Injectable enzymatic cross-linked polysaccharide hydrogel as well as preparation method and application thereof
Through the double cross-linked structure of enzymatically cross-linked polysaccharide hydrogel, the problem of cytotoxicity caused by cross-linking agents in the existing technology is solved, and a hydrogel with high biocompatibility and self-healing function is provided, which is suitable for various applications. A kind of wound treatment that meets the complex needs of chronic wound healing.
Patent Information
- Application Number
- CN202410688312.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-05-30
AI Technical Summary
Existing skin wound dressings suffer from cytotoxicity problems caused by cross-linking agents and are difficult to meet the complex healing needs of chronic wounds. Traditional materials have deficiencies in mechanical strength, tissue viscosity and biocompatibility.
Enzymatic cross-linked polysaccharide hydrogel is used to form a hydrogel with a dynamic covalent network through a mild cross-linking reaction mediated by galactose oxidase and horseradish peroxidase, combining modified chitosan and phenol groups. Clusters form a double cross-linked structure, providing self-healing function and good biocompatibility.
The preparation of hydrogel without additional cross-linking agent is achieved. It has high water content and rich three-dimensional pore structure, promotes cell infiltration and differentiation, provides good biocompatibility and hemostatic properties, and is suitable for various wound treatments.
Smart Images

Figure CN118767201A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of biomedical materials, and in particular, relates to an injectable enzymatically cross-linked polysaccharide hydrogel, a preparation method and an application thereof. Background Art
[0002] The skin is the largest organ in the human body and an important protective barrier for maintaining blood balance. It plays an important role in resisting external attacks. However, in daily life, injuries such as cuts and burns are difficult to avoid, and the integrity of skin tissue is destroyed or dysfunctional, which significantly reduces the quality of life of patients. The mechanism of skin wound healing is very complex, involving hemostasis, inflammation, proliferation and wound remodeling, and scar tissue formation. For wound management, especially chronic wounds (such as infected wounds, burn wounds, and diabetic foot ulcers), traditional dressings (such as gauze, cotton, etc.) can no longer meet clinical needs. Therefore, various biomaterials have emerged, such as electrospun scaffolds, foams, sponges, and membranes.
[0003] An ideal skin wound dressing needs to have good tissue compatibility and moisture retention, be able to absorb tissue exudate, and have certain mechanical strength, tissue adhesion and surface microstructure. It can stably exist on the wound surface, prevent external contamination, inhibit bacterial growth, and promote cell adhesion, proliferation and differentiation. Based on the above characteristics, hydrogels stand out from many candidate materials and become the most promising skin wound dressings. However, the cross-linking method has a huge impact on the structure and function of hydrogels. Common cross-linking methods are mainly divided into physical cross-linking and chemical cross-linking. For example, cross-linking mediated by ultraviolet light will make the hydrogel have certain cytotoxicity due to the addition of photoinitiators.
[0004] Based on this, mild cross-linking reactions mediated by enzyme catalysis have become a simple and effective method for preparing bio-friendly hydrogels. Most of the enzymes involved in cross-linking are enzymes that catalyze reactions that occur naturally in the human body and can function at neutral pH, water environment, and moderate temperature. Therefore, the exploration of new enzymatic cross-linked hydrogels is of great significance and is expected to provide innovative ways for further tissue engineering applications. Summary of the invention
[0005] In order to make up for the deficiencies of the prior art, the present invention provides an injectable enzymatic cross-linked hydrogel, a preparation method and an application thereof, which has excellent biocompatibility and overcomes the shortcomings of the prior hydrogel such as toxic side effects caused by cross-linking agents.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] In a first aspect, the present invention provides an injectable enzymatic cross-linked hydrogel, which is formed by mixing and cross-linking a polysaccharide, a modified polysaccharide and an enzyme, wherein the polysaccharide is a polysaccharide containing a galactose side chain, and the modified polysaccharide is a polysaccharide having an amino group, and the specific weight ratio is as follows: polysaccharide 0.5-20%, modified polysaccharide 0.5-20%, enzyme 0.001-0.1%, and the rest is water.
[0008] Preferably, the polysaccharide comprises one or more of mannan, arabinogalactan, arabinoxylan, xyloglucan and Pleurotus ferulae polysaccharide.
[0009] Preferably, the modified polysaccharide is modified chitosan CPA grafted with arginine and phenol groups.
[0010] Preferably, the enzymes include galactose oxidase Gox and horseradish peroxidase HRP.
[0011] In a second aspect, the present invention provides a method for preparing an injectable enzymatic polysaccharide hydrogel, characterized in that it comprises the following steps:
[0012] (1) extracting polysaccharides from polysaccharide raw materials;
[0013] (2) Synthesizing modified polysaccharides in one pot using polysaccharides and grafted products as raw materials;
[0014] (3) Mixing polysaccharide, modified polysaccharide and enzyme solution.
[0015] Preferably, in step (1), 10 g of the raw material is dissolved in 1000 mL of deionized water, the temperature is gradually raised to 40° C., stirring is continued, and then impurities are removed by centrifugation. The reaction time in the process is 1-48 h.
[0016] Preferably, step (2) comprises the following steps:
[0017] (1) Dissolve 1 g of a polysaccharide having an amino group in an acid solution at room temperature to obtain a solution A;
[0018] (2) At room temperature, 1 g of 3-(4-hydroxyphenyl)propionic acid was dissolved in an ethanol solution, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) were added, and the mixture was stirred to be uniformly mixed. The pH was adjusted and the activation reaction was carried out for 0.5 h to obtain a solution B;
[0019] (3) At room temperature, 2.11 g of L-arginine was dissolved in acetic acid solution, EDC and NHS were added, and the mixture was stirred to make it uniform. The pH was adjusted and the activation reaction was carried out for 2 h to obtain solution C.
[0020] (4) Solution B and solution C are sequentially added dropwise to solution A, stirred to fully mix, and the pH is adjusted to allow coupling reaction for 24 hours; after the reaction is completed, the reaction substances and by-products are removed by dialysis, and the modified polysaccharide is obtained by freeze-drying.
[0021] Preferably, step (3) comprises the following steps:
[0022] (1) dissolving polysaccharides, modified polysaccharides and enzymes;
[0023] (2) The polysaccharide, modified polysaccharide and enzyme are uniformly mixed according to the ratio in claim 1 and continuously stirred until gelation occurs.
[0024] Preferably, the solvent in the process is one or more of water, phosphate buffer, Ringer's solution, and glycerol.
[0025] In a second aspect, the present invention provides the use of injectable enzymatic polysaccharide hydrogel in the preparation of medical wound dressings.
[0026] Preferably, the application includes dressings for mechanically damaged wounds and ulcerative wounds.
[0027] In a specific implementation, the hydrogel is formed by mixing xyloglucan (XG), modified chitosan grafted with arginine and phenol groups (CPA), galactose oxidase (Gox) and horseradish peroxidase (HRP) and stirring them.
[0028] Among them, under the action of Gox, the galactose group in the XG structure is oxidized to generate aldehyde group and releases H2O2. Under the action of H2O2 and HRP, the phenol groups on the modified chitosan are covalently cross-linked, and the aldehyde group in XG and the amino group on the modified chitosan form a dynamic Schiff base bond, thereby forming a double cross-link and containing a dynamic covalent network, which gives the hydrogel the function of self-healing and can be used by injection.
[0029] The purpose of the present invention is to provide the application of injectable enzymatic polysaccharide hydrogel in the preparation of medical wound dressings; the application includes mechanical injury wounds and ulcerative wound dressings.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The present invention provides a novel enzymatic cross-linking method for preparing hydrogels through a one-pot process. The substrates are evenly mixed and can be gelled by magnetic stirring. No heating or other conditions are required, and no additional cross-linking agents or chemical components, such as H2O2, are added. The preparation is simple and is beneficial to improving the biocompatibility of the hydrogel.
[0032] (2) The injectable enzymatic polysaccharide hydrogel provided by the present invention has a high water content and a rich three-dimensional pore structure, which can provide favorable conditions for cell infiltration, proliferation and differentiation, as well as the sprouting of blood vessels in granulation tissue; on the other hand, the modified chitosan gives the hydrogel a hemostatic effect, and the grafted phenol group can play an antioxidant role. In addition, the hydrogel has good biocompatibility. After a series of in vitro biological evaluations, including cytotoxicity experiments, it is proved that the hydrogel has good biocompatibility and is non-irritating to human skin tissue. The injectable enzymatic polysaccharide hydrogel provided by the present invention is simple to prepare, has good repeatability, and is not restricted by delicate operations or instruments. The hydrogel is suitable for the treatment of various types of wounds. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The present invention will be further described below in conjunction with the accompanying drawings.
[0034] Figure 1 This is a schematic diagram of the gel time of Example 3 of the present invention;
[0035] Figure 2 This is a scanning electron microscope image of a cross section of Example 3 of the present invention;
[0036] Figure 3 The rheological properties of Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 3 of the present invention are characterized by rheological properties, which are respectively rheometer time scanning results, rheometer strain scanning results, rheometer "three-platform" scanning results, and rheometer strain alternating scanning results;
[0037] Figure 4 The diagram shows the antioxidant effects of Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 3 of the present invention;
[0038] Figure 5 Characterization of cell compatibility of Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 3 of the present invention;
[0039] Figure 6 This is a diagram showing the hemostatic performance of Example 3 of the present invention;
[0040] Figure 7 These are pictures of repairing chronic wounds in diabetic mice according to Example 3 of the present invention, which are typical pictures of wound healing on days 0, 3, 7, 14 and 21, as well as statistical pictures of wound contraction areas in each group. DETAILED DESCRIPTION
[0041] The present invention is described in detail below with reference to the embodiments.
[0042] Example 1 Preparation of xyloglucan (XG)
[0043] Weigh 10g of tamarind powder and dissolve it in 1000mL of deionized water, gradually raise the temperature to 40℃, and continue stirring for 24h to obtain a uniform solution. Then use centrifugation at 8000r for 10min to centrifuge the insoluble impurities in the solution, remove the impurities and retain the supernatant. Put the prepared supernatant into a -80℃ refrigerator and freeze it in a freeze dryer. The spongy solid obtained after freeze drying is xyloglucan named XG.
[0044] Example 2 Preparation of modified chitosan (CPA)
[0045] At room temperature, 1 g of chitosan (CS) was dissolved in 100 ml of 1% (v / v) acetic acid solution and magnetically stirred until completely dissolved to obtain a 1 wt% CS solution, which was referred to as solution A.
[0046] At room temperature, 1 g of 3-(4-hydroxyphenyl)propionic acid was dissolved in 20 ml of 50% (v / v) ethanol solution, 0.5 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC) and 0.3 g of N-hydroxysuccinimide (NHS) were added, and the mixture was stirred to mix well. 1 M HCL was used to adjust the pH to about 5, the temperature was 25° C., and the activation reaction was carried out for 0.5 h to obtain solution B.
[0047] At room temperature, 2.11 g of L-arginine was dissolved in 1% (v / v) acetic acid solution, 3.49 g of EDC and 1.15 g of NHS were added, and the mixture was stirred to be uniformly mixed. 1 M HCL was used to adjust the pH to about 5, the temperature was 25°C, and the activation reaction was carried out for 2 hours to obtain solution C.
[0048] Solution B and solution C were sequentially added dropwise to solution A, stirred to fully mix, and 1M HCL was used to adjust the pH to 5-6, the temperature was 25°C, and the coupling reaction was carried out for 24 hours; after the reaction, the reaction substances and by-products were removed by dialysis, and lyophilized to obtain chitosan (CPA) modified with arginine and phenol groups.
[0049] Example 3 Xyloglucan / modified chitosan enzymatic polysaccharide hydrogel
[0050] Prepare 3wt% xyloglucan solution, the solvent is deionized water; prepare 4wt% modified chitosan solution, the solvent is deionized water; prepare 16U / ml Gox enzyme solution and 48U / ml HRP enzyme solution. Mix 2mL xyloglucan solution, 1mL modified chitosan solution, 0.25mL deionized water, 0.5ml Gox enzyme solution and 0.25ml HRP enzyme solution, and stir magnetically for a certain period of time to gel. The hydrogel is named XG3 / CPA2 hydrogel.
[0051] Specifically, XG, CPA, Gox and HRP were dissolved in deionized water to prepare 3wt%, 2wt%, 16U / ml and 48U / ml solutions respectively; each component was added into a brown sample bottle according to the proportion, and a gel was formed under the action of magnetic stirring.
[0052] Example 4
[0053] The invention discloses an injectable enzymatic polysaccharide hydrogel, which is formed by mixing xyloglucan, modified chitosan grafted with phenol groups and arginine, and Gox and HRP enzymes and then cross-linking. The specific weight ratio is as follows: 0.5-20% xyloglucan, 0.5-20% modified chitosan, 0.001-0.1% Gox enzyme, 0.001-0.1% HRP enzyme, and the rest is water; wherein the modified chitosan is combined with the xyloglucan through a Schiff base bond, and the phenol groups in the modified chitosan structure are combined through enzymatic reaction to form CC or CO covalent bonds.
[0054] The above-mentioned injectable enzymatic polysaccharide hydrogel can be used in the preparation of medical wound dressings, including dressings for mechanically damaged wounds and ulcerative wounds.
[0055] Example 5
[0056] An injectable enzymatic polysaccharide hydrogel, the hydrogel is formed by cross-linking after mixing polysaccharide, modified polysaccharide and enzyme, and the specific weight ratio is as follows: polysaccharide 0.5-20%, modified polysaccharide 0.5-20%, enzyme 0.001-0.1%, and the rest is water. The polysaccharide is a polysaccharide containing galactose side chains, and the modified polysaccharide is a polysaccharide with amino groups. The polysaccharide includes one or more of mannan, arabinogalactan, arabinoxylan, xyloglucan, and Pleurotus ferulae polysaccharide; the modified polysaccharide is a modified chitosan CPA grafted with arginine and phenol groups; the enzyme is galactose oxidase Gox and horseradish peroxidase HRP.
[0057] Comparative Example 1 Preparation of Xyloglucan / Modified Chitosan Enzymatic Polysaccharide Hydrogel
[0058] Prepare 4wt% xyloglucan solution, the solvent is deionized water; prepare 4wt% modified chitosan solution, the solvent is deionized water; prepare 16U / ml Gox enzyme solution and 48U / ml HRP enzyme solution. Mix 2mL xyloglucan solution, 1mL modified chitosan solution, 0.25mL deionized water, 0.5ml Gox enzyme solution and 0.25ml HRP enzyme solution, and stir magnetically for a certain period of time to gel. The hydrogel is named XG4 / CPA2 hydrogel.
[0059] Comparative Example 2 Preparation of Xyloglucan / Modified Chitosan Enzymatic Polysaccharide Hydrogel
[0060] Prepare 4wt% xyloglucan solution, the solvent is deionized water; prepare 4wt% modified chitosan solution, the solvent is deionized water; prepare 16U / ml Gox enzyme solution and 48U / ml HRP enzyme solution. Mix 2mL xyloglucan solution, 0.5mL modified chitosan solution, 0.75mL deionized water, 0.5ml Gox enzyme solution and 0.25ml HRP enzyme solution, and stir magnetically for a certain period of time to gel. The hydrogel is named XG4 / CPA1 hydrogel.
[0061] Comparative Example 3 Preparation of Xyloglucan / Modified Chitosan Enzymatic Polysaccharide Hydrogel
[0062] Prepare 3wt% xyloglucan solution, the solvent is deionized water; prepare 4wt% modified chitosan solution, the solvent is deionized water; prepare 16U / ml Gox enzyme solution and 48U / ml HRP enzyme solution. Mix 2mL xyloglucan solution, 0.5mL modified chitosan solution, 0.75mL deionized water, 0.5ml Gox enzyme solution and 0.25ml HRP enzyme solution, and stir magnetically for a certain period of time to gel. The hydrogel is named XG3 / CPA1 hydrogel.
[0063] Test Example 1
[0064] The chemical structures of the above-mentioned Examples 2 and 3 were tested, the rheological properties, antioxidant properties, biocompatibility and hemostatic properties of the hydrogels obtained in Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were tested, and the therapeutic effect of Example 3 on diabetic chronic wounds was tested.
[0065] Test Example 2 Scanning Electron Microscope Observation
[0066] The scanning electron microscope was used to observe Example 3, and the results were as follows: Figure 2 As shown, XG3 / CPA2 hydrogel has a stable and clear pore structure, which is conducive to cell migration and proliferation, and promotes normal material exchange between cells and tissues.
[0067] Test Example 3 Rheological Test
[0068] The rheological tests were performed on the hydrogels obtained in Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 3 using a rheometer equipped with a 20 mm parallel plate. Time sweep test (300 s, 1% strain, 10 rad / s frequency), strain sweep (1% -
[0069] 1000% strain, 10 rad / s frequency), "three-platform" scanning (10% strain, 10 rad / s and 50 rad / s frequency for 1.5 cycles, time 80 s) and alternating time scanning test (1% and 1000% for 3.5 cycles, duration 60 s and 30 s, frequency 10 rad / s), each experiment used 300 μL hydrogel, temperature 25 ° C, gap 500 μm. The results are shown in Figure 3 As shown. The time scan results showed that the storage modulus (G') of all hydrogels always exceeded the loss modulus (G"), indicating that each group formed a stable hydrogel network. Among them, the XG3 / CPA1 hydrogel showed the lowest G' of 198.3±10.2Pa, while the XG4 / CPA2 hydrogel showed the highest G' of 595.5±30.5Pa, indicating that with the increase of polysaccharide concentration, the modulus of the hydrogel will increase accordingly, thereby improving the mechanical strength of the hydrogel, making it less likely to be destroyed by external forces and able to adapt to more practical application scenarios. When the applied stress exceeds the fracture stress (1000%), the hydrogel will change from a gel state to a sol state. When the stress returns to 1%, the modulus returns to The hydrogel changes from the sol state to the gel state again. This shows that the XG3 / CPA2 hydrogel has self-healing properties. Through the "three-platform" scanning test with changing shear frequency, in the range of 0 to 80s, the shear frequency of the hydrogel is 10rad / s, and the viscosity of the hydrogel is 89.9±4.6Pa·s; the shear frequency is suddenly increased to 500rad / s, and the viscosity of the hydrogel is instantly reduced to 14.4±1.3Pa·s; then the shear frequency is suddenly reduced to 10rad / s, and the viscosity of the hydrogel returns to the initial value of 91.3±3.3Pa·s, simulating the extrusion process of the hydrogel from the syringe needle, further verifying the injectability of the hydrogel.
[0070] Test Example 4 Antioxidant Test
[0071] The hydrogels in Example 2, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were prepared by soaking 300 μL of the hydrogel in anhydrous ethanol, then adding 100 μL of 1,1-diphenyl-2-trinitrophenylhydrazine (DPPH·) solution (0.5 mM) and standing for 1 h and 24 h. Then, the absorbance at about 520 nm was scanned using a UV-visible spectrophotometer. The free radical scavenging rate was calculated by the following formula:
[0072]
[0073] Among them, A B , A HThey are the absorbance of the blank group (DPPH·free radical + ethanol) at 520 nm and the absorbance of the hydrogel group (DPPH·free radical + ethanol + hydrogel) at 520 nm, respectively.
[0074] XG / CPA hydrogels all showed good free radical scavenging ability, such as Figure 4 Within 24 hours, the scavenging rate of DPPH· free radicals by each group of hydrogels was above 75%.
[0075] Test Example 5 Cell Compatibility Test
[0076] Under sterile conditions, the hydrogels in Example 2, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were prepared and sterilized under UV light for 2 hours. 1 mL of the hydrogel was placed in 10 mL of DMEM complete medium and incubated at 37°C for 24 hours. L929 cells were collected and plated at 3×10 cells per well. 3 The cells were seeded in a 96-well plate at a density of 100 cells / well. After 24 hours, the medium in the wells was replaced with 0.1 mL of the filtered extract. On the 1st, 2nd, and 3rd day of co-culture, the medium in the wells was aspirated and 10 μL of CCK-8 reagent and 90 μL of cell culture medium were added. After incubation in a cell culture incubator for 1 hour, the absorbance was measured at 450 nm. The cell viability was calculated as follows:
[0077]
[0078] At, A0 and Ac represent the absorbance of the hydrogel group, the cck-8 blank group and the control group, respectively.
[0079] The cell viability of each hydrogel cell survival rate was greater than 100% ( Figure 5 ), indicating that each hydrogel has good cell compatibility.
[0080] Test Example 6 Liver hemostasis performance test
[0081] First, by intraperitoneal injection 50 anesthetized mice (ICR, male, 20-25g) were fixed on a vertical operating table. The abdominal cavity of the mouse was opened, the liver lobe was found, and the surrounding tissue fluid was drained with gauze. A pre-weighed filter paper was placed under the liver, a 3 mm long wound was made on the liver with a scalpel, and 0.2 mL of the hydrogel obtained in Example 3 was immediately injected into the wound. The untreated wound was treated as a blank control, and the blood loss was calculated using filter paper.
[0082] XG3 / CPA2 hydrogel can quickly stop liver bleeding in mice ( Figure 6 ), and the amount of blood loss in the liver was approximately one-third of that in the untreated blank group.
[0083] Test Example 7 Chronic wound test in diabetic mice
[0084] A full-thickness skin wound was established on the back of diabetic mice, and the hydrogel prepared in Example 3 was applied to the wound. The wound was compared with that of mice treated with commercial excipients, and the healing process was recorded by taking photos and the wound contraction rate was calculated. Figure 7 As shown, on the 14th day, the wound healing rate in the hydrogel treatment group was over 80%, and was almost completely healed on the 21st day, while the control group still had obvious wounds on the 21st day.
Claims
1. An injectable enzymatic polysaccharide hydrogel, characterized in that: The hydrogel is formed by mixing polysaccharide, modified polysaccharide and enzyme and then cross-linking, wherein the polysaccharide is a polysaccharide containing galactose side chains, and the modified polysaccharide is a polysaccharide with amino groups; the specific weight ratio is as follows: polysaccharide 0.5-20%, modified polysaccharide 0.5-20%, enzyme 0.001-0.1%, and the rest is water.
2. The injectable enzymatic polysaccharide hydrogel according to claim 1, characterized in that: The polysaccharide includes one or more of mannan, arabinogalactan, arabinoxylan, xyloglucan and Pleurotus ferulae polysaccharide.
3. The injectable enzymatic polysaccharide hydrogel according to claim 1, characterized in that: The modified polysaccharide is modified chitosan CPA grafted with arginine and phenol groups; the enzymes are galactose oxidase Gox and horseradish peroxidase HRP.
4. A method for preparing the injectable enzymatic polysaccharide hydrogel according to claim 1, characterized in that: The following steps are involved: (1) extracting polysaccharides from raw materials; (2) Synthesizing modified polysaccharides in one pot using polysaccharides and grafted products as raw materials; (3) Mixing polysaccharide, modified polysaccharide and enzyme solution.
5. The preparation method according to claim 4, characterized in that: In step (1), 10 g of the raw material is dissolved in 1000 mL of deionized water, the temperature is gradually raised to 40° C., stirring is continued, and then impurities are removed by centrifugation. The reaction time in the process is 1-48 h.
6. The preparation method according to claim 4, characterized in that: Step (2) comprises the following steps: (1) At room temperature, dissolve 1 g of polysaccharide in acetic acid solution to obtain solution A; (2) At room temperature, 1 g of 3-(4-hydroxyphenyl)propionic acid was dissolved in an ethanol solution, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) were added, and the mixture was stirred to be uniformly mixed. The pH was adjusted and the activation reaction was carried out for 0.5 h to obtain a solution B; (3) At room temperature, 2.11 g of L-arginine was dissolved in acetic acid solution, EDC and NHS were added, and the mixture was stirred to make it uniform. The pH was adjusted and the activation reaction was carried out for 2 h to obtain solution C. (4) Solution B and solution C are sequentially added dropwise to solution A, stirred to fully mix, and the pH is adjusted to allow coupling reaction for 24 hours; after the reaction is completed, the reaction substances and by-products are removed by dialysis, and the modified polysaccharide is obtained by freeze-drying.
7. The preparation method according to claim 4, characterized in that: Step (3) comprises the following steps: (1) dissolving polysaccharides, modified polysaccharides and enzymes; (2) The polysaccharide, modified polysaccharide and enzyme are mixed according to the ratio in claim 1 and stirred evenly.
8. The preparation method according to claim 4, characterized in that: The solvent in the process is one or more of water, phosphate buffer, Ringer's solution and glycerol.
9. Use of the injectable enzymatic polysaccharide hydrogel according to claim 1 in the preparation of medical wound dressings; the application includes dressings for mechanically damaged wounds and ulcerative wounds.
Citation Information
Patent Citations
Compositions and kits for enzymatic debridement and methods of using the same
CN107106663A
Injectable hydrogel and preparation method thereof
CN110464871A
Preparation method and application of multi-enzyme active nano-enzyme fluorescent hydrogel
CN115386105A
Cu-MOF / GOX functionalized chitosan-arginine temperature-sensitive hydrogel as well as preparation method and application thereof
CN117924537A
Hyaluronic acid / tannic acid / carbon microsphere injectable hydrogel for promoting wound healing and preparation method of hyaluronic acid / tannic acid / carbon microsphere injectable hydrogel
CN118045224A