 to 14 carbon atoms include n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, lauryl, n-tridecyl, n-tetradecyl, isopentyl, neopentyl, 2-methylpentyl, 2-methylhexyl, 2-ethylpentyl, 3-ethylpentyl, isooctyl, 2-ethylhexyl, 3-ethylhexyl, isononyl, 2-ethyloctyl, isodecyl, isododecyl, isotridecyl and isotetradecyl.
[0095] Examples of the unsaturated linear aliphatic group having 5 to 14 carbon atoms include 1-pentenyl, 2-pentenyl, 1-hexenyl, 2-hexenyl, 1-heptenyl, 2-heptenyl, 1-octenyl, 2-octenyl, nonenyl, decenyl, dodecenyl, tridecenyl and tetradecenyl.
[0096] Among them, the above-mentioned chain aliphatic group is preferably a saturated chain aliphatic group, and more preferably a saturated straight-chain aliphatic group. In addition, from the viewpoint of obtaining heat aging resistance, the above-mentioned chain aliphatic group is preferably a carbon number of 6 or more, more preferably a carbon number of 7 or more, further preferably a carbon number of 8 or more, preferably a carbon number of 12 or less, more preferably a carbon number of 10 or less, and further preferably a carbon number of 9 or less. The above-mentioned chain aliphatic group may be only one kind, or may be two or more kinds.
[0097] The above-mentioned chain aliphatic group is particularly preferably at least one selected from the group consisting of n-octyl, isooctyl, 2-ethylhexyl, n-nonyl, isononyl, n-decyl and isodecyl, further preferably at least one selected from the group consisting of n-octyl, isooctyl, 2-ethylhexyl, n-nonyl and isononyl, and most preferably at least one selected from the group consisting of n-octyl, isooctyl and 2-ethylhexyl.
[0098] In addition, from the viewpoint of heat aging resistance, the polyimide resin (A) preferably has only a chain aliphatic group having 5 to 14 carbon atoms at the terminal, in addition to a terminal amino group and a terminal carboxyl group. When a group other than the above is present at the terminal, the content thereof is preferably 10 mol% or less, more preferably 5 mol% or less, relative to the chain aliphatic group having 5 to 14 carbon atoms.
[0099] From the viewpoint of showing excellent heat aging resistance, the content of the above-mentioned chain aliphatic group with 5 to 14 carbon atoms in the polyimide resin (A) is preferably 0.01 mol% or more, more preferably 0.1 mol% or more, and further preferably 0.2 mol% or more, relative to the total of 100 mol% of all repeating structural units constituting the polyimide resin (A). In addition, in order to ensure sufficient molecular weight and obtain good mechanical properties, the content of the above-mentioned chain aliphatic group with 5 to 14 carbon atoms in the polyimide resin (A) is preferably 10 mol% or less, more preferably 6 mol% or less, and further preferably 3.5 mol% or less, relative to the total of 100 mol% of all repeating structural units constituting the polyimide resin (A).
[0100] The content of the linear aliphatic group having 5 to 14 carbon atoms in the polyimide resin (A) can be determined by depolymerizing the polyimide resin (A).
[0101] The polyimide resin (A) preferably has a melting point of 360°C or less and a glass transition temperature of 150°C or more. From the viewpoint of heat resistance, the melting point of the polyimide resin is more preferably 280°C or more, and further preferably 290°C or more. From the viewpoint of high molding processability, it is preferably 345°C or less, more preferably 340°C or less, and further preferably 335°C or less. In addition, from the viewpoint of heat resistance, the glass transition temperature of the polyimide resin (A) is more preferably 160°C or more, and further preferably 170°C or more. From the viewpoint of high molding processability, it is preferably 250°C or less, more preferably 230°C or less, and further preferably 200°C or less.
[0102] The melting point and glass transition temperature of the polyimide resin (A) can be measured using a differential scanning calorimeter.
[0103] In addition, for the polyimide resin (A), from the viewpoint of improving crystallinity, heat resistance, mechanical strength, and chemical resistance, the heat of the crystallization exothermic peak observed when the polyimide resin is melted and cooled at a temperature drop rate of 20° C. / min (hereinafter referred to as “crystallization exothermic heat”) is preferably 5.0 mJ / mg or more, more preferably 10.0 mJ / mg or more, and further preferably 17.0 mJ / mg or more. The upper limit of the crystallization exothermic heat is not particularly limited, and is usually 45.0 mJ / mg or less.
[0104] The melting point, glass transition temperature and crystallization heat of the polyimide resin (A) can be specifically measured by the methods described in Examples.
[0105] The logarithmic viscosity of a 0.5 mass % concentrated sulfuric acid solution of the polyimide resin (A) at 30°C is preferably 0.2 to 2.0 dL / g, more preferably in the range of 0.3 to 1.8 dL / g. If the logarithmic viscosity is 0.2 dL / g or more, sufficient mechanical strength will be obtained when the obtained polyimide resin composition is made into a molded body, and if it is 2.0 dL / g or less, molding processability and operability will become good. Using a Cannon-Fenske viscometer, the flow time of concentrated sulfuric acid at 30°C and the above-mentioned polyimide resin solution is measured respectively, and the logarithmic viscosity μ is obtained by the following formula.
[0106] μ=ln(ts / t0) / C
[0107] t0: Flow time of concentrated sulfuric acid
[0108] ts: Flow time of polyimide resin solution
[0109] C:0.5(g / dL)
[0110] The weight average molecular weight Mw of the polyimide resin (A) is preferably 10,000 to 150,000, more preferably 15,000 to 100,000, further preferably 20,000 to 80,000, further preferably 30,000 to 70,000, further preferably 35,000 to 65,000. If the weight average molecular weight Mw of the polyimide resin (A) is 10,000 or more, the mechanical strength of the obtained molded body will be good, if it is 40,000 or more, the stability of the mechanical strength will be good, and if it is 150,000 or less, the molding processability will be good.
[0111] The weight average molecular weight Mw of the polyimide resin (A) can be measured by gel permeation chromatography (GPC) using polymethyl methacrylate (PMMA) as a standard sample.
[0112] (Method for producing polyimide resin (A))
[0113] The polyimide resin (A) can be produced by reacting a tetracarboxylic acid component containing a tetracarboxylic acid having at least one aromatic ring and / or a derivative thereof with a diamine component containing a diamine having at least one alicyclic hydrocarbon structure and a chain aliphatic diamine.
[0114] The tetracarboxylic acid containing at least one aromatic ring is preferably a compound in which four carboxyl groups are directly bonded to the aromatic ring, and an alkyl group may also be contained in the structure. In addition, the aforementioned tetracarboxylic acid preferably has a carbon number of 6 to 26. The aforementioned tetracarboxylic acid is preferably pyromellitic acid, 2,3,5,6-toluene tetracarboxylic acid, 3,3',4,4'-diphenyl ketone tetracarboxylic acid, 3,3',4,4'-biphenyl tetracarboxylic acid, 1,4,5,8-naphthalene tetracarboxylic acid, etc. Among these, pyromellitic acid is more preferred.
[0115] As the derivative of tetracarboxylic acid containing at least one aromatic ring, anhydride or alkyl ester of tetracarboxylic acid containing at least one aromatic ring can be mentioned. The above-mentioned tetracarboxylic acid derivative preferably has 6 to 38 carbon atoms. As the anhydride of tetracarboxylic acid, pyromellitic acid monoanhydride, pyromellitic acid dianhydride, 2,3,5,6-toluenetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-diphenylketonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride and the like can be mentioned. Examples of the alkyl esters of tetracarboxylic acids include dimethyl pyromellitic acid, diethyl pyromellitic acid, dipropyl pyromellitic acid, diisopropyl pyromellitic acid, dimethyl 2,3,5,6-toluenetetracarboxylate, dimethyl 3,3',4,4'-diphenylsulfonetetracarboxylate, dimethyl 3,3',4,4'-diphenylketonetetracarboxylate, dimethyl 3,3',4,4'-biphenyltetracarboxylate, and dimethyl 1,4,5,8-naphthalenetetracarboxylate. In the alkyl esters of the above tetracarboxylic acids, the number of carbon atoms in the alkyl group is preferably 1 to 3.
[0116] As the tetracarboxylic acid and / or its derivative containing at least one aromatic ring, at least one compound selected from the above may be used alone, or two or more compounds may be used in combination.
[0117] The carbon number of the diamine containing at least one alicyclic hydrocarbon structure is preferably 6 to 22, and for example, 1,2-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 4,4'-diaminodicyclohexylmethane, 4,4'-methylenebis(2-methylcyclohexylamine), carvone diamine, limonene diamine, isophorone diamine, norbornane diamine, bis(aminomethyl)tricyclo[5.2.1.0 2,6] decane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 4,4'-diaminodicyclohexylpropane, etc. These compounds can be used alone, or two or more compounds selected from these can be used in combination. Among these, 1,3-bis(aminomethyl)cyclohexane can be suitably used. In addition, the diamine containing an alicyclic hydrocarbon structure generally has structural isomers, but the ratio of cis-isomers / trans-isomers is not limited.
[0118] The chain aliphatic diamine may be straight chain or branched, and the number of carbon atoms is preferably 5 to 16, more preferably 6 to 14, and further preferably 7 to 12. In addition, if the number of carbon atoms in the chain portion is 5 to 16, an ether bond may be contained therebetween. As the chain aliphatic diamine, for example, 1,5-pentamethylenediamine, 2-methylpentane-1,5-diamine, 3-methylpentane-1,5-diamine, 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 1,10-decamethylenediamine, 1,11-undemethylenediamine, 1,12-dodecamethylenediamine, 1,13-tridecamethylenediamine, 1,14-tetradecamethylenediamine, 1,16-hexadecamethylenediamine, 2,2'-(ethylenedioxy)bis(ethyleneamine) and the like are preferred.
[0119] The chain aliphatic diamine may be used alone or in combination of two or more. Among these, chain aliphatic diamines having 8 to 10 carbon atoms are preferably used, and at least one selected from the group consisting of 1,8-octamethylenediamine and 1,10-decamethylenediamine is particularly preferably used.
[0120] When the polyimide resin (A) is produced, the molar ratio of the amount of the diamine containing at least one alicyclic hydrocarbon structure to be charged is preferably 20 to 70 mol% relative to the total amount of the diamine containing at least one alicyclic hydrocarbon structure and the chain aliphatic diamine. The molar amount is preferably 25 mol% or more, more preferably 30 mol% or more, and further preferably 32 mol% or more. From the viewpoint of expressing high crystallinity, it is preferably 60 mol% or less, more preferably 50 mol% or less, further preferably less than 40 mol%, and further preferably 35 mol% or less.
[0121] The diamine component may contain a diamine containing at least one aromatic ring. The diamine containing at least one aromatic ring preferably has 6 to 22 carbon atoms, and examples thereof include o-xylylenediamine, m-xylylenediamine, p-xylylenediamine, 1,2-diethynylphenylenediamine, 1,3-diethynylphenylenediamine, 1,4-diethynylphenylenediamine, 1,2-diaminobenzene, 1,3-diaminobenzene, 1,4-diaminobenzene, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene, α,α'-bis(3-aminophenyl)-1,4-diisopropylbenzene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,6-diaminonaphthalene, and 1,5-diaminonaphthalene.
[0122] In the above, the molar ratio of the amount of the diamine containing at least one aromatic ring to the total amount of the diamine containing at least one alicyclic hydrocarbon structure and the chain aliphatic diamine is preferably 25 mol% or less. On the other hand, the lower limit is not particularly limited and may be greater than 0 mol%.
[0123] From the viewpoint of improving heat resistance, the molar ratio is preferably 5 mol % or more, more preferably 10 mol % or more, while from the viewpoint of maintaining crystallinity, it is preferably 20 mol % or less, more preferably 15 mol % or less.
[0124] Furthermore, from the viewpoint of reducing coloration of the polyimide resin (A), the molar ratio is preferably 12 mol% or less, more preferably 10 mol% or less, further preferably 5 mol% or less, and further preferably 0 mol%.
[0125] When producing the polyimide resin (A), the charging amount ratio of the said tetracarboxylic acid component and the said diamine component is preferably 0.9-1.1 mol of diamine component with respect to 1 mol of tetracarboxylic acid component.
[0126] In addition, when manufacturing the polyimide resin (A), in addition to the aforementioned tetracarboxylic acid component and the aforementioned diamine component, an end-capping agent may also be mixed. The end-capping agent is preferably at least one selected from the group consisting of monoamines and dicarboxylic acids. The amount of the end-capping agent used is an amount that can introduce a desired amount of terminal groups into the polyimide resin (A), preferably 0.0001 to 0.1 mol, more preferably 0.001 to 0.06 mol, and further preferably 0.002 to 0.035 mol relative to 1 mol of the aforementioned tetracarboxylic acid and / or its derivative.
[0127] Among them, the end-capping agent is preferably a monoamine end-capping agent. From the viewpoint of introducing the aforementioned chain aliphatic group having 5 to 14 carbon atoms into the end of the polyimide resin (A) to improve the heat aging resistance, a monoamine having a chain aliphatic group having 5 to 14 carbon atoms is more preferred, and a monoamine having a saturated straight-chain aliphatic group having 5 to 14 carbon atoms is further preferred.
[0128] The blocking agent is particularly preferably at least one selected from the group consisting of n-octylamine, isooctylamine, 2-ethylhexylamine, n-nonylamine, isononylamine, n-decylamine and isodecylamine, further preferably at least one selected from the group consisting of n-octylamine, isooctylamine, 2-ethylhexylamine, n-nonylamine and isononylamine, and most preferably at least one selected from the group consisting of n-octylamine, isooctylamine and 2-ethylhexylamine.
[0129] As a polymerization method for producing the polyimide resin (A), a known polymerization method can be applied, and the method described in International Publication No. 2016 / 147996 can be used.
[0130] <Compound (B)>
[0131] The polyimide resin composition of the present invention contains a polyimide resin (A) and a compound (B) represented by the following formula (5).
[0132] By using the compound (B) shown in formula (5) as a flame retardant for the polyimide resin (A) having the above-mentioned specific structure, the obtained molded body can still obtain high flame retardancy and good appearance even when the thickness is thin. In addition, by using the compound (B), the extrudability of the polyimide resin composition is also improved, and as a resin material, an extremely low dielectric constant and dielectric loss tangent can be achieved.
[0133]
[0134] (R 51 R is an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms. 52 ~R 53 and R 61 ~R 66 Each independently represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms. 51 is an integer from 0 to 6, p 52 and p 53 are each independently an integer from 0 to 4, p 63 and p 66 Each independently represents an integer from 0 to 3. 51 ~p 53 、p 63 or p 66 When it is 2 or more, multiple R 51 ~R53 , R 63 or R 66 They are optionally the same or different from each other. n is an integer of 1 to 10.
[0135] In formula (5), R 51 It is an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and further preferably an alkyl group having 1 to 4 carbon atoms.
[0136] The alkyl group having 1 to 10 carbon atoms may be any of a linear and branched group, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a 2-methylbutyl group, a 1-methylbutyl group, a 1,2-dimethylpropyl group, a neopentyl group (2,2-dimethylpropyl group), a tert-pentyl group (1,1-dimethylpropyl group), an n-hexyl group, an isohexyl group, a 1-methylpentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 1-ethylbutyl group, a 2-ethylbutyl group, a 1,1-dimethylbutyl group, a 1,2-dimethylbutyl group, a 1,3-dimethylbutyl group, a 2,2-dimethylbutyl group, a 2,3-dimethylbutyl group, a 1-ethyl-1-methylpropyl group, a 1-ethyl-2-methylpropyl group, an n-heptyl group, an isoheptyl group, a 1-methylhexyl group, a 2-methylhexyl group, a 3-methyl 1-ethylhexyl, 4-methylhexyl, 1-ethylpentyl, 2-ethylpentyl, 3-ethylpentyl, 1-propylbutyl, 1,1-dimethylpentyl, 1,2-dimethylpentyl, 1,3-dimethylpentyl, 1,4-dimethylpentyl, 1-ethyl-1-methylbutyl, 1-ethyl-2-methylbutyl, 1-ethyl-3-methylbutyl, 2-ethyl-1-methylbutyl, 2-ethyl-1-methylbutyl, 2-ethyl-2-methylbutyl, 2-ethyl-3-methylbutyl, 1,1-diethylpropyl, n-octyl, isooctyl, 1-methylheptyl, 2-methylheptyl, 3-methylheptyl, 4-methylheptyl, 5-methylheptyl, 1-ethylhexyl, 2-ethylhexyl, 3-ethylhexyl, 4-ethylhexyl, 1-propylheptyl, 2-propylheptyl, nonyl and decyl.
[0137] Among the above alkyl groups, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, 2-methylbutyl, 1-methylbutyl, 1,2-dimethylpropyl, neopentyl (2,2-dimethylpropyl), tert-pentyl (1,1-dimethylpropyl), n-hexyl, isohexyl, 1-methylpentyl, 2-methylpentyl, 3-methylpentyl, 1-ethylbutyl, 2-ethylbutyl, 1,1-dimethylbutyl, 1,2-dimethylbutyl, 1,3-dimethylbutyl, 2,2-dimethylbutyl, 2,3-dimethylbutyl, 1-ethyl-1-methylpropyl or 1-ethyl-2-methylpropyl is preferred; methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl or tert-butyl is more preferred; methyl or ethyl is further preferred; and methyl is still more preferred.
[0138] The alkoxy group having 1 to 10 carbon atoms may be straight chain or branched. Examples thereof include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, a tert-butoxy group, an n-pentoxy group, an isopentoxy group, a 2-methylbutoxy group, a 1-methylbutoxy group, a 1,2-dimethylpropoxy group, a neopentoxy group (2,2-dimethylpropoxy group), a tert-pentoxy group (1,1-dimethylpropoxy group), an n-hexyloxy group, an isohexyloxy group, a 1-methylpentoxy group, a 2-methylpentoxy group, a 3-methylpentoxy group, a 1-ethylbutoxy group, a 2-ethylbutoxy group, a 1,1-dimethylbutoxy group, a 1,2-dimethylbutoxy group, a 1,3-dimethylbutoxy group, a 2,2-dimethylbutoxy group, a 2,3-dimethylbutoxy group, a 1-ethyl-1-methylpropoxy group, a 1-ethyl-2-methylpropoxy group, an n-heptyloxy group, an isoheptyloxy group, a 1-methylhexyloxy group, a 2-methylhexyloxy group, a 3-methyl 1-ethylpentyloxy, 2-ethylpentyloxy, 3-ethylpentyloxy, 1-propylbutoxy, 1,1-dimethylpentyloxy, 1,2-dimethylpentyloxy, 1,3-dimethylpentyloxy, 1,4-dimethylpentyloxy, 1-ethyl-1-methylbutoxy, 1-ethyl-2-methylbutoxy, 1-ethyl-3-methylbutoxy, 2-ethyl-1-methylbutoxy, 2-ethyl-1-methylbutoxy, 2-ethyl-2-methylbutoxy, 2-ethyl-3-methylbutoxy, 1,1-diethylpropoxy, n-octyloxy, isooctyloxy, 1-methylheptyloxy, 2-methylheptyloxy, 3-methylheptyloxy, 4-methylheptyloxy, 5-methylheptyloxy, 1-ethylhexyloxy, 2-ethylhexyloxy, 3-ethylhexyloxy, 4-ethylhexyloxy, 1-propylheptyloxy, 2-propylheptyloxy, nonyloxy, decyloxy and the like.
[0139] Among the above alkoxy groups, a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, a tert-butoxy group, an n-pentoxy group, an isopentoxy group, a 2-methylbutoxy group, a 1-methylbutoxy group, a 1,2-dimethylpropoxy group, a neopentoxy group (2,2-dimethylpropoxy group), a tert-pentoxy group (1,1-dimethylpropoxy group), an n-hexyloxy group, an isohexyloxy group, a 1-methylpentoxy group, a 2-methylpentoxy group, a 3-methylpentoxy group, a 1-ethylbutoxy group, a 2-ethylbutoxy group, a 1,1-dimethylbutoxy group, a 1,2-dimethylbutoxy group, a 1,3-dimethylbutoxy group, a 2,2-dimethylbutoxy group, a 2,3-dimethylbutoxy group, a 1-ethyl-1-methylpropoxy group or a 1-ethyl-2-methylpropoxy group is preferred, and a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group or a tert-butoxy group is more preferred.
[0140] R 52 ~R 53 and R 61 ~R 66 Each independently represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms, preferably an alkyl group having 1 to 4 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and further preferably an alkyl group having 1 or 2 carbon atoms.
[0141] The alkyl group having 1 to 4 carbon atoms may be linear or branched, and examples thereof include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, and tert-butyl.
[0142] Among the above-mentioned alkyl groups, a methyl group, an ethyl group, an n-propyl group or an isopropyl group is preferred, a methyl group or an ethyl group is more preferred, and a methyl group is further preferred.
[0143] The alkoxy group having 1 to 4 carbon atoms may be linear or branched, and examples thereof include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, and a tert-butoxy group.
[0144] Among the above-mentioned alkoxy groups, a methoxy group, an ethoxy group, an n-propoxy group or an isopropoxy group is preferred, and a methoxy group or an ethoxy group is more preferred.
[0145] In formula (5), p 51 It is an integer of 0-6, preferably 0-5, and more preferably 0-3.
[0146] p 52 and p 53 Each independently represents an integer of 0 to 4, preferably 0 to 2, and more preferably 0.
[0147] p 63 and p 66 Each independently represents an integer of 0 to 3, preferably 0 to 1, and more preferably 0.
[0148] n is an integer of 1 to 10, preferably 1 to 5, more preferably 1 to 3, and even more preferably 1.
[0149] From the viewpoint of achieving both high flame retardancy and good appearance even in a thin molded article having a thickness of, for example, 500 μm or less, the compound (B) is preferably at least one selected from the group consisting of compounds represented by the following structural formulas (B1) to (B3). More preferably, the compound (B) is a compound represented by the following structural formula (B3).
[0150]
[0151] As the compound (B), commercially available products such as “SR-3000” manufactured by DAIHACHI CHEMICAL INDUSTRY CO., LTD. can also be used.
[0152] The content of the compound (B) in the polyimide resin composition is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 30 parts by mass, further preferably 1 to 30 parts by mass, further preferably 2 to 30 parts by mass, further preferably 4 to 25 parts by mass, further preferably 5 to 25 parts by mass, further preferably 5 to 20 parts by mass, further preferably 5 to 15 parts by mass, relative to 100 parts by mass of the polyimide resin (A). If the content of the compound (B) is 0.1 parts by mass or more, it is easy to impart flame retardancy improvement and low dielectric properties, and if it is 30 parts by mass or less, good appearance and heat resistance can be maintained.
[0153] <Component (C): at least one selected from the group consisting of a phosphinate metal salt (C1) and a fluororesin (C2)>
[0154] The polyimide resin composition of the present invention may contain at least one component (C) selected from the group consisting of metal phosphinates (C1) and fluororesins (C2) in order to improve the anti-drip effect, further enhance the flame retardancy, and the like.
[0155] (Phosphinate Metal Salt (C1))
[0156] From the viewpoint of improving the anti-drip effect, the metal phosphinate (C1) is preferably a salt of at least one metal selected from the group consisting of Mg, Ca, Al, Zn, Ti, Sn, Zr and Fe. The metal is more preferably at least one selected from the group consisting of Mg, Ca and Al, and further preferably Al.
[0157] From the viewpoint of improving the anti-dripping effect and obtaining a good appearance, the metal phosphinate (C1) is more specifically preferably a compound represented by the following formula (i).
[0158]
[0159] (R' and R" are each independently a hydrocarbon group having 1 to 12 carbon atoms, M is a metal atom, and P is the valence of the metal atom represented by M.)
[0160] In the above formula (i), R' and R" each independently represent a hydrocarbon group having 1 to 12 carbon atoms. Examples of the hydrocarbon group include an alkyl group, a cycloalkyl group, an alkenyl group, an aryl group, and an aralkyl group.
[0161] Examples of the alkyl group include alkyl groups having 1 to 12 carbon atoms, such as methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, lauryl, isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, 2-methylpentyl, 2-methylhexyl, 2-ethylpentyl, 3-ethylpentyl, isooctyl, 2-ethylhexyl, 3-ethylhexyl, isononyl, 2-ethyloctyl, isodecyl and isododecyl.
[0162] Examples of the cycloalkyl group include cycloalkyl groups having 5 to 12 carbon atoms, such as cyclopentyl, cyclohexyl, cyclooctyl, and cyclodecyl.
[0163] Examples of the alkenyl group include alkenyl groups having 2 to 12 carbon atoms, such as vinyl, allyl, butenyl, 1-pentenyl, 2-pentenyl, 1-hexenyl, 2-hexenyl, 1-heptenyl, 2-heptenyl, 1-octenyl, 2-octenyl, nonenyl, decenyl and dodecenyl.
[0164] Examples of the aryl group include aryl groups having 6 to 12 carbon atoms, such as phenyl, tolyl, biphenyl and naphthyl.
[0165] Examples of the aralkyl group include aralkyl groups having 7 to 12 carbon atoms, such as benzyl, phenethyl, and phenylpropyl.
[0166] Among the above, R' and R" are preferably alkyl groups. The number of carbon atoms in the alkyl group is preferably 1 to 8, more preferably 1 to 6, and even more preferably 1 to 3.
[0167] R' and R" may be the same or different, and are preferably the same.
[0168] In the above formula (i), M is a metal atom, preferably at least one selected from the group consisting of Mg, Ca, Al, Zn, Ti, Sn, Zr and Fe. M is more preferably at least one selected from the group consisting of Mg, Ca and Al, and further preferably Al.
[0169] The metal phosphinate (C1) is preferably a compound (aluminum dialkylphosphinate) in which R' and R" in the above formula (i) are alkyl groups having 1 to 12 carbon atoms and M is Al. In this case, p in the above formula (i) is 3. More preferred embodiments of R' and R" are the same as those described above.
[0170] It is further preferred that the metal phosphinate (C1) is a compound (aluminum diethylphosphinate) in which R' and R" are ethyl groups and M is Al in the above formula (i). Aluminum diethylphosphinate is a compound represented by the following structural formula (ii).
[0171]
[0172] Since the metal phosphinate (C1) is a metal phosphinate, it is usually a solid compound, and from the perspective of dispersibility of the polyimide resin (A), it is preferably in powder form. In addition, from the perspective of improving the anti-drip effect and maintaining a good appearance, the particle size of the metal phosphinate (C1) is preferably small. From the above-mentioned perspectives, the particle size (D50) of the metal phosphinate (C1) is preferably 40 μm or less, more preferably 30 μm or less, further preferably 20 μm or less, further preferably 10 μm or less, and further preferably 5 μm or less. If the particle size (D50) of the metal phosphinate (C1) is 40 μm or less, especially 10 μm or less, the obtained polyimide resin composition and molded body will obtain higher flame retardancy and good appearance. In addition, from the perspective of operability (upward) and suppression of agglomeration, the particle size (D50) of the metal phosphinate (C1) is preferably 0.1 μm or more, more preferably 0.5 μm or more, and further preferably 1 μm or more.
[0173] The particle size (D50) of the metal phosphinate (C1) can be measured using a laser diffraction particle size distribution analyzer.
[0174] From the viewpoint of improving the anti-drip effect, the phosphorus content of the metal phosphinate (C1) is preferably 0.5% by mass or more, more preferably 1% by mass or more, and from the viewpoint of showing high flame retardancy in addition to the anti-drip effect, it is preferably 10% by mass or more, more preferably 15% by mass or more, and further preferably 20% by mass or more. In addition, from the viewpoint of improving the dispersibility of the polyimide resin (A) and maintaining a good appearance, the phosphorus content of the metal phosphinate (C1) is preferably 40% by mass or less.
[0175] The metal phosphinate (C1) can be manufactured by a known method. In addition, a commercially available metal phosphinate flame retardant can also be used as the metal phosphinate (C1). As commercially available metal phosphinate flame retardants, for example, "EXOLIT OP1230", "EXOLIT OP1240", "EXOLIT OP1400", "EXOLIT OP930", "EXOLIT OP935", "EXOLIT OP945", "EXOLIT OP945TP" etc. made by Clariant Chemicals Ltd. can be cited.
[0176] (Fluororesin (C2))
[0177] As fluororesin (C2), for example, polytetrafluoroethylene (PTFE), polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF), copolymer of tetrafluoroethylene and hexafluoropropylene (FEP), copolymer of tetrafluoroethylene and perfluoroalkyl vinyl ether (PFA), copolymer of tetrafluoroethylene and ethylene (ETFE), copolymer of tetrafluoroethylene and perfluoroalkoxyethylene, etc. can be mentioned, among which, one or more kinds can be used. Among them, polytetrafluoroethylene is preferred from the viewpoint of improving the anti-drip effect, maintaining a good appearance and heat resistance.
[0178] From the viewpoint of dispersibility and handling of the polyimide resin (A), the fluororesin (C2) used in the present invention is preferably in powder form. When the fluororesin (C2) is in powder form, the average particle size (D50) thereof is not particularly limited, but from the viewpoint of dispersibility and handling of the polyimide resin (A), it is preferably 1 to 50 μm, more preferably 2 to 40 μm, further preferably 3 to 30 μm, and further preferably 5 to 20 μm.
[0179] The average particle size (D50) can be measured using a laser diffraction light scattering particle size distribution analyzer.
[0180] As the fluororesin (C2), a commercially available product may also be used. Examples of polytetrafluoroethylene among commercially available fluororesins include “KT-300M”, “KT-400M”, “KT-600M”, “KTL-450A”, “KTL-450”, “KTL-610”, “KTL-610A”, “KTL-620”, “KTL-20N”, “KTL-10N”, “KTL-10S”, “KTL-9N”, “KTL-9S”, “KTL-8N”, “KTL-4N”, “KTL-2N”, “KTL-1N”, “KTL-8F”, “KTL-8FH”, and “KTL-500F” manufactured by Kitamura Co., Ltd., 3M Dyneon PTFE fine powders “TF9201Z”, “TF9205”, and “TF9207” manufactured by 3M Japan Limited, “POLYFLON MPA” series such as FA-500H and FA-5601 manufactured by Daikin Industries, Ltd., and “POLYFLON PTFE-M" series, "POLYFLONPTFE-F" series, "POLYFLON PTFE Lubron" series, etc.
[0181] Component (C) may be used alone or in combination with a metal phosphite (C1) and a fluororesin (C2). Component (C) is preferably a metal phosphite (C1) from the viewpoint of improving the anti-drip effect, maintaining good appearance and heat resistance, and adhesion to metals such as copper and steel plates.
[0182] When component (C) is used, the content of component (C) in the polyimide resin composition is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, further preferably 0.1 to 2 parts by mass, and further preferably 0.2 to 2 parts by mass, relative to 100 parts by mass of the polyimide resin (A). If the content of component (C) in the polyimide resin composition is 0.01 parts by mass or more relative to 100 parts by mass of the polyimide resin (A), it is easy to impart an anti-drip effect, and if it is 5 parts by mass or less, good appearance and heat resistance can be maintained.
[0183] When component (C) is used, the mass ratio of component (B) to component (C) in the polyimide resin composition [(B) / (C)] is preferably 1.0 to 40, more preferably 5.0 to 30, and even more preferably 10 to 20, from the viewpoint of obtaining an anti-drip effect, flame retardancy, good appearance and heat resistance.
[0184] However, from the viewpoint of obtaining high flame retardancy, good appearance and heat resistance even in a thin molded body with a thickness of 500 μm or less, and in particular from the viewpoint of reducing the burning time of the obtained polyimide resin composition and the molded body, it is preferred that the content of component (C) in the polyimide resin composition is small. From the viewpoint of preferentially reducing the burning time of the polyimide resin composition and the molded body, the content of component (C) in the polyimide resin composition can be set to 1.5 parts by mass or less, more preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, and more preferably 0.1 parts by mass or less relative to 100 parts by mass of the polyimide resin (A).
[0185] <Additives>
[0186] In the polyimide resin composition of the present invention, additives other than component (C) such as fillers, reinforcing fibers, matting agents, plasticizers, antistatic agents, anti-coloring agents, anti-gelling agents, colorants, slip improvers, antioxidants, conductive agents, resin modifiers, etc. can be mixed as needed. Regarding the effects of various additives, for example, inorganic fillers such as mica and talc, especially when micron-submicron or nanometer-sized powders (solid particles) are added, the low CTE (linear expansion coefficient) effect of the filler can be given while ensuring the appearance of the obtained molded body (especially thin film), so it is more suitable. In addition, when hollow materials headed by hollow silica are added, among which the hollow materials are micron-submicron or nanometer-sized, the low dielectric property improvement effect of the filler can be given on the basis of ensuring the appearance of the film, so it is more suitable. From the viewpoint of providing a low CTE effect or a low dielectric property improvement effect on the basis of ensuring a good appearance, the particle size (D50) of the solid particles and hollow materials is preferably 40 μm or less, more preferably 30 μm or less, further preferably 20 μm or less, further preferably 10 μm or less, and further preferably 5 μm or less. In addition, from the viewpoint of improving operability (suppressing upward movement) and suppressing agglomeration, it is preferably 0.1 μm or more, more preferably 0.5 μm or more, and further preferably 1 μm or more. D50 can be measured by a laser diffraction particle size distribution meter.
[0187] When the above-mentioned additives are used, there is no particular limitation on the amount thereof blended. However, from the viewpoint of maintaining the physical properties derived from the polyimide resin (A) while expressing the effects of the additives, the amount thereof in the polyimide resin composition is usually 50% by mass or less, preferably 0.0001 to 30% by mass, more preferably 0.001 to 15% by mass, and still more preferably 0.01 to 10% by mass.
[0188] In addition, in the polyimide resin composition of the present invention, other resins other than polyimide resin (A) can be mixed within the range that does not hinder its characteristics. As the other resins, preferably thermoplastic resins with high heat resistance, for example, polyimide resins other than polyamide resin, polyester resin, polyimide resin (A), polycarbonate resin, polyetherimide resin, polyamide-imide resin, polyphenylene ether imide resin, polyphenylene sulfide resin, polysulfone resin, polyether sulfone resin, polyarylate resin, liquid crystal polymer, polyether ether ketone resin, polyether ketone resin, polyether ketone ketone resin, polyether ether ketone ketone resin, polybenzimidazole resin etc. can be cited. Among these, from the viewpoint of heat resistance, molding processability, strength and solvent resistance, preferably one or more selected from the group consisting of polyetherimide resin, polyphenylene sulfide resin and polyether ether ketone resin, from the viewpoint of low water absorption, preferably liquid crystal polymer, from the viewpoint of obtaining high flame retardancy, preferably polyphenylene sulfide resin.
[0189] When the polyimide resin (A) and other resins are used in combination, the blending ratio is not particularly limited as long as it is within a range that does not inhibit the properties of the polyimide resin composition.
[0190] However, from the viewpoint of obtaining the effects of the present invention, the total content of the polyimide resin (A) and the compound (B) in the polyimide resin composition of the present invention is preferably 30% by mass or more, more preferably 40% by mass or more, further preferably 50% by mass or more, further preferably 70% by mass or more, further preferably 80% by mass or more, further preferably 90% by mass or more, further preferably 95% by mass or more, and is 100% by mass or less.
[0191] The polyimide resin composition of the present invention may be in any form, but is preferably in the form of pellets.
[0192] The polyimide resin composition of the present invention and the polyimide resin (A) used therein are thermoplastic, and therefore, can be prepared by, for example, adding the polyimide resin (A), the compound (B) and various optional components as required and dry mixing them, or feeding the compound (B) and the optional components separately from the feeding point of the polyimide resin (A) to the extruder, and then melt-kneading in the extruder, extruding strands, and cutting the strands to form pellets. In addition, by introducing the pellets into various molding machines and performing thermoforming by the method described below, a molded body having a desired shape can be easily manufactured.
[0193] During the manufacturing process and the thermoforming process of the pellets, the flame retardant may bleed out or undergo thermal decomposition, coloration, whitening, etc. However, the polyimide resin composition of the present invention is less likely to suffer from these defects and can maintain a good appearance.
[0194] The polyimide resin composition of the present invention preferably contains no solvent from the viewpoint of forming a pellet. Specifically, the content of the solvent in the polyimide resin composition is preferably 5% by mass or less, more preferably 1% by mass or less, and further preferably 0.1% by mass or less.
[0195] [Molding body]
[0196] The present invention provides a molded article comprising the polyimide resin composition.
[0197] The shape of the molded body is not particularly limited. From the viewpoint of effectively exerting the effect of the present invention that high flame retardancy and good appearance can be obtained even with a thin molded body, a film shape with a thickness of 500 μm or less, preferably 200 μm or less, more preferably less than 100 μm, further preferably 80 μm or less, and further preferably 60 μm or less is preferred. The lower limit of the thickness is usually 5 μm or more, preferably 10 μm or more.
[0198] In this specification, the "thickness of a film-shaped molded body" refers to the average value of the thickness of the film-shaped molded body. In addition, the film-shaped molded body includes the form of the resin layer constituting the multilayer laminate, the form of the coating layer, etc. in addition to the form of the resin film.
[0199] However, the shape of the molded article of the present invention is not limited to a film shape with a thickness of 500 μm or less. For example, even a flat plate-shaped molded article with a thickness exceeding 500 μm can still achieve the effects of the present invention.
[0200] The polyimide resin composition of the present invention can be easily manufactured by thermoforming because it has thermoplasticity. As a thermoforming method, injection molding, extrusion molding, inflation molding, blow molding, thermoforming, vacuum forming, compression molding, laser forming, welding, welding, etc. can be cited. As long as it is a molding method via a hot melt process, any method can be molded. When manufacturing a film-shaped molded body with a thickness of less than 500 μm, extrusion molding is preferred. In addition, when manufacturing a flat molded body with a thickness exceeding 500 μm, injection molding, etc. can be used.
[0201] Thermoforming is preferred because it can be performed without setting the molding temperature to a high temperature, for example, exceeding 400°C. Among them, in the case of injection molding, it is preferred because it can be performed without setting the molding temperature and the mold temperature during molding to a high temperature. For example, in injection molding, the molding temperature is preferably set to 400°C or less, more preferably to 360°C or less, and the mold temperature is preferably set to 260°C or less, more preferably to 220°C or less to enable molding. It should be noted that the polyimide resin (A) used in the present invention can be crystallized even at a mold temperature that is significantly lower than the glass transition temperature (for example, Tg-50°C) because it crystallizes very quickly compared to general crystalline resins.
[0202] As a method for producing a molded body, it is preferred to have a step of thermoforming the polyimide resin composition at 290 to 360° C. Thermoforming at a temperature exceeding 360° C. to 390° C. is also possible, but from the viewpoint of suppressing the degradation of the polyimide resin (A) and other resin components, thermoforming is preferably performed at a temperature of 360° C. or less. As a specific procedure, for example, the following method can be cited.
[0203] First, the compound (B) and various optional components as required are added to the polyimide resin (A) and dry-mixed, and then introduced into an extruder, preferably melted at 290 to 360° C., melt-kneaded and extruded in the extruder to produce pellets. Alternatively, the polyimide resin (A) may be introduced into an extruder, preferably melted at 290 to 360° C., and the compound (B) and various optional components as required are introduced therein, melt-kneaded and extruded with the polyimide resin (A) in the extruder to produce the pellets.
[0204] After the pellets are dried, they are introduced into various molding machines and thermoformed preferably at 290 to 360° C. to produce a molded body having a desired shape.
[0205] The polyimide resin composition of the present invention can be thermoformed by extrusion molding at a relatively low temperature of 290 to 360° C., so a molded product having a desired shape and excellent molding processability can be easily produced. The temperature during thermoforming is preferably 310 to 360° C.
[0206] <Flame retardancy>
[0207] The polyimide resin composition and molded article of the present invention exhibit high flame retardancy even when formed into a thin molded article with a thickness of 500 μm or less. The flame retardancy can be evaluated by a method based on the UL94 VTM test (thin material vertical combustion test; ASTM D4804), specifically, based on the method described in the examples.
[0208] <Low dielectric properties>
[0209] The polyimide resin composition and molded article of the present invention have low dielectric properties, for example, a dielectric constant of less than 3.0 and a dielectric loss tangent of less than 0.005 at a measurement frequency of 10 GHz can be achieved. The dielectric constant is preferably less than 2.90, more preferably less than 2.85, and the dielectric loss tangent is preferably less than 0.004, more preferably less than 0.003. For the dielectric constant and the dielectric loss tangent, specifically, the method described in the embodiments can be measured.
[0210] <Purpose>
[0211] According to the polyimide resin composition of the present invention, even when the thickness is thin (for example, 500 μm or less), a molded body having both high flame retardancy and good appearance can be produced.
[0212] In addition, the polyimide resin composition and the molded article containing the same have high heat resistance (high glass transition temperature) and low dielectric properties, so they can be used in applications requiring high flame retardancy, as well as low dielectric constant and low dielectric loss tangent, such as: 5G, or 6th generation mobile communication system (6G) related components using a frequency band of 70G to 300GHz (smartphones, flexible printed circuit boards, copper-clad laminates and other metal foil laminates, antennas, antenna substrates, etc.), various antennas other than the above (microwave antennas, millimeter wave antennas, waveguide slot antennas, horn antennas, lens antennas, printed antennas, three-plate antennas, microstrip antennas, patch antennas, etc.), various antenna substrates (antenna substrates for 77GHz vehicle-mounted millimeter wave radars, antenna substrates for terahertz wave radars, antenna substrates for aircraft radars, antenna substrates for tracked special vehicles, antenna substrates for WiGig, etc.), wire covering materials (low dielectric wire covering materials, etc.), bonding sheets, insulating films, raw materials for carbon fiber reinforced plastics (CFRP), high-frequency circuit substrates, printed wiring Substrates, chip-on-film (COF) flexible substrates, multi-layer laminates, LED-mounted substrates, industrial robot substrates, communication substrates for household robots, semiconductor component materials, high-frequency component wafers, Wi-fi chips, wireless communication equipment, transmission lines (coaxial lines, strip lines, microstrip lines, coplanar lines, parallel lines, etc.), bearing coatings, heat-insulating shafts, trays, various belts (seamless belts, etc.), heat-resistant low-dielectric belts, heat-resistant low-dielectric tubes, various sensors (touch sensors, etc.), various radars (automotive radars, aerospace radars, etc.), antenna covers (radomes), optical communication modules (TOSA / ROSA), wired mobile terminals or digital home appliances for 8k-TV (tablet terminals, notebook PCs, thin TVs, roll-up TVs, digital cameras, smart glasses, smart watches, etc.), base stations (macro cell base stations, small cell base stations, C-RAN base stations, etc.), drones (commercial drones, long-distance mobile drones, etc.), surveillance cameras, indoor or outdoor servers, artificial satellites, and communication equipment for space stations.
[0213] Among the above, the polyimide resin composition and molded article of the present invention are more preferably used for metal foil laminates, mainly copper-clad laminates. The metal foil laminates will be described below.
[0214] [Metal foil laminate]
[0215] The present invention provides a metal foil laminate having a layer formed of a molded product containing the polyimide resin composition and a layer formed of a metal foil.
[0216] As the metal foil laminate, a copper-clad laminate can be mainly mentioned, and the copper-clad laminate can be any one having a layer formed by a film-shaped molded body containing the aforementioned polyimide resin composition (hereinafter, also referred to as "resin film layer") and at least one copper foil layer. For example, a laminate having a structure in which copper foil is laminated on at least one side, preferably on both sides, of a resin film containing the aforementioned polyimide resin composition can be mentioned.
[0217] The resin film used in the manufacture of the copper-clad laminate can be manufactured by the same method as the manufacturing method of the molded body. From the viewpoint of ensuring the strength of the copper-clad laminate and improving the adhesion between the resin film layer and the copper foil layer, the thickness of the resin film and the resin film layer in the copper-clad laminate is preferably 5 to 500 μm, more preferably 10 to 300 μm, and further preferably 12.5 to 200 μm.
[0218] The copper foil used in the manufacture of the copper-clad laminate is not particularly limited, and commercially available rolled copper foil, electrolytic copper foil, etc. can be used, but rolled copper foil is preferred from the viewpoint of flexibility. From the viewpoint of ensuring sufficient conductivity and improving adhesion to the resin film layer, the thickness of the copper foil layer and the copper foil used in its formation is preferably 2 to 50 μm, more preferably 3 to 30 μm, and further preferably 5 to 20 μm. This thickness is the thickness of each copper foil layer or each copper foil.
[0219] In addition, the surface roughness of the copper foil used in the manufacture of the copper-clad laminate is not particularly limited, but the surface roughness of the copper foil is directly related to the electrical properties of the laminate itself obtained after the resin film is laminated. Generally speaking, the lower the roughness, the better the dielectric properties of the laminate. Therefore, the value of the maximum height Rz of the copper foil surface is preferably 0.1 to 1 μm, and more preferably in the range of 0.2 to 0.8 μm. The maximum height Rz of the copper foil surface can be measured, for example, by a surface roughness meter.
[0220] From the viewpoint of improving the strength and conductivity of the copper-clad laminate, the thickness of the copper-clad laminate is preferably 15 to 600 μm, more preferably 25 to 500 μm, and further preferably 50 to 300 μm. It should be noted that the copper-clad laminate may also have any layer other than the resin film layer and the copper foil layer as long as the effect of the present invention is not impaired.
[0221] The method for manufacturing the copper-clad laminate is not particularly limited, and a known method can be used. For example, a method of laminating by overlapping the above-mentioned resin film with copper foil and then laminating them under heating and pressurizing conditions can be cited. Since the resin film contains a thermoplastic polyimide resin (A), the surface can be pressed and bonded to the copper foil in a hot-melted state.
[0222] As a device used in the manufacture of copper-clad laminates, any device that can bond resin film and copper foil under heating and pressurizing conditions can be used, for example, a roller press, a flat laminator, a vacuum pressing device, a double-belt pressing device, etc. can be cited. Among these, from the perspective of the productivity of the copper-clad laminate and the perspective of obtaining a copper-clad laminate with good appearance, a vacuum pressing device or a double-belt pressing device is preferably used. The double-belt pressing device refers to a device that is equipped with a pair of endless belts arranged up and down, between which materials (resin film and copper foil) forming the film shape of each layer are continuously fed, and the aforementioned materials are heated and pressurized by a heating and pressing mechanism across the endless belt to form a device capable of manufacturing a laminate.
[0223] Examples of the double-belt press include a device described in Japanese Patent Application Laid-Open No. 2010-221694 and a double-belt press device manufactured by Dimenco Co., Ltd.
[0224] The heating temperature when manufacturing the copper-clad laminate using the above method is not particularly limited as long as it is a temperature that can soften or melt the resin film. From the perspective of reducing the burden on the device and manufacturing, it is preferably 250 to 400°C, and more preferably in the range of 280 to 350°C. In addition, for the pressurization conditions when manufacturing the copper-clad laminate, from the perspective of improving the adhesion between the resin film and the copper foil and reducing the burden on the device and manufacturing, the pressure is preferably 0.1 to 20 MPa, more preferably 0.15 to 15 MPa, and further preferably 0.2 to 12 MPa. In addition, from the perspective of improving production efficiency, the pressurization time is preferably 1 to 600 seconds, more preferably 5 to 400 seconds, and further preferably in the range of 10 to 300 seconds.
[0225] It should be noted that the aforementioned resin film has the feature of being heat-weldable, but in the manufacture of the copper-clad laminate, the resin film and the copper foil can also be bonded using an adhesive. The adhesive can arbitrarily select a varnish-like adhesive, a sheet-like adhesive, a powdery adhesive, etc. On the other hand, from the viewpoint of guaranteeing low dielectric properties, it is preferred that the adhesive still has low dielectric properties. As an adhesive of low dielectric properties, for example, the polyimide adhesive "PIAD" series made by Arakawa Chemical Industries, Ltd. can be cited.
[0226] Example
[0227] Next, the present invention will be described in more detail with reference to Examples, but the present invention is not limited thereto. In addition, various measurements and evaluations in each of the production examples and examples were performed in the following manner.
[0228] <Infrared spectroscopy analysis (IR measurement)>
[0229] The IR measurement of the polyimide resin was performed using “JIR-WINSPEC50” manufactured by JEOL Ltd.
[0230] <Logarithmic viscosity μ>
[0231] After drying the polyimide resin at 190 to 200° C. for 2 hours, 0.100 g of the polyimide resin was dissolved in 20 mL of concentrated sulfuric acid (96%, manufactured by Kanto Chemical Co., Ltd.), and the obtained polyimide resin solution was used as a measurement sample and measured using a Cannon-Fenske viscometer at 30° C. The logarithmic viscosity μ was determined by the following formula.
[0232] μ=ln(ts / t0) / C
[0233] t0: Flow time of concentrated sulfuric acid
[0234] ts: Flow time of polyimide resin solution
[0235] C: 0.5 g / dL
[0236] <Melting point, glass transition temperature, crystallization temperature, crystallization heat>
[0237] The melting point Tm, glass transition temperature Tg, crystallization temperature Tc, and crystallization heat ΔHm of the polyimide resin or the polyimide resin composition were measured using a differential scanning calorimeter (“DSC-6220” manufactured by SII NanoTechnology).
[0238] In a nitrogen atmosphere, the polyimide resin or polyimide resin composition was subjected to a thermal history of the following conditions: first heating (heating rate 10°C / min), followed by cooling (temperature drop rate 20°C / min), and then second heating (heating rate 10°C / min).
[0239] The melting point Tm is determined by reading the peak value of the endothermic peak observed in the second heating. The glass transition temperature Tg is determined by reading the value observed in the second heating. The crystallization temperature Tc is determined by reading the peak value of the exothermic peak observed during cooling.
[0240] In addition, the crystallization heat ΔHm (mJ / mg) was calculated from the area of the exothermic peak observed during cooling.
[0241] <Half crystallization time>
[0242] The crystallization half time of the polyimide resin is measured using a differential scanning calorimeter (“DSC-6220” manufactured by SII NanoTechnology).
[0243] The measurement conditions for the polyimide resin with a half-crystallization time of less than 20 seconds are as follows: in a nitrogen atmosphere, keep it at 420°C for 10 minutes to completely melt the polyimide resin, and then calculate the time from the appearance of the crystallization peak observed during a rapid cooling operation with a cooling rate of 70°C / min to the time it reaches the peak top.
[0244] <Weight Average Molecular Weight>
[0245] The weight average molecular weight (Mw) of the polyimide resin was measured under the following conditions using a gel permeation chromatography (GPC) measuring apparatus "Shodex GPC-101" manufactured by Showa Denko K.K.
[0246] Chromatographic column:Shodex HFIP-806M
[0247] Mobile phase solvent: HFIP containing 2 mM sodium trifluoroacetate
[0248] Column temperature: 40°C
[0249] Mobile phase flow rate: 1.0mL / min
[0250] Sample concentration: about 0.1% by mass
[0251] Detector: IR detector
[0252] Injection volume: 100μm
[0253] Standard curve: Standard PMMA
[0254] <Flame retardancy>
[0255] For Examples 1 to 8 and Comparative Examples 1 to 3, a 200 mm × 50 mm × 0.05 ± 0.01 mm thick molded body (film) was prepared by the method described below using the polyimide resin or the polyimide resin composition obtained in each example. The film was conditioned at 23 ± 2°C and 50 ± 5% RH for 48 hours and then used in a UL94VTM test (vertical burning test for thin materials; ASTM D4804) under a test environment of 25 ± 10°C and 75% RH or less.
[0256] Specifically, the film was rolled into a cylindrical shape and mounted vertically on a jig. Flame contact with a 20 mm flame using methane gas was performed twice for 3 seconds, and the flame retardancy was evaluated based on the combustion behavior.
[0257] Regarding Example 9, a flat plate-shaped molded body of 80 mm × 10 mm × 4 mm thickness was prepared by the method described below, and the flat plate was conditioned at 23 ± 2 ° C. and 50 ± 5% RH for 48 hours, and then used in the UL94V test (20 mm vertical combustion test; ASTM D3801) under a test environment of 25 ± 10 ° C. and 75% RH or less. Specifically, the flat plate was vertically mounted on a fixture, and flame contact was performed twice based on a 20 mm flame using methane gas for 10 seconds, and the flame retardancy was evaluated based on its combustion behavior.
[0258] (Maximum flame burning time after the first and second flame contact)
[0259] The maximum flame burning time (seconds) after the flame contact in the two flame contacts are shown in Tables 2 and 5 (n=5). A short burning time means good flame retardancy.
[0260] (Total burning time with flame)
[0261] The total flame burning time (seconds) is shown in Table 2 and Table 5 (n=5). A short total time means good flame retardancy.
[0262] ((Total burning time with / without flame after the second flame contact)
[0263] The total of the flame / no flame burning time after the second flame contact is shown in Table 2 and Table 5 (n=5). A shorter total time means better flame retardancy.
[0264] (Whether the burning reaches the 125mm mark)
[0265] In Examples 1 to 8 and Comparative Examples 1 to 3, whether the flame reached the mark 125 mm from the lower end of the film was observed, and the number of times the flame reached the 125 mm mark in 5 tests is shown in Table 3. A small number of reaching times means good flame retardancy.
[0266] (Whether the cotton is on fire)
[0267] In the above-mentioned combustion test, the presence or absence of ignition caused by dripping on the cotton set 300 mm below the film or the flat plate was observed. The number of ignitions of the cotton in the 5 tests is shown in Table 3 and Table 5. The case where there was no ignition was marked as "0 / 5". The smaller the number of ignitions, the higher the anti-drip effect.
[0268] (Determination of flame retardancy)
[0269] In Table 3, the level of flame retardancy is determined based on the UL94VTM criteria. In the UL94VTM criteria, the flame retardancy equivalent to VTM-0 is marked as "VTM-0", the flame retardancy equivalent to VTM-1 is marked as "VTM-1", and the flame retardancy equivalent to VTM-2 is marked as "VTM-2". The order of flame retardancy from high to low is VTM-0>1>2, and the case of not reaching the flame retardancy equivalent to VTM-2 is set as "VTM unsuitable".
[0270] In Table 5, the level of flame retardancy is determined based on the UL94V criteria. In the UL94V criteria, the flame retardancy equivalent to V-0 is marked as "V-0", the flame retardancy equivalent to V-1 is marked as "V-1", and the flame retardancy equivalent to V-2 is marked as "V-2". The order of flame retardancy from high to low is V-0>1>2, and the case of not reaching the flame retardancy equivalent to V-2 is set as "V unsuitable".
[0271] <Dielectric Constant and Dielectric Loss Tangent>
[0272] Using the polyimide resin or the polyimide resin composition obtained in each example, extrusion molding is performed by the method described below to make a film-like molded body, and then cut to obtain a 62mm×75mm×thickness 0.05±0.01mm evaluation film. After the film is dried at 100°C for 24 hours in a hot air dryer, it is conditioned at 23±2°C and 50±5%RH for 48 hours. Then, it is quickly used for measurement.
[0273] The dielectric constant and dielectric loss tangent were measured using "P5008A Keysight Streamline USB Vector Network Analyzer, 53 GHz" manufactured by Keysight Technologies at 23°C, 50% RH and a measurement frequency of 10 GHz in accordance with IEC 62631-2-1 and are shown in Table 4. The measured values are set as the average value of n=3.
[0274] <Appearance>
[0275] Using the polyimide resin or the polyimide resin composition obtained in each example, a molded body of 200 mm×50 mm×0.05±0.01 mm in thickness was prepared by the method described below, and its appearance was visually observed and evaluated according to the following criteria and shown in Table 4.
[0276] A: The film surface is smooth and has a good appearance.
[0277] B: Slight bumps and wrinkles can be observed on the film surface.
[0278] C: The film is warped and has uneven thickness.
[0279] <Strand extrudability>
[0280] The strand extrudability of the polyimide resin or the polyimide resin composition was evaluated based on the following criteria and the results are shown in Table 4.
[0281] AA: The strand diameter is kept constant and can be continuously extruded without breaking. In addition, it takes more than 3 seconds for the strand to become opaque after extrusion.
[0282] A: The strand diameter is kept constant and can be continuously extruded without breaking. In addition, the strand will become opaque within 3 seconds after extrusion.
[0283] B: Pulsation of the strand is observed and the strand diameter becomes unstable, or weak smoke is observed but the strand is not broken and can be continuously extruded.
[0284] C: Strand breakage, strong smoke generation, and venting occurred, making continuous extrusion difficult.
[0285] Production Example 1 (Production of Polyimide Resin 1)
[0286] 500 g of 2-(2-methoxyethoxy)ethanol (manufactured by Nippon Emulsifier Co., Ltd.) and 218.12 g (1.00 mol) of pyromellitic dianhydride (manufactured by Mitsubishi Gas Chemical Co., Ltd.) were introduced into a 2L separable flask equipped with a Dean-Stark apparatus, a Liebig cooling tube, a thermocouple, and four stirring blades, and after purging with nitrogen, the mixture was stirred at 150 rpm to form a uniform suspension solution. On the other hand, 49.79 g (0.35 mol) of 1,3-bis(aminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Co., Ltd., cis / trans ratio = 7 / 3) and 93.77 g (0.65 mol) of 1,8-octamethylenediamine (manufactured by Kanto Chemical Co., Ltd.) were dissolved in 250 g of 2-(2-methoxyethoxy)ethanol using a 500 mL beaker to prepare a mixed diamine solution. The mixed diamine solution was slowly added using a plunger pump. Although the dripping will cause heat, the internal temperature was adjusted to 40-80°C. The nitrogen purge state was set during the dripping of the mixed diamine solution, and the stirring blade speed was set to 250rpm. After the dripping was completed, 130g of 2-(2-methoxyethoxy)ethanol and 1.284g (0.0100mol) of n-octylamine (manufactured by Kanto Chemical Co., Ltd.) as a capping agent were added and further stirred. A light yellow polyamic acid solution was obtained at this stage. Then, after setting the stirring speed to 200rpm, the polyamic acid solution in the 2L separable flask was heated to 190°C. During the heating process, the precipitation of polyimide resin powder and the dehydration accompanying imidization were confirmed at a liquid temperature of 120-140°C. After being kept at 190°C for 30 minutes, it was allowed to cool to room temperature and filtered. The obtained polyimide resin powder was washed with 300 g of 2-(2-methoxyethoxy)ethanol and 300 g of methanol, filtered, and then dried at 180° C. for 10 hours using a dryer to obtain 317 g of a powder of polyimide resin 1.
[0287] The IR spectrum of polyimide resin 1 was measured, and the results showed that ν(C=O) was 1768, 1697 (cm -1 ) The characteristic absorption of the imide ring was observed. The logarithmic viscosity was 1.30 dL / g, Tm was 323°C, Tg was 184°C, Tc was 266°C, the crystallization exotherm was 21.0 mJ / mg, the semi-crystallization time was less than 20 seconds, and the Mw was 55,000.
[0288] The composition and evaluation results of the polyimide resin in Production Example 1 are shown in Table 1. In addition, the mol% of the tetracarboxylic acid component and the diamine component in Table 1 are values calculated from the input amount of each component when producing the polyimide resin.
[0289] [Table 1]
[0290] Table 1
[0291]
[0292] *1: Content ratio (mol %) of the structural unit of formula (1) relative to the total of the repeating structural unit of formula (1) and the repeating structural unit of formula (2) in the polyimide resin 1
[0293] The abbreviations in Table 1 are as follows.
[0294] PMDA: Pyromellitic Dianhydride
[0295] 1,3-BAC: 1,3-bis(aminomethyl)cyclohexane
[0296] OMDA: 1,8-octamethylenediamine
[0297] Examples 1 to 8 and Comparative Examples 1 to 3 (Production and Evaluation of Polyimide Resin Compositions and Molded Articles (Resin Films))
[0298] The polyimide resin 1 obtained in Preparation Example 1, the compounds shown in Tables 2 to 4, and other components were fully mixed by dry mixing. The obtained mixed powder was extruded into strands with a diameter of 2 to 3 mm using a co-rotating twin-screw kneading extruder ("HK-25D-41D" manufactured by Parker Corporation) at a barrel temperature of 350°C and a screw speed of 120 rpm. The strand extrudability at this time was evaluated according to the above criteria.
[0299] The strands extruded from the extruder were air-cooled and pelletized using a pelletizer ("FAN CUTTER FC-Mini-4 / N" manufactured by Hoshi Plastic Co., Ltd.) The obtained pellets (polyimide resin composition) were dried at 190° C. for 10 hours and then used for extrusion molding.
[0300] The pellets were fed into a 20 mm single screw extruder equipped with a 150 mm wide T die, melt kneaded at a resin temperature of 340 to 360° C., and continuously extruded from the T die of the single screw extruder. Then, the pellets were cooled using a metal roll as a cooling roll at 140° C. to obtain a resin film having a thickness of 0.05±0.01 mm.
[0301] Here, the temperature of the Φ20 mm single-screw extruder was adjusted to 340 to 355°C, and the temperature of the T-die was adjusted to 350°C.
[0302] Using the obtained pellets (polyimide resin composition) or the produced resin film, various evaluations were performed by the above-mentioned methods. The results are shown in Tables 2 to 4.
[0303] [Table 2]
[0304] Table 2
[0305]
[0306] [Table 3]
[0307] Table 3
[0308]
[0309] [Table 4]
[0310] Table 4
[0311]
[0312] The details of each component shown in Tables 2 to 4 are as follows.
[0313] <Polyimide resin (A)>
[0314] (A) Polyimide resin 1 obtained in Production Example 1, Mw: 55,000
[0315] <Compound (B)>
[0316] (B) SR-3000: a compound represented by the following structural formula (B3), manufactured by DAIHACHI CHEMICAL INDUSTRY CO., LTD.
[0317]
[0318] <Ingredient (C)>
[0319] (C1) EXOLIT OP945: a metal phosphinate flame retardant (aluminum diethylphosphinate) represented by the following structural formula (ii), manufactured by Clariant Chemicals Ltd., particle size (D50): 1.3 μm, phosphorus content: 23% by mass
[0320]
[0321] (C2) KTL-450: Polytetrafluoroethylene (PTFE), manufactured by Kitamura Co., Ltd.
[0322] The flame retardancy evaluation results are shown in Tables 2 to 3. As shown in Table 2, the molded body comprising the polyimide resin composition of the present invention has a shorter burning time and better flame retardancy than the molded body of the comparative example. In addition, according to Table 3, especially in Examples 2 to 8, despite being a very thin molded body with a thickness of 0.05 mm ± 0.01 mm, a flame retardancy equivalent to VTM-0 in the UL94VTM criterion can be achieved.
[0323] Table 4 shows the evaluation results of thermal properties, dielectric properties, appearance and strand extrusion. According to Table 4, the molded bodies containing the polyimide resin composition of the present invention all have good appearance. Regarding strand extrusion, the polyimide resin compositions of Examples 1 to 5 containing only compound (B) as a flame retardant show particularly good results. It is believed that this is because compound (B) does not act as a crystal nucleating agent, unlike other flame retardants (component (C1)), but has the effect of delaying the crystallization of polyimide resin (A).
[0324] Furthermore, the dielectric constant of the molded body including the polyimide resin composition of the present invention is 3 or less and the dielectric loss tangent is 0.005 or less, which are extremely low dielectric constant and dielectric loss tangent for a resin molded body.
[0325] Example 9 (Manufacture and evaluation of a polyimide resin composition and a molded product (a flat plate having a thickness of 4 mm))
[0326] Pellets of a polyimide resin composition were prepared in the same manner as in Example 2. The pellets were dried at 190° C. for 10 hours and then used for injection molding.
[0327] An injection molding machine ("ROBOSHOT α-S30iA" manufactured by FANUC) was used to perform injection molding at a barrel temperature of 350°C, a mold temperature of 200°C, and a molding cycle of 50 seconds to produce a type 1A test piece specified in JIS K7161-2:2014.
[0328] The obtained 1A type test piece was processed into a flat plate of 80 mm×10 mm×4 mm thick, and flame retardancy was evaluated by the above method. The results are shown in Table 5. The evaluation results other than flame retardancy were the same as those of Example 2.
[0329] [Table 5]
[0330] Table 5
[0331]
[0332] According to Table 5, the molded body including the polyimide resin composition of the present invention exhibits good flame retardancy even when the thickness exceeds 500 μm.
[0333] Industrial Applicability
[0334] According to the polyimide resin composition of the present invention, even when the thickness is thin (e.g., less than 500 μm), a molded body having both high flame retardancy and good appearance can be produced. In addition, the polyimide resin composition and the molded body containing the same have high heat resistance (high glass transition temperature) and low dielectric properties. Therefore, the polyimide resin composition and the molded article of the present invention can be applied to applications requiring high flame retardancy and low dielectric constant and low dielectric loss tangent, for example, 5G, or 6th generation mobile communication system (6G) related components using a frequency band of 70G to 300GHz, various antennas, various antenna substrates, wire coating materials, bonding sheets, insulating films, raw materials for carbon fiber reinforced plastics (CFRP), high-frequency circuit substrates, printed wiring substrates, chip-on-film (COF) flexible substrates, multi-layer laminates, LED mounting substrates, industrial robot substrates, communication substrates for household robots, semiconductor element materials, high-frequency device wafers, Wi-fi chips, wireless communication equipment, transmission lines, bearing coatings, heat-insulating shafts, trays, various belts, heat-resistant low-dielectric belts, heat-resistant low-dielectric tubes, various sensors, various radars, antenna covers (radomes), optical communication modules (TOSA / ROSA), wired mobile terminals or digital home appliances for 8k-TV, base stations, drones, surveillance cameras, indoor or outdoor servers, artificial satellites, and communication equipment for space stations.
Claims
1. A polyimide resin composition comprising a polyimide resin (A) and a compound (B) represented by the following formula (5), wherein the polyimide resin (A) comprises a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), and the content ratio of the repeating structural unit of the formula (1) is 20 to 70 mol% relative to the total of the repeating structural unit of the formula (1) and the repeating structural unit of the formula (2). R1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure; R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms; X1 and X2 are each independently a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring, R 51 is an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms; R 52 ~R 53 and R 61 ~R 66 Each independently represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms; 51 is an integer from 0 to 6, p 52 and p 53 are each independently an integer from 0 to 4, p 63 and p 66 Each independently represents an integer from 0 to 3; p 51 ~p 53 、p 63 or p 66 When it is 2 or more, multiple R 51 ~R 53 , R 63 or R 66 are optionally the same as or different from each other; and n is an integer of 1 to 10.
2. The polyimide resin composition according to claim 1, wherein The content of the compound (B) in the polyimide resin composition is 0.1 to 30 parts by mass relative to 100 parts by mass of the polyimide resin (A).
3. The polyimide resin composition according to claim 1 or 2, wherein The compound (B) is at least one selected from the group consisting of compounds represented by the following structural formulas (B1) to (B3), 4 . A molded product comprising the polyimide resin composition according to claim 1 .
5. The molded article according to claim 4, wherein The molded body is in the form of a film having a thickness of 500 μm or less. 6 . A metal foil laminate comprising a layer formed of the molded product according to claim 4 or 5 and a layer formed of a metal foil.