Alginic acid derivative / organic montmorillonite synergistic stable drug-loaded Pickering emulsion based on oxidation-Ugi reaction and preparation method of drug-loaded Pickering emulsion

Through oxidation-Ugi reaction and wet ball milling technology, a Pickering emulsion in which alginic acid derivatives and organic montmorillonite are synergistically stabilized is prepared, which solves the problems of low bioavailability and poor stability of traditional food preparations and realizes the purification of β-carotene. High encapsulation efficiency and sustained and controlled release effect have significant application value.

CN118766067APending Publication Date: 2024-10-15HAINAN NORMAL UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410779068.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The problems of low bioavailability and poor stability in traditional food preparations, especially the limited research on composite systems of alginate and montmorillonite as drug carriers, especially chemically modified alginic acid derivatives and physical ultrasound modified ones There are few reports on green and stable Pickering emulsions combined with organic montmorillonite.

Method used

A drug-loaded Pickering emulsion synergistically stabilized by alginic acid derivatives and organic montmorillonite was synthesized through the oxidation-Ugi reaction. Ugi was performed using sodium periodate to oxidize alginate, β-mercaptoethylamine, glacial acetic acid, and isocyanatocyclohexane. Four-component reaction, combined with wet ball milling, was used to prepare organic montmorillonite to form Ugi-OSA-SH/OMMT water-dispersed suspension, and a stable Pickering emulsion was prepared through ultrasonic and shear emulsification technology.

Benefits of technology

It achieves high encapsulation efficiency and protection ability for β-carotene, has good sustained and controlled release effect, improves the stability and viscoelasticity of the emulsion, and solves the problems of low bioavailability and poor stability of traditional food preparations. It has high application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118766067A_ABST
    Figure CN118766067A_ABST
Patent Text Reader

Abstract

The invention provides an alginic acid derivative / organic montmorillonite synergistically stable drug-loaded Pickering emulsion based on oxidation-Ugi reaction and a preparation method thereof, and belongs to the technical field of food active factor carrier materials. A sodium periodate specific oxidation reaction and a Ugi four-component reaction are combined together to synthesize amphipathic Ugi-OSA-SH, polyoxyethylene ether is inserted between lamellas of montmorillonite through ball milling to prepare organic montmorillonite OMMT with good interfacial activity, then Ugi-OSA-SH and OMMT are mixed to obtain a Ugi-OSA-SH / OMMT water dispersion suspension, the Ugi-OSA-SH / OMMT water dispersion suspension is used as a Pickering emulsifier, and the Pickering emulsifier is used for preparing a Pickering emulsifier. The Pickering emulsion loaded with food active factors is prepared through high-speed shearing, and the Pickering emulsion has the advantages of being good in stability, high in beta-carotene encapsulation efficiency and protection capacity and good in sustained and controlled release effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of food active factor carrier materials, and in particular relates to a drug-loaded Pickering emulsion based on oxidation-Ugi reaction synergistic stabilization of alginate derivatives / organic montmorillonite and a preparation method thereof. Background Art

[0002] Many fat-soluble bioactive substances in food, such as vitamins, carotenes, flavonoids and polyphenols, especially β-carotene, which belongs to carotenoids, are beneficial to human health, but their application is limited by disadvantages such as low solubility, poor stability and low bioavailability. Pickering emulsion is a good encapsulant that can effectively improve the storage stability of functional active substances and increase their bioavailability. Currently, Pickering emulsion technology has been widely used to encapsulate, protect and deliver hydrophobic bioactive ingredients. The bioactive substances are mixed with the oil phase before emulsion homogenization, and the Pickering emulsion containing the bioactive substances is formed using food-grade solid particles with low toxicity, high biocompatibility and biodegradability. Li et al. (Li MF, He ZY, Li GY, et al. The formation and characterization of antioxidant pickering emulsions: Effect of the interactions between gliadin and chitosan. Food Hydrocolloids, 2019, 90: 482-489.) prepared Pickering emulsions stabilized by gliadin-chitosan nanoparticles with three structures by changing the pH value, and confirmed through accelerated heat storage experiments that the gliadin-chitosan stabilized emulsions encapsulating curcumin can effectively reduce lipid oxidation. Yi et al. (Yi J., Gan C., Wen Z., et al. Development of pea protein and high methoxyl pectin colloidal particles stabilized high internal phase pickering emulsions for β-carotene protection and delivery. Food Hydrocolloids, 2021, 113: 106497.) prepared pea protein isolate (PPI) and high methoxyl pectin (HMP) colloidal particles and used them to stabilize the high internal phase Pickering emulsion loaded with β-carotene. The Pickering emulsion has good storage stability and controlled release performance under the condition of pH = 6.

[0003] Natural alginate (SA) has a large molecular weight, strong hydrophilicity, and a large number of intramolecular and intermolecular hydrogen bonds in its molecular structure, which makes it rigid, limiting its many applications in drug carriers. Studies have shown that the molecular weight of SA will be greatly reduced after being oxidized by sodium periodate, and aldehyde groups with high reactivity will be generated. The generated alginate aldehyde derivative (OSA) not only retains the advantages of SA such as water solubility, low toxicity and biocompatibility, but also shows good biodegradability and better flexibility. Therefore, the development of OSA-based drug carriers for the delivery of hydrophobic drugs has great application value. The Ugi reaction is a multi-component reaction involving four components: ketone or aldehyde, amine, carboxylic acid and isocyanide. It is widely used in drug discovery for the environmentally friendly synthesis of peptides or candidate drugs. It has the advantages of powerful function, simple operation, low cost, simple and efficient, no catalyst, and good atom economy. Since many bioactive molecules and drug molecules contain α-amidoamide structures, the use of Ugi reaction to synthesize some new drugs or new materials has always attracted much attention.

[0004] Montmorillonite (MMT) is known as one of the most promising Pickering emulsion emulsifiers due to its excellent properties, including high specific surface area, high absorption capacity, good rheological properties, chemical inertness and low toxicity. However, natural MMT has extremely strong hydrophilicity. Therefore, modifying MMT is a necessary condition for obtaining a stable Pickering emulsion emulsifier. The existing modification method is to change the wettability of MMT by physical adsorption of MMT by surfactants or polymers or chemically modifying MMT by surfactants. Wang et al. (Wang J., Deng H., Sun Y., et al. Montmorillonite and alginate co-stabilized biocompatible Pickering emulsions with multiple-stimulus tunable rheology. Journal of Colloid and Interface Science, 2020, 562: 529-539) used alginate and MMT to synergistically stabilize a water-in-oil Pickering emulsion with good storage stability and aggregation stability. The results showed that the sodium alginate / MMT composite material was formed by hydrogen bonding and electrostatic forces between sodium alginate and MMT, and the addition of alginate not only increased the viscosity of the emulsion, but also increased the wettability of MMT, making the Pickering emulsion more stable. Kang et al. (Kang Y., Zan Y., Cong Y., et al. A clay-based Pickering nanoemulsion with antibacterial activity. Colloids and Surfaces A: Physicochemical and Engineering Aspects, 2024, 686: 133337) developed a simple method to prepare a Pickering emulsion with chitosan-coated MMT nanosheets. The emulsion exhibited good stability and small size, and had good antibacterial activity.Yang et al. (Yang Z., Wang W., Tai X., et al. Preparation of modified montmorillonite with different quaternary ammonium salts and application in Pickering emulsion. New Journal of Chemistry, 2019, 43: 11543-11548) used quaternary ammonium salts with different carbon chain lengths to organically modify MMT, and used the prepared organic montmorillonite (OMMT) as an emulsifier to obtain Pickering emulsions with different properties. OMMT-stabilized emulsions have smaller emulsion droplets than MMT-stabilized emulsions and show better stability. As the carbon chain length of the modifier increases, the stability of the Pickering emulsion is enhanced. However, to date, research based on SA and MMT composite systems as drug carriers is still limited. In particular, there are few reports on combining chemically modified alginate derivatives with physically ultrasonically modified OMMT to construct green and stable Pickering emulsions as hydrophobic drug carriers. Summary of the invention

[0005] In order to solve the above technical problems, the present invention proposes a drug-loaded Pickering emulsion based on oxidation-Ugi reaction synergistically stabilized alginate derivative / organic montmorillonite and a preparation method thereof.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing a drug-loaded Pickering emulsion based on oxidation-Ugi reaction and synergistic stabilization of alginate derivatives / organic montmorillonite, comprising the following steps:

[0008] (1) adding β-mercaptoethylamine, glacial acetic acid, and isocyanocyclohexane to a sodium periodate oxidized alginate derivative solution in sequence to carry out an Ugi four-component reaction, followed by dilution, precipitation, centrifugation, alcohol washing, re-centrifugation, dialysis, and freeze drying to obtain an oxidized-Ugi reaction alginate derivative Ugi-OSA-SH;

[0009] (2) placing montmorillonite, polyoxyethylene ether and water in a ball mill for ball milling, centrifuging, washing, re-centrifuging and freeze-drying to obtain organic montmorillonite OMMT;

[0010] (3) mixing the oxidized-Ugi reaction alginic acid derivative Ugi-OSA-SH obtained in step (1) with water to obtain a Ugi-OSA-SH aqueous solution, and then adding the organic montmorillonite OMMT obtained in step (2), and obtaining a Ugi-OSA-SH / OMMT aqueous dispersion suspension by ultrasonication and stirring;

[0011] (4) using olive oil containing food active factors as the oil phase and the Ugi-OSA-SH / OMMT aqueous dispersion suspension obtained in step (3) as the aqueous phase, mixing the two and then performing shear emulsification to obtain a drug-loaded Pickering emulsion based on oxidation-Ugi reaction alginate derivative / organic montmorillonite synergistic stabilization;

[0012] There is no order of precedence for steps (1) and (2).

[0013] Preferably, in step (1), the molar ratio of the theoretical aldehyde functional group of the sodium periodate oxidized alginate derivative to β-mercaptoethylamine, glacial acetic acid and isocyanocyclohexane in the sodium periodate oxidized alginate derivative solution is (0.7:1:1:1)-(1:1:1:1).

[0014] Preferably, in step (2), the CEC of the montmorillonite is 1.20 mmol / g; the molecular weight of the polyoxyethylene ether is 1123.51, and the amount of the polyoxyethylene ether used is 1.0-4.0 times the CEC of the montmorillonite.

[0015] Preferably, in step (2), when the amount of montmorillonite used is 2.0-4.0 g, the grinding balls used for ball milling include 2 agate balls with a diameter of 20 mm, 6 agate balls with a diameter of 10 mm, and 10 agate balls with a diameter of 6 mm; the rotation speed of the ball mill is 500 r / min, and the ball milling time is 2 h.

[0016] Preferably, in step (3), the concentration of the Ugi-OSA-SH aqueous solution is 1.0-5.0 mg / mL; and the mass fraction of the organic montmorillonite OMMT in the Ugi-OSA-SH / OMMT aqueous dispersion is 0.5-2.5%.

[0017] Preferably, in step (3), the power of the ultrasound is 100-200W, and the method is probe ultrasound.

[0018] Preferably, in step (4), the concentration of the food active factor in the olive oil containing the food active factor is 1.0-8.0 mg / mL; and the volume ratio of the olive oil containing the food active factor to the Ugi-OSA-SH / OMMT aqueous dispersion suspension is (2:8)-(4:6).

[0019] Preferably, in step (4), the food active factor includes one of β-carotene, lutein, zeaxanthin, astaxanthin and lycopene.

[0020] Preferably, in step (4), the shear emulsification speed is 12000 r / min and the time is 5 min.

[0021] The present invention also provides a drug-loaded Pickering emulsion prepared by the preparation method described in the above technical scheme based on the synergistic stabilization of alginate derivatives / organic montmorillonite by oxidation-Ugi reaction.

[0022] Compared with the prior art, the present invention has the following advantages and technical effects:

[0023] The present invention organically combines the sodium periodate specific oxidation reaction and the Ugi four-component reaction to simply and efficiently synthesize a novel amphiphilic Ugi-OSA-SH. At the same time, a non-toxic nonionic surfactant polyoxyethylene ether is inserted between the lamellae of montmorillonite by simple and fast wet ball milling to prepare an organic montmorillonite OMMT with good interfacial activity. Then, Ugi-OSA-SH and OMMT are mixed to obtain a Ugi-OSA-SH / OMMT water-dispersible suspension, which is used as a Pickering emulsifier to prepare a Pickering emulsion loaded with food active factors by high-speed shearing. The drug-loaded Pickering emulsion prepared by the present invention based on the synergistic stabilization of the oxidation-Ugi reaction alginate derivative / organic montmorillonite has a high encapsulation rate and protection ability for β-carotene, and it has a good sustained-release effect on the coated β-carotene. Moreover, under the condition of a certain Ugi-OSA-SH concentration, as the OMMT concentration increases, the droplet size and emulsion instability coefficient of the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion decrease, and the stability and viscoelasticity increase, indicating that OMMT and Ugi-OSA-SH form a three-dimensional network structure at the oil-water interface, which makes the emulsion highly stable and can keep the emulsion from flowing when inverted. These characteristics of the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion effectively solve the problems of low bioavailability and poor stability of traditional food preparations, and have extremely high application value in the food industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0025] Figure 1 The synthetic route of Ugi-OSA-SH in Examples 1-8 of the present invention;

[0026] Figure 2 is SA, OSA and Ugi-OSA-SH in Example 2 of the present invention 1 HNMR spectrum;

[0027] Figure 3 FT-IR spectra of SA, OSA and Ugi-OSA-SH in Example 2 of the present invention (a) and FT-IR spectra of OMMT, Ugi-OSA-SH and Ugi-OSA-SH / OMMT (b);

[0028] Figure 4 TEM and SEM images of montmorillonite and OMMT in Example 2 of the present invention;

[0029] Figure 5 XRD spectra of SA, OSA, OMMT, Ugi-OSA-SH and Ugi-OSA-SH / OMMT in Example 2;

[0030] Figure 6 It is a curve diagram of particle size and Zeta potential change of the Ugi-OSA-SH / OMMT water dispersion suspension in Example 2, Examples 5-8 and Comparative Example 1;

[0031] Figure 7 is the creaming index of the Ugi-OSA-SH / OMMT stable emulsions of Example 2, Examples 5-8 and Comparative Example 1;

[0032] Figure 8 The actual pictures are of the Ugi-OSA-SH / OMMT stable emulsions of Example 2, Examples 5-8 and Comparative Example 1 after being left to stand for different time periods;

[0033] Fig. 9 The centrifugal stability of the Ugi-OSA-SH / OMMT stable emulsions of Example 2, Examples 5-8 and Comparative Example 1;

[0034] Fig.10 The graph is a relationship between the instability coefficient and time of the Ugi-OSA-SH / OMMT stable emulsions of Example 2, Examples 5-8 and Comparative Example 1;

[0035] Fig.11 It is a microscope picture of the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion in Example 2, Examples 5-8 and Comparative Example 1;

[0036] Fig.12 The SEM images of the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsions in Example 2, Examples 5-8 and Comparative Example 1;

[0037] Fig.13 The rheological properties of the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsions in Example 2, Examples 5-8 and Comparative Example 1;

[0038] Fig.14 The encapsulation efficiency curve (a) and drug release kinetics curve (b) of β-carotene by the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion in Examples 7-8 are shown. DETAILED DESCRIPTION

[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0041] The embodiment of the present invention provides a method for preparing a drug-loaded Pickering emulsion based on oxidation-Ugi reaction synergistically stabilized alginate derivative / organic montmorillonite, comprising the following steps:

[0042] (1) adding β-mercaptoethylamine, glacial acetic acid, and isocyanocyclohexane to a sodium periodate oxidized alginate derivative solution in sequence to carry out an Ugi four-component reaction, followed by dilution, precipitation, centrifugation, alcohol washing, re-centrifugation, dialysis, and freeze drying to obtain an oxidized-Ugi reaction alginate derivative Ugi-OSA-SH;

[0043] (2) placing montmorillonite, polyoxyethylene ether and water in a ball mill for ball milling, centrifuging, washing, re-centrifuging and freeze-drying to obtain organic montmorillonite OMMT;

[0044] (3) mixing the oxidized-Ugi reaction alginic acid derivative Ugi-OSA-SH obtained in step (1) with water to obtain a Ugi-OSA-SH aqueous solution, and then adding the organic montmorillonite OMMT obtained in step (2), and obtaining a Ugi-OSA-SH / OMMT aqueous dispersion suspension by ultrasonication and stirring;

[0045] (4) using olive oil containing food active factors as the oil phase and the Ugi-OSA-SH / OMMT aqueous dispersion suspension obtained in step (3) as the aqueous phase, mixing the two and then performing shear emulsification to obtain a drug-loaded Pickering emulsion based on oxidation-Ugi reaction alginate derivative / organic montmorillonite synergistic stabilization;

[0046] There is no order of precedence for steps (1) and (2).

[0047] In a preferred embodiment, in step (1), the preparation method of the sodium periodate oxidized alginate derivative comprises the following steps: dissolving 5 g of sodium alginate SA in 200 mL of distilled water, adding 50 mL of anhydrous ethanol and mixing evenly, then adding sodium periodate, stirring electrically in the dark for 24 h at room temperature, then adding 10 mL of ethylene glycol, stirring magnetically in the dark for 2 h to terminate the reaction; precipitating the reaction solution with 5 g of sodium chloride and 800 mL of anhydrous ethanol, then re-dissolving the obtained precipitate in 100 mL of distilled water, and then precipitating with 3 g of sodium chloride and 600 mL of anhydrous ethanol, repeating the precipitation 3 times, and placing the obtained solution into a dialysis bag with a molecular weight cutoff of 3500 for 5 days, and freeze-drying to obtain the sodium periodate oxidized alginate derivative OSA.

[0048] In a preferred embodiment, the mass average molecular weight Mw of the sodium alginate is ≤200000, and the molar ratio of guluronic acid (G) to mannuronic acid (M) in the sodium alginate is G / M ≤1.0.

[0049] In a preferred embodiment, the amount of sodium periodate used is 30% of the molar amount of uronic acid monomer in sodium alginate.

[0050] In a preferred embodiment, the theoretical oxidation degree of the alginate derivative OSA oxidized by sodium periodate is 10-30%.

[0051] In a preferred embodiment, in step (1), the molar ratio of the theoretical aldehyde functional group of the sodium periodate oxidized alginate derivative to β-mercaptoethylamine, glacial acetic acid and isocyanocyclohexane in the sodium periodate oxidized alginate derivative solution is (0.7:1:1:1)-(1:1:1:1). The β-mercaptoethylamine in the present invention has the advantages of safety, non-toxicity and high coupling activity. The β-mercaptoethylamine is reacted with the sodium periodate oxidized alginate derivative, glacial acetic acid and isocyanocyclohexane in the Ugi four-component reaction, which is conducive to obtaining amphiphilic Ugi-OSA-SH.

[0052] In a preferred embodiment, in step (1), the degree of substitution of the alginate derivative Ugi-OSA-SH produced by the oxidation-Ugi reaction is 18-28%.

[0053] In a preferred embodiment, the calculation formula for the degree of substitution of the oxidative-Ugi reaction alginate derivative Ugi-OSA-SH is:

[0054]

[0055] Among them, α is the content ratio of N / C, M C and M N are the relative atomic masses of C and N respectively.

[0056] In a preferred embodiment, in step (1), the reagent used for dilution is distilled water; the reagent used for precipitation is anhydrous ethanol; the molecular weight cutoff of the dialysis bag used for dialysis is 3500, and the dialysis time is 3 days; the temperature of freeze-drying is -60 to -50°C, and the time is 48 hours.

[0057] In a preferred embodiment, in step (2), the CEC of the montmorillonite is 1.20 mmol / g. The present invention uses montmorillonite with a CEC in the above range, which has the advantages of high surface area, high absorption capacity and low toxicity.

[0058] In a preferred embodiment, in step (2), the molecular weight of the polyoxyethylene ether is 1123.51, and the amount of the polyoxyethylene ether used is 1.0-4.0 times that of montmorillonite CEC.

[0059] In a preferred embodiment, in step (2), the volume ratio of the mass of the montmorillonite to water is 2.0-4.0 g:10 mL.

[0060] In a preferred embodiment, in step (2), when the amount of montmorillonite used is 2.0-4.0 g, the grinding balls used for ball milling include 2 agate balls with a diameter of 20 mm, 6 agate balls with a diameter of 10 mm, and 10 agate balls with a diameter of 6 mm.

[0061] In a preferred embodiment, in step (2), the rotation speed of the ball mill is 500 r / min, the ball milling time is 2 h, and the ball milling equipment is a PM type planetary ball mill.

[0062] In a preferred embodiment, in step (2), the centrifugal speed is 8000 r / min and the time is 10 min; the washing reagent is deionized water; the re-centrifugal speed is 8000 r / min and the time is 10 min; the freeze-drying temperature is -60 to -50°C and the time is 48 h.

[0063] In a preferred embodiment, in step (3), the concentration of the Ugi-OSA-SH aqueous solution is 1.0-5.0 mg / mL; and the mass fraction of the organic montmorillonite OMMT in the Ugi-OSA-SH / OMMT aqueous dispersion is 0.5-2.5%.

[0064] In a preferred embodiment, in step (3), the power of the ultrasound is 100-200 W, the method is probe ultrasound, and the time is 30 minutes.

[0065] In a preferred embodiment, in step (3), the stirring method is magnetic stirring.

[0066] In a preferred embodiment, in step (4), the concentration of the food active factor in the olive oil containing the food active factor is 1.0-8.0 mg / mL; the volume ratio of the olive oil containing the food active factor to the Ugi-OSA-SH / OMMT aqueous dispersion suspension is (2:8)-(4:6).

[0067] In a preferred embodiment, in step (4), the food active factor includes one of β-carotene, lutein, zeaxanthin, astaxanthin and lycopene.

[0068] In a preferred embodiment, in step (4), the shear emulsification is carried out at a rotation speed of 12000 r / min and for a time of 5 min.

[0069] The present invention also provides a drug-loaded Pickering emulsion prepared by the preparation method described in the above technical scheme based on the synergistic stabilization of alginate derivatives / organic montmorillonite by oxidation-Ugi reaction.

[0070] The drug-loaded Pickering emulsion based on oxidation-Ugi reaction and synergistic stabilization of alginate derivatives / organic montmorillonite provided by the present invention has high stability, high encapsulation rate and protection ability for food active factors, and good sustained-release effect, effectively solving the problems of low bioavailability and poor stability of traditional food preparations, and has extremely high application value in the field of food industry.

[0071] The room temperature in the embodiments of the present invention refers to "25±2°C".

[0072] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources.

[0073] Example 1

[0074] A method for preparing a drug-loaded Pickering emulsion based on oxidation-Ugi reaction and synergistic stabilization of alginate derivatives / organic montmorillonite:

[0075] (1) 5 g of sodium alginate SA was dissolved in 200 mL of distilled water, and then 50 mL of anhydrous ethanol was added to mix evenly, and then 1.62 g (30% molar amount of sodium alginate uronic acid monomer) of sodium periodate was added, and the mixture was stirred electrically in the dark for 24 h at room temperature, and then 10 mL of ethylene glycol was added, and the reaction was terminated by magnetic stirring in the dark for 2 h; the solution after the reaction was precipitated with 5 g of sodium chloride and 800 mL of anhydrous ethanol, and then the precipitate was redissolved in 100 mL of distilled water, and then precipitated with 3 g of sodium chloride and 600 mL of anhydrous ethanol. After repeating the precipitation for 3 times, the resulting solution was placed in a dialysis bag with a molecular weight cutoff of 3500, dialyzed for 5 days, and freeze-dried to obtain a sodium periodate oxidized alginate derivative OSA with a theoretical oxidation degree of 30%;

[0076] (2) 2.0 g (containing 10.1 mmol uronic acid monomer) of the sodium periodate oxidized alginate derivative OSA obtained in step (1) was placed in a 250 mL round-bottom flask, 100 mL of distilled water was added, and the OSA was dissolved into a homogeneous solution by stirring to obtain a sodium periodate oxidized alginate derivative solution with an OSA mass fraction of 2.0%; 8.48 mmol (0.65 g) of β-mercaptoethylamine was added to the above sodium periodate oxidized alginate derivative solution, and the reaction was stirred for 30 min, and then 8.48 mmol (0.49 mL) of glacial acetic acid was added to make it uniformly dispersed in the solution, and finally 8.48 mmol (0.93 g) of dense The reaction mixture was stirred at room temperature for 24 hours and then diluted with 50 mL of distilled water. Then, 5 times the volume of anhydrous ethanol was added to precipitate the reaction product. The precipitated product was centrifuged, washed with alcohol, and centrifuged again before being loaded into a dialysis bag with a molecular weight cutoff of 3500. The product was dialyzed in double distilled water for 3 days to remove residual small molecular impurities, and then freeze-dried at -60°C for 48 hours to obtain Ugi-OSA-SH with a degree of substitution of 27.5%.

[0077] (3) 2.0 g of dry montmorillonite with a CEC of 1.20 mmol / g was placed in a 50 mL ball mill, and then 5.39 g of polyoxyethylene ether (the molecular weight of polyoxyethylene ether is 1123.51, and the amount is 2.0 times the CEC of montmorillonite) and 10 mL of deionized water were added. Then, 2 agate balls with a diameter of 20 mm, 6 agate balls with a diameter of 10 mm, and 10 agate balls with a diameter of 6 mm were added. The ball mill was then placed in a PM planetary ball mill and the main disc speed was 500 r / min. The montmorillonite was modified by wet ball milling under the condition of ball milling for 2 hours; after the modification, the reaction solution was transferred into a beaker, and then the ball mill and the agate ball were washed with deionized water to obtain a washing solution; the reaction solution and the washing solution were collected together, centrifuged at high speed (8000r / min) for 10 minutes, the upper clear liquid was removed, the lower precipitate was repeatedly washed with deionized water, and centrifuged at high speed again, and the operation was repeated for more than 3 times to remove the residual modifier, and then freeze-dried at -60°C for 48 hours to obtain dry OMMT;

[0078] (4) mixing the Ugi-OSA-SH with a substitution degree of 27.5% obtained in step (2) with water to prepare a Ugi-OSA-SH aqueous solution with a mass concentration of 2.0 mg / mL, and then adding the organic montmorillonite OMMT obtained in step (3) to make the mass fraction of OMMT in the Ugi-OSA-SH / OMMT aqueous dispersion suspension be 1.0%, ultrasonically treating at 100 W for 30 min, and magnetically stirring overnight to obtain a Ugi-OSA-SH / OMMT aqueous dispersion suspension;

[0079] (5) Using olive oil containing β-carotene as the oil phase (the concentration of β-carotene is 1.0 mg / mL) and the Ugi-OSA-SH / OMMT aqueous dispersion suspension obtained in step (4) as the aqueous phase, the two are mixed in a volume ratio of 3:7, and then shear emulsified at 12000 r / min at room temperature for 5 min using a high-speed shear emulsifier to obtain a drug-loaded Pickering emulsion based on oxidation-Ugi reaction of alginate derivative / organic montmorillonite synergistically stabilized, recorded as Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion.

[0080] Example 2

[0081] A method for preparing a drug-loaded Pickering emulsion based on oxidation-Ugi reaction and synergistic stabilization of alginate derivatives / organic montmorillonite:

[0082] (1) 5 g of sodium alginate SA was dissolved in 200 mL of distilled water, and then 50 mL of anhydrous ethanol was added to mix evenly, and then 1.08 g (20% molar amount of sodium alginate uronic acid monomer) of sodium periodate was added, and the mixture was stirred electrically in the dark for 24 h at room temperature, and then 10 mL of ethylene glycol was added, and the reaction was terminated by magnetic stirring in the dark for 2 h; the solution after the reaction was precipitated with 5 g of sodium chloride and 800 mL of anhydrous ethanol, and then the precipitate was redissolved in 100 mL of distilled water, and then precipitated with 3 g of sodium chloride and 600 mL of anhydrous ethanol. After repeating the precipitation for 3 times, the obtained solution was loaded into a dialysis bag with a molecular weight cutoff of 3500, dialyzed for 5 days, and freeze-dried to obtain a sodium periodate oxidized alginate derivative OSA with a theoretical oxidation degree of 20%;

[0083] (2) 2.0 g (containing 10.1 mmol uronic acid monomer) of the sodium periodate oxidized alginate derivative OSA obtained in step (1) was placed in a 250 mL round-bottom flask, 100 mL of distilled water was added, and the OSA was dissolved into a homogeneous solution by stirring to obtain a sodium periodate oxidized alginate derivative solution with an OSA mass fraction of 2.0%; 4.85 mmol (0.37 g) of β-mercaptoethylamine was added to the above sodium periodate oxidized alginate derivative solution, and the reaction was stirred for 30 min, and then 4.85 mmol (0.28 mL) of glacial acetic acid was added to make it uniformly dispersed in the solution, and finally 4.85 mmol (0.53 g) of dense The reaction mixture was stirred at room temperature for 24 hours and then diluted with 50 mL of distilled water. Then, 5 times the volume of anhydrous ethanol was added to precipitate the reaction product. The precipitated product was centrifuged, washed with alcohol, and centrifuged again before being loaded into a dialysis bag with a molecular weight cutoff of 3500. The product was dialyzed in double distilled water for 3 days to remove residual small molecular impurities, and then freeze-dried at -60°C for 48 hours to obtain Ugi-OSA-SH with a degree of substitution of 18.6%.

[0084] (3) 2.0 g of dry montmorillonite with a CEC of 1.20 mmol / g was placed in a 50 mL ball mill, and then 2.69 g of polyoxyethylene ether (the molecular weight of polyoxyethylene ether is 1123.51, and the amount is 1.0 times the CEC of montmorillonite) and 10 mL of deionized water were added. Then, 2 agate balls with a diameter of 20 mm, 6 agate balls with a diameter of 10 mm, and 10 agate balls with a diameter of 6 mm were added. The ball mill was then placed in a PM planetary ball mill and the main disc speed was 500 r / min. The montmorillonite was modified by wet ball milling under the condition of ball milling time of 2 hours; after the modification, the reaction solution was transferred into a beaker, and then the ball mill and the agate ball were washed with deionized water to obtain a washing solution; the reaction solution and the washing solution were collected together, centrifuged at high speed (8000r / min) for 10 minutes, the upper clear liquid was removed, the lower precipitate was repeatedly washed with deionized water, and centrifuged at high speed again, and the operation was repeated for more than 3 times to remove the residual modifier, and then freeze-dried at -60°C for 48 hours to obtain dry OMMT;

[0085] (4) mixing the Ugi-OSA-SH having a substitution degree of 18.6% obtained in step (2) with water to prepare a Ugi-OSA-SH aqueous solution having a mass concentration of 1.0 mg / mL, and then adding the organic montmorillonite OMMT obtained in step (3) to make the mass fraction of OMMT in the Ugi-OSA-SH / OMMT aqueous dispersion suspension be 1.0%, ultrasonically treating at 100 W for 30 min, and magnetically stirring overnight to obtain a Ugi-OSA-SH / OMMT aqueous dispersion suspension;

[0086] (5) Using olive oil containing β-carotene (the concentration of β-carotene is 1.0 mg / mL) as the oil phase and the Ugi-OSA-SH / OMMT aqueous dispersion suspension obtained in step (4) as the aqueous phase, the two are mixed in a volume ratio of 3:7, and then shear emulsified at 12000 r / min at room temperature for 5 min using a high-speed shear emulsifier to obtain a drug-loaded Pickering emulsion synergistically stabilized by an oxidation-Ugi reaction of alginate derivatives / organic montmorillonite, which is recorded as Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion.

[0087] Example 3

[0088] A method for preparing a drug-loaded Pickering emulsion based on oxidation-Ugi reaction and synergistic stabilization of alginate derivatives / organic montmorillonite:

[0089] Steps (1)-(2) are the same as in Example 2;

[0090] (3) 2.0 g of dry montmorillonite with a CEC of 1.20 mmol / g was placed in a 50 mL ball mill, and then 5.39 g of polyoxyethylene ether (the molecular weight of polyoxyethylene ether is 1123.51, and the amount is 2.0 times the CEC of montmorillonite) and 10 mL of deionized water were added. Then, 2 agate balls with a diameter of 20 mm, 6 agate balls with a diameter of 10 mm, and 10 agate balls with a diameter of 6 mm were added. The ball mill was then placed in a PM planetary ball mill and the main disc speed was 500 r / min. The montmorillonite was modified by wet ball milling under the condition of ball milling for 2 hours; after the modification, the reaction solution was transferred into a beaker, and then the ball mill and the agate ball were washed with deionized water to obtain a washing solution; the reaction solution and the washing solution were collected together, centrifuged at high speed (8000r / min) for 10 minutes, the upper clear liquid was removed, the lower precipitate was repeatedly washed with deionized water, and centrifuged at high speed again, and the operation was repeated for more than 3 times to remove the residual modifier, and then freeze-dried at -60°C for 48 hours to obtain dry OMMT;

[0091] (4) mixing the Ugi-OSA-SH having a degree of substitution of 18.6% obtained in step (2) with water to prepare a Ugi-OSA-SH aqueous solution having a mass concentration of 1.0 mg / mL, and then adding the organic montmorillonite OMMT obtained in step (3) to make the mass fraction of OMMT in the Ugi-OSA-SH / OMMT aqueous dispersion suspension be 2.0%, ultrasonically treating at 100 W for 30 min, and magnetically stirring overnight to obtain a Ugi-OSA-SH / OMMT aqueous dispersion suspension;

[0092] (5) Using olive oil containing β-carotene (the concentration of β-carotene is 1.0 mg / mL) as the oil phase and the Ugi-OSA-SH / OMMT aqueous dispersion suspension obtained in step (4) as the aqueous phase, the two are mixed in a volume ratio of 4:6, and then shear emulsified at 12000 r / min at room temperature for 5 min using a high-speed shear emulsifier to obtain a drug-loaded Pickering emulsion based on oxidation-Ugi reaction of alginate derivative / organic montmorillonite synergistically stabilized, recorded as Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion.

[0093] Example 4

[0094] A method for preparing a drug-loaded Pickering emulsion based on oxidation-Ugi reaction and synergistic stabilization of alginate derivatives / organic montmorillonite:

[0095] Steps (1)-(2) are the same as in Example 1;

[0096] (3) 2.0 g of dry montmorillonite with a CEC of 1.20 mmol / g was placed in a 50 mL ball mill, and then 2.69 g of polyoxyethylene ether (the molecular weight of polyoxyethylene ether is 1123.51, and the amount is 1.0 times the CEC of montmorillonite) and 10 mL of deionized water were added. Then, 2 agate balls with a diameter of 20 mm, 6 agate balls with a diameter of 10 mm, and 10 agate balls with a diameter of 6 mm were added. The ball mill was then placed in a PM planetary ball mill and the main disc speed was 500 r / min. The montmorillonite was modified by wet ball milling under the condition of ball milling time of 2 hours; after the modification, the reaction solution was transferred into a beaker, and then the ball mill and the agate ball were washed with deionized water to obtain a washing solution; the reaction solution and the washing solution were collected together, centrifuged at high speed (8000r / min) for 10 minutes, the upper clear liquid was removed, the lower precipitate was repeatedly washed with deionized water, and centrifuged at high speed again, and the operation was repeated for more than 3 times to remove the residual modifier, and then freeze-dried at -60°C for 48 hours to obtain dry OMMT;

[0097] (4) mixing the Ugi-OSA-SH having a degree of substitution of 27.5% obtained in step (2) with water to prepare a Ugi-OSA-SH aqueous solution having a mass concentration of 3.0 mg / mL, and then adding the organic montmorillonite obtained in step (3) so that the mass fraction of OMMT in the Ugi-OSA-SH / OMMT aqueous dispersion suspension is 2.0%, ultrasonicating at 100 W for 30 min, and magnetically stirring overnight to obtain a Ugi-OSA-SH / OMMT aqueous dispersion suspension;

[0098] (5) Using olive oil containing β-carotene (the concentration of β-carotene is 1.0 mg / mL) as the oil phase and the Ugi-OSA-SH / OMMT aqueous dispersion suspension obtained in step (4) as the aqueous phase, the two are mixed in a volume ratio of 4:6, and then shear emulsified at 12000 r / min at room temperature for 5 min using a high-speed shear emulsifier to obtain a drug-loaded Pickering emulsion based on oxidation-Ugi reaction of alginate derivative / organic montmorillonite synergistically stabilized, recorded as Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion.

[0099] Example 5

[0100] The only difference from Example 2 is that in step (4), the mass fraction of OMMT in the Ugi-OSA-SH / OMMT aqueous dispersion suspension is 0.05%.

[0101] Example 6

[0102] The only difference from Example 2 is that in step (4), the mass fraction of OMMT in the Ugi-OSA-SH / OMMT aqueous dispersion suspension is 0.1%.

[0103] Example 7

[0104] The only difference from Example 2 is that in step (4), the mass fraction of OMMT in the Ugi-OSA-SH / OMMT aqueous dispersion suspension is 0.5%.

[0105] Example 8

[0106] The only difference from Example 2 is that in step (4), the mass fraction of OMMT in the Ugi-OSA-SH / OMMT aqueous dispersion suspension is 1.5%.

[0107] Comparative Example 1

[0108] The difference from Example 2 is that in step (4), the mass fraction of OMMT in the Ugi-OSA-SH / OMMT aqueous dispersion suspension is 0%.

[0109] Figure 1 The synthetic route of Ugi-OSA-SH in Examples 1-8 of the present invention is shown in FIG. Figure 1 It can be seen that the present invention first uses sodium periodate to oxidize alginate to obtain sodium periodate oxidized alginate derivative OSA, and then adds β-mercaptoethylamine, glacial acetic acid, and isocyanocyclohexane in sequence to carry out Ugi reaction, thereby obtaining amphiphilic Ugi-OSA-SH.

[0110] Figure 2 is the SA, OSA and Ugi-OSA-SH in Example 2 1 H NMR spectrum. Figure 2 It can be seen that the chemical shift δ between 5.0-3.5 belongs to the proton signal peak of the SA main chain. 1 It can be seen from the HNMR spectrum that there are two more characteristic signal peaks at 5.3 and 5.6 ppm compared with SA, which is attributed to the two hydroxyl groups of sodium alginate being oxidized to form aldehyde groups, and hemiacetal is formed between the aldehyde groups and the adjacent hydroxyl groups, which is a characteristic signal peak of the aldehyde group, indicating that OSA was successfully prepared using sodium periodate. Compared with the NMR spectrum of OSA, Ugi-OSA-SH has new proton signal peaks at δ1.9~1.3ppm and 1.20~0.9ppm, which are attributed to the proton signal peaks of -CH2- on β-mercaptoethylamine and cyclohexyl isonitrile, respectively. This spectrum shows that the Ugi reaction successfully grafted β-mercaptoethylamine and cyclohexyl isonitrile onto OSA to synthesize Ugi-OSA-SH.

[0111] Figure 3FT-IR spectra of SA, OSA and Ugi-OSA-SH in Example 2 and FT-IR spectra of OMMT, Ugi-OSA-SH and Ugi-OSA-SH / OMMT. Figure 3 It can be seen that compared with the absorption peak of SA, OSA has a peak at 1735 cm -1 A new characteristic absorption peak appears at 3426cm -1 The stretching vibration peak of -OH at 2937cm-1 becomes sharper and narrower after oxidation, indicating that the number of -OH groups on the main chain of sodium alginate is reduced. Therefore, it can be shown that sodium periodate successfully oxidizes SA, oxidizing the adjacent hydroxyl groups at C-2 and C-3 to aldehyde groups to obtain OSA. At the same time, compared with the infrared absorption peak of OSA, the peak of Ugi-OSA-SH at 2937cm-1 is -1 The absorption peak at 2852 cm -1 New characteristic peaks appeared at , which were attributed to the stretching vibration of -CH2- on β-mercaptoethylamine and cyclohexyl isocyanide. The changes in these absorption peaks indicate that β-mercaptoethylamine and cyclohexyl isocyanide were successfully grafted onto the main chain of OSA through the Ugi reaction to generate Ugi-OSA-SH. In addition, in the infrared spectrum of Ugi-OSA-SH / OMMT, in addition to the clear characteristic peaks of Ugi-OSA-SH and OMMT, it was also found that the characteristic peak of OMMT was slightly shifted, indicating that hydrogen bonds and electrostatic interactions may have occurred between Ugi-OSA-SH and OMMT.

[0112] Figure 4 TEM and SEM images of montmorillonite and OMMT in Example 2, wherein (A) is a TEM image of montmorillonite and OMMT, and (B) is a SEM image of montmorillonite and OMMT. Figure 4 It can be seen that the raw material montmorillonite exhibits dense and regular layered lattice stripes, and its interlayer spacing is about 1.2nm. The OMMT layers are stretched and the interlayer spacing increases. This is because the intercalation of polyoxyethylene ether weakens the interaction force (hydrogen bonding) between the layers. In addition, Figure 4 (A) It can be seen that after ball milling modification, the flake structure and block structure of OMMT are significantly reduced, and a fine particle structure appears. The results show that ball milling modification has a certain pulverization effect on montmorillonite particles and successfully inserts polyoxyethylene ether into the montmorillonite layer.

[0113] Figure 5 The XRD spectra of SA, OSA, OMMT, Ugi-OSA-SH and Ugi-OSA-SH / OMMT in Example 2 are shown in FIG. Figure 5It can be seen that the structures of all the tested samples are amorphous structures. Compared with the two weak and broad diffraction peaks of SA, the two peaks of OSA are shifted to 2θ=14.9° and 23.0°, and the diffraction peak at 2θ=23.0° is wider. However, Ugi-OSA-SH only has a wider diffraction peak at 2θ=25°. This shows that after the modification of Ugi-OSA-SH, the hydrogen bonds in the molecules are destroyed and the crystal diffraction peaks are transformed. In addition, the diffraction peaks of OMMT and Ugi-OSA-SH can be found in the curve of Ugi-OSA-SH / OMMT, proving the formation of Ugi-OSA-SH / OMMT composite particles.

[0114] Figure 6 The particle size and Zeta potential change curves of the Ugi-OSA-SH / OMMT water-dispersible suspension in Example 2, Examples 5-8 and Comparative Example 1 (Ugi-OSA-SH concentration is 1.0 mg / mL), wherein (a) is a particle size change curve measured by a Malvern laser particle size analyzer, and (b) is a Zeta potential change curve. Figure 6 It can be seen that since Ugi-OSA-SH has hydrophilic and hydrophobic properties, it can self-assemble to form micelles in the aqueous phase, so the particle size of Comparative Example 1 is relatively large. As the concentration of OMMT increases, more and more Ugi-OSA-SH is adsorbed on the surface of OMMT to form Ugi-OSA-SH / OMMT composite nanoparticles, and its adsorption stability is enhanced. The electrostatic repulsion between particles is getting stronger and stronger, preventing the agglomeration between particles, so the particle size becomes smaller. In addition, all the Zeta potential values ​​of the water-dispersed suspensions are negative, and as the concentration of OMMT increases, the absolute value of the Zeta potential gradually increases. This may be because more Ugi-OSA-SH / OMMT composite nanoparticles lead to an increase in the surface charge density of the droplets, which is conducive to increasing the electrostatic repulsion between the droplets and enhancing the interfacial stability of the droplets. Therefore, the smaller the particle size of the Ugi-OSA-SH / OMMT composite particles, the greater the favorable factors provided for the stability of the Pickering emulsion.

[0115] The Ugi-OSA-SH / OMMT aqueous dispersion suspensions in Example 2, Examples 5-8 and Comparative Example 1 were subjected to high-speed shear emulsification to prepare Ugi-OSA-SH / OMMT stable Pickering emulsions.

[0116] Figure 7 It is the creaming index of the Ugi-OSA-SH / OMMT stable emulsion of Example 2, Examples 5-8 and Comparative Example 1.

[0117] Figure 8The following are the actual pictures of the Ugi-OSA-SH / OMMT stable emulsions of Example 2, Examples 5-8 and Comparative Example 1 after being left standing for different time periods, wherein (A) is left standing for 3 hours, (B) is left standing for 1 day, (C) is left standing for 30 days, and (D) is left standing in an inverted state for 30 days. Figure 7 and Figure 8 It can be seen that when the OMMT concentration is less than 1.0wt%, the stable emulsion undergoes a rapid stratification effect in the first 3 hours after the emulsion shear is completed, and then the phase separation rate weakens. When the OMMT concentration is greater than 1.0wt%, the stable emulsion undergoes a smaller phase separation after 12 hours. And all emulsions basically reached a stable state within 1 day. In addition, after the vials containing the emulsions were inverted after 30 days, all emulsions showed gel-like properties and maintained high stability. This may be because more Ugi-OSA-SH / OMMT composite particles are adsorbed at the oil-water interface to form a three-dimensional network structure, which prevents droplet aggregation and Ostwald ripening, weakens emulsion separation, significantly reduces the proportion of the water layer, and increases the stability of the emulsion. Therefore, a higher concentration of OMMT can not only improve the static stability of the emulsion, but also increase the viscosity of the emulsion.

[0118] The dynamic changes of infrared transmittance of the Ugi-OSA-SH / OMMT stable emulsions of Example 2, Examples 5-8 and Comparative Example 1 were recorded by a full-function stability analyzer LUMiSize to characterize the centrifugal stability of the emulsions. The results are as follows: Fig. 9 shown.

[0119] Fig.10 The graphs are the relationship between the instability coefficient and time of the Ugi-OSA-SH / OMMT stable emulsions of Example 2, Examples 5-8 and Comparative Example 1. Fig. 9 and Fig.10 It can be seen that the higher the concentration of OMMT in the emulsion, the smaller the range of its infrared transmittance change, the larger the stable area in the middle of the emulsion, and the smaller the instability coefficient. This shows that the more OMMT there is, the more Ugi-OSA-SH / OMMT composite particles are formed, the larger the particle size concentration, the smaller the emulsion droplets, and the better the stability of the formed emulsion.

[0120] Fig.11 The microscopic images of the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsions in Example 2, Examples 5-8 and Comparative Example 1. Fig.11It can be seen that with the increase of OMMT, the droplet size of the emulsion gradually decreases and the size tends to be uniform. This is because with the increase of OMMT concentration, the concentration of Ugi-OSA-SH / OMMT composite nanoparticles in the dispersion gradually increases. This is because the stability of the oil-water interface requires a certain number of nanoparticles. When the concentration of Ugi-OSA-SH / OMMT nanoparticles is small, it can only stabilize a limited oil-water interface, so only larger droplets can be formed. On the contrary, more composite nanoparticles are conducive to stabilizing a larger oil-water interface, thereby forming smaller droplets to increase the total oil-water interface, achieve full coverage of all droplet surfaces, and enhance the formation ability and stability of the emulsion. A large amount of experimental data proves that the smaller the droplet size, the better the stability of the emulsion.

[0121] Styrene containing 2.0 mol% AIBN was used as the oil phase to replace the olive oil containing β-carotene in Example 2, Examples 5-8 and Comparative Example 1, and the emulsion droplets were solidified. The microstructure of the Ugi-OSA-SH / OMMT particles stabilized at the oil-water interface was observed using SEM. Figure 12 is the SEM image of the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion in Example 2, Examples 5-8 and Comparative Example 1 (styrene containing 2.0 mol% AIBN as the oil phase). Fig.12 It can be seen that the Pickering emulsion stabilized only by Ugi-OSA-SH colloidal particles has a low coverage on the droplet surface. With the increase of OMMT concentration, it can be clearly observed that Ugi-OSA-SH / OMMT particles are adsorbed and arranged in a dense, uniform and orderly manner on the surface of styrene oil droplets. It can be seen that OMMT can effectively reduce the size of emulsion droplets and enhance the physical stability of Pickering emulsions by increasing the concentration of emulsifier adsorbed at the oil-water interface.

[0122] Fig.13 The rheological properties of the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsions in Example 2, Examples 5-8 and Comparative Example 1 are shown in Figure 1, wherein (a) is the viscosity, measured using a DHR-2 rotational rheometer, and (b) is the angular frequency. Fig.13 (a) shows that all emulsions exhibit typical shear thinning behavior, and the viscosity decreases with increasing shear rate, indicating that the emulsions have pseudoplastic fluid characteristics. At the same shear rate, the viscosity of the emulsion increases with the increase of OMMT. This is because the increase in Ugi-OSA-SH / OMMT composite particles on the oil-water interface strengthens the three-dimensional network structure of the emulsion, resulting in an increase in the viscosity of the emulsion. Fig.13(b) It can be seen that when the OMMT concentration is greater than 0.5wt%, the storage modulus of the emulsion is greater than the loss modulus, which indicates that they both present a gel-like structure, indicating that the increase in Ugi-OSA-SH / OMMT composite particles can form a stable particle film or a three-dimensional network structure region to stabilize the emulsion, which not only improves the stability of the emulsion but also improves the mechanical properties of the emulsion. When the OMMT concentration is less than 0.5wt%, the storage modulus of the emulsion is less than or even equal to the loss modulus, indicating that the emulsion is gradually forming a particle interface film that stabilizes the emulsion, presenting a viscous semi-solid structure, and is transforming towards a gel-like structure. Therefore, when the OMMT concentration is 1.5wt%, the emulsion has good stability.

[0123] The β-carotene standard sample was dissolved in n-hexane to prepare a β-carotene standard solution with a concentration of 0.1 mg / mL, and the standard solution was diluted to concentrations of 1.0, 2.5, 5.0, 7.5 and 10 μg / mL in sequence, and its absorbance was measured at 450 nm using an ultraviolet spectrophotometer to construct a standard curve for β-carotene; 1 mL was taken out from the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion samples prepared in Examples 1-4 and 7-8, and added to a mixed solution of anhydrous ethanol and n-hexane in a volume ratio of 2:3, and placed in an oscillator for thorough mixing and shaking, and the n-hexane phase was collected, and the process was repeated 3 times until the ethanol phase became colorless, and finally the n-hexane phases were combined, and their absorbance was measured at 450 nm using an ultraviolet-visible spectrophotometer, and the β-carotene encapsulation efficiency (EE) of different emulsion samples was calculated according to the obtained β-carotene standard curve, and the calculation formula is shown in Formula (2),

[0124]

[0125] Wherein, m1 is the measured content of β-carotene in the emulsion, and m2 is the content of added β-carotene.

[0126] It was measured that the encapsulation efficiency (EE) of β-carotene by the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion prepared in Example 1 was as high as 93.7%, the encapsulation efficiency (EE) of β-carotene by the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion prepared in Example 2 was as high as 84.2%, the encapsulation efficiency (EE) of β-carotene by the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion prepared in Example 3 was as high as 73.4%, and the encapsulation efficiency (EE) of the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion prepared in Example 4 was as high as 90.1%.

[0127] One portion (4 mL) of the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion prepared in Example 7 and two portions (4 mL each) of the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion prepared in Example 8 were respectively loaded into a dialysis bag with a molecular weight cutoff of 8000, and then the dialysis bag containing the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion prepared in Example 7 was immersed in 50 mL of PBS solution containing 0.5% SDS and pH 7.4 for 5 min. n, immerse the dialysis bags containing the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion prepared in Example 8 into 50 mL of PBS solution containing 0.5% SDS and pH 7.4 and 2.0 for 5 minutes respectively; then, at 37°C, within the set time, immerse the three dialysis bags again into the same volume of fresh PBS solution to avoid saturation effect due to drug release, and take out 5 mL of the solution in the dialysis bag at each time point, measure its absorbance at 450 nm with an ultraviolet spectrophotometer, and calculate the β-carotene content. The β-carotene content in each time period is added to the total amount of drug released in the previous time period to obtain the cumulative total amount of β-carotene released in this period. The ratio of the total amount released to the drug loading is the cumulative drug release rate. The drug release kinetic curve of the cumulative drug release rate changing with time is drawn based on the experimental data. The results are shown in Fig.14 (b).

[0128] Fig.14 The encapsulation efficiency curve and drug release kinetics curve of β-carotene by the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion in Example 7-8, wherein (a) is the encapsulation efficiency curve and (b) is the drug release curve. Fig.14 It can be seen that when the OMMT concentration is high, the drug loading rate of the emulsion is high and the cumulative release rate is low. This shows that the emulsion stabilized by Ugi-OSA-SH / OMMT has a good ability to protect β-carotene. The reason is that the more OMMT there is, the more Ugi-OSA-SH / OMMT composite particles there are, which show a high emulsion surface coverage rate. After adsorbing on the emulsion interface, a more complete and dense interface film is formed, which prevents the migration of droplets and the diffusion of drugs, thereby improving the drug loading capacity and sustained release capacity of the emulsion. Therefore, the higher the OMMT concentration, the more beneficial it is to the stability and sustained release capacity of the emulsion.

[0129] In addition, under the condition that the concentration of Ugi-OSA-SH is fixed at 1.0 mg / mL, 2.0 mg / mL or 3.0 mg / mL, as the concentration of OMMT increases, the droplet size and emulsion instability coefficient of the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion prepared by the present invention decrease, and the stability and viscoelasticity both increase, indicating that OMMT and Ugi-OSA-SH form a three-dimensional network structure at the oil-water interface, which makes the emulsion have high stability and can keep the emulsion from flowing when inverted. These characteristics of the Ugi-OSA-SH / OMMT synergistically stabilized drug-loaded Pickering emulsion effectively solve the problems of low bioavailability and poor stability of traditional food preparations, and make it show great application potential in the field of functional food active factor carrier material preparation technology.

[0130] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing a drug-loaded Pickering emulsion based on oxidation-Ugi reaction of alginate derivatives / organic montmorillonite synergistic stabilization, characterized in that: The following steps are involved: (1) adding β-mercaptoethylamine, glacial acetic acid, and isocyanocyclohexane to a sodium periodate oxidized alginate derivative solution in sequence to perform an Ugi four-component reaction, followed by dilution, precipitation, centrifugation, alcohol washing, re-centrifugation, dialysis, and freeze drying to obtain an oxidized-Ugi reaction alginate derivative Ugi-OSA-SH; (2) placing montmorillonite, polyoxyethylene ether and water in a ball mill for ball milling, centrifuging, washing, re-centrifuging and freeze-drying to obtain organic montmorillonite OMMT; (3) mixing the oxidized-Ugi reaction alginic acid derivative Ugi-OSA-SH obtained in step (1) with water to obtain a Ugi-OSA-SH aqueous solution, and then adding the organic montmorillonite OMMT obtained in step (2), and obtaining a Ugi-OSA-SH / OMMT aqueous dispersion suspension by ultrasonication and stirring; (4) using olive oil containing food active factors as the oil phase and the Ugi-OSA-SH / OMMT aqueous dispersion suspension obtained in step (3) as the aqueous phase, mixing the two and then performing shear emulsification to obtain a drug-loaded Pickering emulsion based on oxidation-Ugi reaction alginate derivative / organic montmorillonite synergistic stabilization; There is no order of precedence for steps (1) and (2).

2. The preparation method according to claim 1, characterized in that: In step (1), the molar ratio of the theoretical aldehyde functional group of the sodium periodate oxidized alginate derivative to β-mercaptoethylamine, glacial acetic acid and isocyanocyclohexane in the sodium periodate oxidized alginate derivative solution is (0.7:1:1:1)-(1:1:1:1).

3. The preparation method according to claim 1, characterized in that: In step (2), the CEC of the montmorillonite is 1.20 mmol / g; the molecular weight of the polyoxyethylene ether is 1123.51, and the amount of the polyoxyethylene ether used is 1.0-4.0 times the CEC of the montmorillonite.

4. The preparation method according to claim 1, characterized in that: In step (2), when the amount of montmorillonite used is 2.0-4.0 g, the grinding balls used for ball milling include 2 agate balls with a diameter of 20 mm, 6 agate balls with a diameter of 10 mm, and 10 agate balls with a diameter of 6 mm; the rotation speed of the ball mill is 500 r / min, and the ball milling time is 2 h.

5. The preparation method according to claim 1, characterized in that: In step (3), the concentration of the Ugi-OSA-SH aqueous solution is 1.0-5.0 mg / mL; the mass fraction of the organic montmorillonite OMMT in the Ugi-OSA-SH / OMMT aqueous dispersion is 0.5-2.5%.

6. The preparation method according to claim 1, characterized in that: In step (3), the power of the ultrasound is 100-200W, and the method is probe ultrasound.

7. The preparation method according to claim 1, characterized in that: In step (4), the concentration of the food active factor in the olive oil containing the food active factor is 1.0-8.0 mg / mL; the volume ratio of the olive oil containing the food active factor to the Ugi-OSA-SH / OMMT aqueous dispersion suspension is (2:8)-(4:6).

8. The preparation method according to claim 1, characterized in that: In step (4), the food active factor includes one of β-carotene, lutein, zeaxanthin, astaxanthin and lycopene.

9. The preparation method according to claim 1, characterized in that: In step (4), the shear emulsification speed is 12000r / min and the time is 5min.

10. The drug-loaded Pickering emulsion prepared by the preparation method according to any one of claims 1 to 9, which is synergistically stabilized by an alginate derivative / organic montmorillonite based on oxidation-Ugi reaction.

Citation Information

Patent Citations

  • Alginic acid derivative micelle loaded with carotenoid as well as preparation method and application of alginic acid derivative micelle

    CN115363212A