Method for manufacturing fuel cell separator with integrated elastomeric seal

Through the combination of UV curable elastomer composition and flexible sheet mold, the problems of fragile thin sheets and long production cycle in the separator manufacturing process in the prior art are solved, fast and reliable seal application is achieved, and fuel efficiency is improved. Production efficiency of battery separators.

CN118765446APending Publication Date: 2024-10-11ILLUMING POWER INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023711.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-11
Filing Date
2023-02-23
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the existing technology, when manufacturing separators for solid polymer electrolyte fuel cells, liquid injection molding technology easily causes sheet breakage, high clamping pressure and thermal curing processes lead to slow production cycles, and UV curing methods are limited by mold materials and thicknesses. , it is difficult to achieve fast and reliable seal production.

Method used

Using a UV curable elastomer composition and a flexible PTFE or polystyrene sheet mold, the seal is injected and cured in the clamping block through UV irradiation, and the flexibility of the flexible sheet is used to avoid damage to the fragile seal. damage and reduce processing pressure through moderate clamping and injection pressure to achieve rapid seal application.

Benefits of technology

It achieves the rapid and reliable manufacturing of fuel cell separators with integrated seals in commercial production, reduces the risk of breakage and production cycle during processing, improves production efficiency, and avoids the problem of delamination of seals and plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765446A_ABST
    Figure CN118765446A_ABST
Patent Text Reader

Abstract

Using a UV curable elastomeric composition for a seal, a simple, fast method for making a fuel cell separator with an integrated elastomeric seal has been developed. A mold for the seal is used, the mold comprising a flexible sheet made of PTFE or polystyrene. The mold is compressed against the diaphragm between the support and the UV-permeable clamping block. The elastomer is then suitably injected and cured using UV light. Thereafter, the flexible sheet is peeled, rather than one-time overall removal, thereby avoiding delamination of the frangible seal from the septum.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for making a separator for a fuel cell. In particular, the present invention relates to a method for making a separator with an integrated elastomeric seal for a solid polymer electrolyte fuel cell.

[0002] background

[0003] Fuel cells have been used in niche applications for decades, but still show promise for many other applications that require electricity. They are generally considered clean (green), with desirable efficiency and safety features. However, cost remains a challenge, as some of the materials used can be expensive and some components are complex in design and expensive to manufacture. One such component may be a separator or partition used in a fuel cell stack, and particularly in a solid polymer electrolyte fuel cell stack.

[0004] There are several types of fuel cell designs, including high operating temperature types (such as solid oxide fuel cells) and low operating temperature types (such as alkaline fuel cells). Solid polymer electrolyte fuel cells belong to the latter type and are preferably used in power applications such as automobiles, ships and trains. Such fuel cells electrochemically convert fuel (typically hydrogen) and oxidant (typically oxygen) to generate electricity. They usually use proton-conducting polymer membrane electrolytes between two electrodes (i.e., cathode and anode). The cathode and anode electrodes include suitable catalysts to accelerate the desired reaction occurring in the fuel cell. Often, the cathode and anode are directly applied to the membrane electrolyte to form an integrated assembly called a catalyst-coated membrane assembly (CCM). A gas diffusion layer (typically a porous conductive layer including carbon fiber, etc.) is provided on the electrode surface adjacent to the CCM to improve the distribution of fluids to and from the electrodes during operation. The structure of the CCM comprising a CCM sandwiched between two gas diffusion layer electrodes is referred to as a membrane electrode assembly (MEA). In a typical solid polymer electrolyte fuel cell, a flow field plate including a number of fluid distribution channels for reactants is provided on either side of the MEA to deliver the fuel and oxidant first to the corresponding gas diffusion layer and then to the electrodes in the cell, and then remove the byproducts of the electrochemical reaction occurring in the cell. Water is the main byproduct in cells that work with hydrogen and air reactants and typically work in the range of about 80°C to 100°C. Since the output voltage of a single cell is on the order of 1V, multiple cells are usually stacked in series for commercial applications. Some kind of separator is used to separate the individual cells in such a stack from each other. For efficiency and convenience, the flow field plate is typically also used as such a separator. The fuel cell stack can be further connected in an array of interconnected stacks in series and / or parallel for automotive applications, etc.

[0005] In addition to water, heat is also an important byproduct from the electrochemical reactions that occur in the fuel cell. Therefore, a device for cooling the fuel cell stack is generally required. Stacks designed to achieve high power density (e.g., automotive stacks) typically circulate liquid coolant throughout the stack to quickly and effectively remove heat. To achieve this, a coolant flow field including many coolant channels is also typically incorporated into the flow field plate (or separator) of the battery in the stack. The coolant flow field can be formed on the electrochemically inactive surface of the flow field plate, and thus the coolant can be evenly distributed throughout the battery while keeping the coolant reliably separated from the reactants.

[0006] Therefore, bipolar separator assemblies including anode flow field plates and cathode flow field plates are commonly used in the art, and the anode flow field plates and cathode flow field plates have been combined and properly sealed together to form a sealed coolant flow field between the plates. Various transition channels, ports, pipes and other features involving all three working fluids (i.e., fuel, oxidant and coolant) may also appear on the inactive sides of these plates. These working fluids may be provided under considerable pressure, and therefore all these features in the plates must be properly sealed to prevent leakage between the fluids and to the external environment. The bipolar separator must be chemically resistant to these fluids at elevated temperatures. Another requirement for the bipolar separator assembly is that there is a satisfactory electrical connection between the two plates. This is because a large amount of current generated by the fuel cell stack must pass between the two plates.

[0007] Many variations of flow field plate designs and materials for bipolar separator plate assemblies are known in the art. The plates and / or assemblies may alternatively be metallic, in which case they are typically formed from one or more sheets of a suitable specialty metal using various stamping steps. They are then welded or adhesively bonded and sealed together so as to properly seal all fluid passages from each other and from the external environment.

[0008] Flow field (separator) plate and bipolar separator assembly can also be made of carbon optionally. Carbon can be the preferred material for such applications due to its expected high corrosion resistance, good electrical conductivity, relatively easy to manufacture and relatively low cost. Flexible graphite or expanded graphite sheet etc. are usually used as the substrate for the flow field plate of the manufacture of fuel cell. These carbon sheets are easy to handle, and complex structures can be easily imprinted therein. However, they are porous and must be impregnated with suitable filler or monomer composition, so that the plate is properly sealed and prevented from leaking liquid or gas through it. In addition, the impregnated monomer composition of solidification is also needed to give the product flow field plate additional other desired mechanical properties, including rigidity within the fuel cell operating temperature range. Therefore, high glass transition temperature Tg is considered to be desired.

[0009] As is apparent from the above, the design of typical flow fields / separators and assemblies for solid polymer electrolyte fuel cell stacks is quite complex. In order to reduce volume and increase energy density, such plates are usually thin and fragile. Many reliable seals are required not only between the plates constituting the bipolar plate assembly but also between adjacent cells in the assembled fuel cell stack. In order to simplify the assembly of the cell stack, the seal employed is preferably attached to or integrated on one of the separators (or bipolar separator assemblies, as the case may be) associated with each individual cell in the stack.

[0010] Due to the many mechanical and chemical properties required for long-term, reliable function, the choice of sealing materials that can be used in typical solid polymer electrolyte fuel cells is limited. Silicone and polyisobutylene (PIB) elastomers are commonly used in this regard. For example, US 7686854 discusses the use of silicone compositions in seals. The typical prior art method for incorporating silicone sealants directly into the separator is to use liquid injection molding (LIM) technology to mold a suitable liquid silicone composition on the plate. The composition is then typically cured at elevated temperatures. However, these LIM methods have some disadvantages, including: the high injection pressures used may break thin and relatively thin plates, especially because they are more fragile at elevated temperatures; the high clamping pressures used to seal the mold to the plate during processing may also break the plate, especially because they are more fragile at elevated temperatures; and the required thermal curing process results in slow production cycle times, especially when compared with faster curing processes (such as UV curing).

[0011] In this regard, it is well known that a variety of elastomers (including silicone elastomers) can be rapidly cured by exposing a suitable precursor composition to UV light. "Silicone rubber is cured quickly by UV light", Sealing Technology, Vol. 2009, No. 11, November 2009, p. 2. Although UV curing processes may be desirable, there are significant limitations on the material selection and thickness of suitable molds (and therefore on coating capabilities) because a large UV transmittance through the mold must be maintained. Nevertheless, a variety of mold materials (including polymethyl methacrylate or PMMA and PTFE) and / or UV curing techniques have been desirably used to apply a variety of plastics (including epoxy resins, elastomers, etc.) to other substrates (e.g., as disclosed in US2005 / 0167894 or EP1700680).

[0012] In US20090004541, it is proposed to use PIB elastomer sealant materials and methods involving UV curing and UV penetrable molds to apply sealants to fuel cell components (including flow field plates). US 6057054 and US5264299 are discussed for the prior art of silicone sealants molded on MEA and plates. As disclosed, the mold member is desirably penetrable to actinic radiation (such as UV radiation), that is, transmissive or substantially transmissive. Optionally, if necessary, a release agent (such as dry PTFE spray, spray oil, etc.) can be applied before introducing the liquid composition used to facilitate the removal of the cured gasket from the mold cavity. However, the use of release agents is generally not preferred because they are consumables, thereby increasing costs, they are difficult to apply to recessed features, and the release agent is ultimately left on the product parts. Example discloses the preparation of certain formulations and several UV-cured polyisobutylene / silane samples.

[0013] Despite the many advances made to date in the economical, efficient production of fuel cell components and commercial fuel cell stacks, there remains a need for improved manufacturing methods to produce these items more reliably and faster. The present invention satisfies these needs and provides further related advantages as disclosed below.

[0014] Overview

[0015] Manufacturing methods for making fuel cell separators with integrated elastomeric seals that are more suitable for commercial production have been developed. These methods are simple and fast, and include UV curing of UV curable elastomeric compositions molded directly on the separator. Importantly, these methods allow the removal of the associated mold without delamination or damage of the fragile integrated seal. These methods are particularly suitable for producing separators with integrated seals for solid polymer electrolyte fuel cells.

[0016] Specifically, the method of the present invention includes obtaining a non-porous plate (i.e., a desired separator), placing the plate on a suitable support so that the surface of the plate opposite to the expected sealing surface is adjacent to the support, and placing a mold for a seal against the expected sealing surface of the plate. The mold includes a flexible sheet made of polytetrafluoroethylene (PTFE) or polystyrene, a cavity for a seal formed on the surface of the flexible sheet adjacent to the expected sealing surface of the non-porous plate, and at least one injection port connected to the cavity fluid. Then, the method further includes placing a UV-permeable clamping block against the mold, compressing the UV-permeable clamping block toward the support so that the flexible sheet is sealed against the expected sealing surface of the plate, injecting a UV-curable elastomeric composition into the injection port and the cavity, irradiating UV light through the UV-permeable clamping block and through the mold so that the injected elastomeric composition is cured, removing the clamping block from the mold, and finally peeling the flexible sheet from the plate.

[0017] In the method, the non-porous plate may be selected from the group consisting of graphite, expanded graphite, impregnated expanded graphite, porous carbon foam, porous carbon, carbon, carbon composites, and metal foils.

[0018] The method is applicable to various types of non-porous fuel cell separators, including those of single plate or bipolar plate assemblies. In addition, the method is applicable to separators including flow fields formed on one or both surfaces, and is particularly applicable to separators including inlet and outlet ports for various reactants and coolants used in a typical assembled fuel cell stack. The thickness of the relevant non-porous plate can typically range from as low as 0.1 mm (for separators in which no flow field is formed) to 2.0 mm thick (for separators with flow fields formed on both surfaces).

[0019] An exemplary flexible sheet used in the method may have a thickness of 0.5 to 3 mm. An exemplary cavity in the associated mold may have a depth of 0.3 to 1.5 mm.

[0020] Suitable material choices for the UV-transparent clamping blocks involved include polymethylmethacrylate (PMMA) or glass. Suitable UV-curable elastomeric compositions include silicone precursors and polyisobutylene precursors. And suitable wavelengths of UV light involved in the irradiation step and subsequent curing step are in the range of 250 to 500 nm.

[0021] These and other aspects of the invention will become apparent upon reference to the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1a An isometric view of an exemplary bipolar separator including flow fields, fluid ports, and integrated seals for a solid polymer electrolyte fuel cell is shown.

[0023] Figure 1b Shown along Figure 1a A cross section of the bipolar separator along line AA is shown in FIG.

[0024] Figures 2a to 2e A schematic diagram of the various steps generally included in the method of the present invention is shown. For illustrative purposes, the separators shown are Figure 1a and Figure 1b The bipolar separator shown in is similar.

[0025] Specifically, Figure 2a Shown are initial acquisition and placement steps for certain components involved.

[0026] Figure 2b The injection step is shown.

[0027] Figure 2c A UV irradiation step is shown to complete the curing.

[0028] Figure 2d The stripping step is shown after removal of the clamping blocks (not shown).

[0029] Figure 2e The fabricated bipolar separator is shown. DETAILED DESCRIPTION

[0030] Unless the context requires otherwise, throughout this specification and claims, the words "comprise", "comprising", etc. should be interpreted in an open, inclusive sense. The words "a / an", etc. should be taken to mean at least one and not limited to only one.

[0031] Additionally, the following definitions are used herein.

[0032] As used herein, "PTFE" stands for polytetrafluoroethylene.

[0033] In the context of this disclosure, "flexible sheet" is defined as a sheet having a thickness range of up to 15 mm. PTFE and / or polystyrene sheets within this range flex sufficiently so that the stresses on the fragile seal (just injection molded and cured onto the separator) are small enough to avoid delamination of the seal from the plate when the sheet is peeled therefrom. (For reference, the Young's modulus of PTFE and polystyrene are 400 and 3250 MPa, respectively. The deflection achieved will be a function of this modulus and the thickness of the sheet.)

[0034] The method of the present invention represents an improved means for manufacturing fuel cell separators with integrated elastomeric seals. It is simple, rapid and reliable and comprises the use of a UV-curable elastomeric composition for the seal and UV curing technology to apply the seal to the separator.

[0035] Figure 1a and 1b Shown is a view of an exemplary expanded graphite bipolar separator with an integrated seal intended for use in a solid polymer electrolyte fuel cell. Figure 1a and 1b An isometric view and a cross-sectional view along line AA of a bipolar separator 1 are shown, respectively. The bipolar separator 1 includes a cathode flow field plate (or separator) 1a and an anode flow field plate (or separator) 1b, which are combined together to form an integral bipolar separator. Both the cathode and anode flow field plates 1a, 1b include 2 ports for inlet and outlet of fluids (i.e., fuel, oxidant, and coolant) supplied to and removed from the assembled fuel cell stack. In addition, channels have been formed on one surface of the cathode flow field plate 1a to produce a cathode flow field 3, and channels have been formed on the opposite surface to produce a portion of a coolant flow field 5. In a similar manner, channels have also been formed on one surface of the anode flow field plate 1b to produce an anode flow field 4, and channels have been formed on the opposite surface to produce another portion of the coolant flow field 5.

[0036] exist Figure 1a and 1b Also present is an elastomeric seal 6 which has been integrated into (attached to) the cathode flow field plate 1a of the bipolar separator 1. The elastomeric seal 6 is complex in shape and includes sealing portions around the port 2 and the periphery of the cathode flow field plate 1a, and may also include sealing portions in other areas (e.g. around transition areas or other special features) if / as required. Due to the properties of the materials used (e.g., carbon for the cathode flow field plate 1a and silicone for the elastomeric seal 6) and the small thickness of the components (typically at most a few millimeters), the bond between the cathode flow field plate 1a and the elastomeric seal 6 is very fragile and easily damaged or destroyed.

[0037] Figures 2a to 2e shows how to make Figure 1a and 1b Schematic diagram of an exemplary bipolar separator with integrated seal. Initially, a non-porous plate to be integrated with a seal is obtained. Here, the non-porous plate is a bipolar separator plate including an integral cathode flow field plate 1a and an anode flow field plate 1b, hereinafter referred to as plate 1a / 1b. Now as Figure 2aAs shown in , the plate 1a / 1b is placed on the support 10 so that its surface opposite to the intended sealing surface is adjacent to the support 10. The mold 11 is placed against the intended sealing surface of the plate 1a / 1b. In this specific example, the mold 11 is a single piece, namely a flexible PTFE sheet. (However, in other embodiments of the present invention, the mold 11 can be a flexible polystyrene sheet and / or a flexible sheet having both PTFE and polystyrene components. In addition, the mold 11 can also include certain other elements for other mechanical purposes.) The mold / flexible PTFE sheet 11 includes a cavity 11a for the seal and an injection port 11b fluidly connected to the cavity 11a to allow the injected silicone elastomer composition to enter the cavity 11a. It should be noted that in these figures, the injection port 11b is shown in the form of a straight cylindrical opening. Although satisfactory results can be obtained thereby (as confirmed by experimental tests), in alternative embodiments, a moderately tapered injection port can be used to allow easier demoulding (i.e., separation from the runner formed after curing). It should also be noted that the injection port 11b slightly deviates from the main body of the seal 6 so that the runner can be easily accessed and removed, and it is in a position that does not affect the sealing function. In addition, the mold / flexible PTFE sheet 11 includes a sheet 11c that can be pulled by a machine, and the sheet can be grabbed and pulled by an appropriate mechanical device, which is used for the subsequent stripping step included in the method. Finally, as shown, a UV-permeable clamping block 12 is placed against the mold / flexible PTFE sheet 11. The UV-permeable clamping block 12 includes two injection ports 12b, which are used for the same purpose as the injection port 11b and are consistent with it. A UV blocking sleeve 12a is arranged around the injection port 12b to prevent UV radiation from curing the elastomeric composition injected in the injection port 12b (additional explanation is given below). As shown in these figures, the UV blocking sleeve 12a is optionally made long enough to extend into the flexible PTFE sheet 11 during the compression, injection and UV irradiation steps. However, in alternative embodiments, the UV blocking sleeve 12a may be just long enough that it extends through the thickness of the UV transparent clamping block 12 .

[0038] Figure 2b The schematic diagram shown in describes the compression and injection steps included in the general method of the present invention. Here, the UV-transmissive clamping block 12 is compressed toward the support 10 (indicated by arrow 13), so that the mold / PTFE sheet 11 is sealed against the intended sealing surface of the plate 1a / 1b. (The compression device, such as a press, is not shown in these figures.) Next, the desired UV-curable elastomeric composition 14 is injected into the injection port 12b, through the injection port 11b and into the cavity 11a, thereby forming the seal 6. (The injection device, such as a pump, is not shown in these figures.)

[0039] Next, and if Figure 2c As shown in the schematic diagram of , UV light 15 of an appropriate wavelength is irradiated through both the UV-transmissive clamping block 12 and the inherently UV-transmissive flexible PTFE sheet 11 for a sufficient time to cure the injected elastomeric composition 14 and thereby form a cured elastomeric seal 6 and thereby integrate it onto the plate 1a / 1b. Because the mold / flexible PTFE sheet 11 is inherently UV-transmissive, the elastomeric composition in the injection port 11b is also cured by the UV light. However, because the injection port 12b is shielded from the UV light by the UV blocking sleeve 12a, the elastomeric composition in the injection port 12b remains uncured and fluid. Therefore, the cured elastomer in the injection port 12b does not need to be removed from the UV-transmissive clamping block 12 before it is ready for reuse.

[0040] With the seal 6 now formed and integrated onto the plate 1a / 1b, the UV transparent clamping block 12 is removed from the mold / flexible PTFE sheet 11 and Figure 2d As shown in FIG. 1 , the flexible PTFE sheet 11 is peeled from the plate 1a / 11b. The peeling can be accomplished using a suitable mechanical device (not shown) to grab the machine-pullable sheet 11c and pull it off the plate 11a / 11b at a desired angle and along a desired path (indicated by arrow 16). The angle and path and the peeling speed are selected so that the sheet 11 deflects appropriately and separates from the plate 11a / 11b from left to right in a smooth, stable manner, as shown in FIG. Figure 2d By appropriately selecting these parameters, the flexible PTFE sheet 11 can be reliably and relatively quickly removed without damaging the seal 6 or causing it to delaminate from the plates 11a / 11b. And of course, in order to enable the PTFE sheet 11 to flex appropriately, a sheet that is thin enough must be selected to enable it to flex in this manner. Figure 2e described in (and similar to Figure 1b ), with the stripping step completed, the manufacture of the bipolar separator 1 with an integrated seal is completed.

[0041] As is apparent from the foregoing, the method of the present invention is very simple and requires very few steps. Both the clamping pressure and the injection pressure employed can be significantly less than those used by conventional LIM techniques, thereby significantly reducing the likelihood of the separator breaking during processing, especially at higher temperatures used in thermal curing. For example, clamping pressures of the order of 0.5-4 tons and injection pressures of the order of 1-30 bar can be used in the method of the present invention, rather than about 20-80 tons and 100-150 bar, respectively, which are typically used for LIM processing. In addition, and very advantageously, the time required to inject and fully cure the elastomeric composition using the UV curing method of the present invention is much faster than using a typical thermal curing method. For example, the former only requires about 2-10 seconds, while the latter typically requires 30-60 seconds. Still further, and importantly, during processing using the prior art method, the sealing material may significantly adhere to the mold. This adhesion leads to problems in demolding the sealant from the mold cavity without delaminating the sealant from the board. However, the present invention substantially overcomes this problem by gradually and reliably demolding the sealant from the cavity by peeling the sealant away, thereby preventing delamination and damage.

[0042] Although the foregoing disclosure is mainly directed to integrating silicone elastomer seals into carbon bipolar separators intended for solid polymer electrolyte fuel cells, it will be appreciated by those of ordinary skill that the present invention has the potential for wider applications. For example, it can be advantageously used to manufacture other fuel cell types (e.g., alkaline fuel cells). In addition, the one or more imperforate plates involved can be made not only of carbon (e.g., graphite, expanded graphite, impregnated expanded graphite, porous carbon foam, porous carbon, carbon, carbon composite materials, etc.), but also of alternative conventional materials (e.g., metal foil). In addition, the present invention is applicable to use with separators comprising a single plate and bipolar separators comprising two or more plates. Still further, the present invention is applicable to use with separators having flow fields and / or ports incorporated therein, or without such flow fields and / or ports incorporated therein. Typically, the thickness of such optional plates is then about 0.1 to 2.0 mm. Outside of fuel cell applications, this technology can be used to apply seals to almost any component of a LIM currently using an elastomeric material.

[0043] Furthermore, any elastomeric composition that is compatible for use in the intended fuel cell application and is UV curable may be considered. The elastomeric composition used may then be changed to a polyisobutylene precursor or other suitable composition in addition to the silicone precursor. Also, although UV light with a wavelength in the range of 250 to 500 nm may be preferred for curing certain silicone precursors, other more suitable wavelengths should be considered depending on the composition used.

[0044] As for the hardware used in the present method, it is contemplated to use any flexible PTFE and / or polystyrene sheet as defined above, for example by using reinforcements made of glass beads or fibers. However, in exemplary embodiments, an acceptable thickness appears to be 0.5 mm to 3 mm. The depth of the cavity used in such a sheet (and therefore the size of the seal formed) can be about 0.3 to 1.5 mm. And, for the UV-permeable clamping block, a variety of materials (e.g., PMMA or glass) and thicknesses can be considered, as long as it allows sufficient UV transmission therethrough and is mechanically and chemically suitable for clamping, compression and injection purposes.

[0045] Those skilled in the art will appreciate that many other variations besides the foregoing are possible while still obtaining the benefits of the present invention.

[0046] The following examples are illustrative of the present invention but should not be construed as limiting in any way.

[0047] Examples

[0048] In the following, we try to prepare Figure 1a and 1b Multiple segments of bipolar separators with integrated silicone elastomer seals similar to those shown in . The imperforate plate segments are all taken from the end of a single flow field plate and therefore include all seals in and around the fluid ports. The imperforate plate segments are resin impregnated expanded graphite foils of approximately 500×200×1.4 mm in size.

[0049] PIB was used as the elastomer precursor, and the groove depth in each mold cavity used was about 0.25 mm deep. During injection molding, compressive pressures of about several hundred pounds (as opposed to the tons typically used in LIM molding) were used to clamp the components together. UV light with an average wavelength of about 405 nm was irradiated around the injection port and through the mold and clamping block for about 30 seconds to cure the injected elastomer samples.

[0050] Comparative Examples

[0051] As suggested in the prior art, attempts were made to use a mold made of PMMA and a PTFE release spray to prepare a substantially Figures 2a to 2e The separator section with integrated sealant shown in . The PMMA mold is about 6.4 mm thick and has a 0.6 mm deep groove cavity for the sealant formed therein. An aluminum block is used as a support and the sample is prepared by injecting the sealant material until the cavity is full and then curing the sealant. When the separator section is removed from the mold, partial delamination of the applied sealant occurs.

[0052] Examples of the present invention

[0053] According to the present invention and generally as Figures 2a to 2e As shown in, four exemplary separator sections with integrated seals are prepared. Two of the exemplary sections are made of expanded graphite, which is stamped and impregnated with resin, and the resin is cured to make a rigid part. The other two samples are made of carbon particles, which are melted with resin in a heated compression molding process. Here, a 2.0mm PTFE sheet is used as a flexible sheet, in which a 0.6mm deep groove cavity for sealing is formed. The clamping block used is a 32mm thick PMMA, and an aluminum block is used as a support. In each case, the seal is injected until the cavity is full, and then the UV light is used to cure the sealing material. The separator section with the applied flexible sheet is then removed from the mold and the separator section is placed on a flat surface. The flexible sheet is slowly bent upward from a corner, after which the flexible sheet is cleanly separated from the separator section, and the seal is completely integrated on the separator section.

[0054] Except using 2.0mm polystyrene sheet to replace PTFE sheet as flexible sheet, prepare other exemplary separator section with integrated seal in a similar manner to the foregoing.Equally, in each case, inject seal until cavity is full.Then the separator section with applied flexible sheet is removed from mold and placed on a flat surface.Flexible sheet is slowly bent upwards from a corner, after which the flexible sheet is once again cleanly separated from the separator section, and the seal is completely integrated on the separator section simultaneously.

[0055] All of the above U.S. patents, U.S. patent application publications, U.S. patent applications, foreign patents, foreign patent applications, and non-patent publications mentioned in this specification are incorporated herein by reference in their entirety.

[0056] Although specific elements, embodiments and applications of the present invention have been shown and described, it will of course be understood that the present invention is not limited thereto, since modifications may be made by those skilled in the art without departing from the spirit and scope of the present disclosure, particularly in light of the foregoing teachings. Such modifications are considered to be within the purview and scope of the appended claims.

Claims

1. A method for manufacturing a fuel cell separator having an integrated elastomeric seal, the method comprising: Obtain a non-porous plate; placing the plate on a support such that a surface of the plate opposite the intended sealing surface is adjacent to the support; placing a mold for the seal against the intended sealing surface of the plate, wherein the mold comprises: A flexible sheet comprising PTFE or polystyrene; a cavity for the seal, the cavity being formed on a surface of the flexible sheet adjacent the intended sealing surface of the panel; and at least one injection port, the at least one injection port being fluidly connected to the cavity; placing a UV transparent clamping block against the mold; compressing the UV-transmissive clamping mass toward the support such that the flexible sheet seals against the intended sealing surface of the panel; injecting a UV-curable elastomeric composition into the injection port and the cavity; shining UV light through the UV-transmissive clamping blocks and through the mold, thereby curing the injected elastomeric composition; removing the clamping block from the mold; and The flexible sheet is peeled off from the plate.

2. The method of claim 1, wherein: The non-porous plate is selected from the group consisting of graphite, expanded graphite, impregnated expanded graphite, porous carbon foam, porous carbon, carbon, carbon composites and metal foils.

3. The method of claim 1, wherein: The thickness of the imperforate plate is 0.1 to 2.0 mm.

4. The method of claim 1, wherein: The thickness of the flexible sheet is 0.5 to 3 mm.

5. The method of claim 1, wherein: The depth of the cavity is 0.3 to 1.5 mm.

6. The method of claim 1, wherein: The UV transparent clamping block is selected from the group consisting of PMMA and glass.

7. The method of claim 1, wherein: The UV curable elastomeric composition is selected from the group consisting of a silicone precursor and a polyisobutylene precursor.

8. The method of claim 1, wherein: The wavelength of the UV light in the irradiating step is in the range of 250 to 500 nm.

9. The method of claim 1, wherein: The fuel cell separator includes ports and a flow field formed on a surface of the imperforate plate.