Anticoagulant intravascular stent and preparation method thereof

By hydroxylating and grafting dimethyl sulfoxide on the micro-textured scaffold, an anticoagulant vascular scaffold with U-shaped grooves is formed, which solves the coagulation problem caused by blood flow friction, achieves efficient anticoagulant effect, and reduces It improves platelet adhesion and activation and improves the safety of vascular stents.

CN118767221APending Publication Date: 2024-10-15ARMOR ACADEMY OF CHINESE PEOPLES LIBERATION ARMY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410993169.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

During the vascular stent implantation process, the coagulation mechanism caused by blood flow friction triggers abnormalities, forming intra-stent thrombosis, which seriously hinders the treatment of cardiovascular diseases. Existing anticoagulation methods are complicated and difficult to effectively prevent thrombosis.

Method used

By performing hydroxylation treatment and dimethyl sulfoxide grafting reaction on the micro-textured scaffold, an anticoagulant vascular scaffold with U-shaped grooves is formed, which increases blood flow rate, reduces platelet adhesion, and forms dimethyl sulfoxide on the surface of the scaffold. Sulfone molecule coating, has anti-platelet activation effect.

Benefits of technology

It achieves a simple and efficient anticoagulant effect, significantly reduces platelet adhesion and activation, improves the anticoagulant performance of the vascular stent, and avoids the occurrence of restenosis within the stent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767221A_ABST
    Figure CN118767221A_ABST
Patent Text Reader

Abstract

The invention provides an anticoagulant intravascular stent and a preparation method thereof, and relates to the technical field of medical instruments. The preparation method comprises the following steps: carrying out hydroxylation treatment on a micro-texture stent, and immersing the micro-texture stent into dimethyl sulfoxide to carry out grafting reaction, so as to obtain the anticoagulant intravascular stent. U-shaped grooves are formed in the inner surface of the micro-texture stent in the axial direction of the stent, and the U-shaped grooves are distributed in the inner surface of the stent. The U-shaped grooves are formed in the inner surface of the stent in the axial direction of the stent to form a micro-texture structure, the shear stress of the stent is changed, the blood flow velocity is increased, and adhesion of platelets is reduced; through hydroxylation treatment and grafting reaction, a dimethyl sulfoxide molecular coating is formed on the surface of the stent, and dimethyl sulfoxide has the effect of resisting platelet activation. The preparation method provided by the invention is simple and efficient, excessive complex chemical reactions are not needed, and the obtained stent has an excellent anticoagulant effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of medical devices, and in particular to an anticoagulant vascular stent and a preparation method thereof. Background Art

[0002] Cardiovascular disease has become a disease with a high mortality rate. Vascular stent implantation has become the primary means of treating cardiovascular disease because of its simple and safe operation.

[0003] However, during the implantation of vascular stents, friction will occur between the stent and the human soft tissue. Among them, the fluid friction formed by blood flow on the surface of the stent will trigger an abnormal coagulation mechanism. The inner surface of the stent will promote coagulation through a series of interrelated processes, including protein adsorption, platelet activation and adhesion, thrombin generation and complement activation, thereby forming a thrombus in the stent, causing restenosis in the stent, which seriously hinders the treatment of cardiovascular diseases. Among them, the rapid adsorption of plasma proteins on the surface of the stent is the first step in the formation of thrombus, which is generally completed within a few minutes; then, thrombin is generated on the surface of the stent material and promotes the coagulation cascade reaction, such as the conversion of fibrinogen into fibrin; then, the blood flow generates fluid friction on the surface of the stent, and the adsorbed fibrinogen adheres to the platelets in the blood, further causing platelet activation and creating a lesion for the generation of thrombin, and finally forming a thrombus. This brings huge challenges to the design and application of cardiovascular stent implantation devices.

[0004] At present, thrombosis is mainly prevented by oral anticoagulant drugs and anticoagulant modification of the stent surface. Anticoagulant modification of the surface of vascular stents can greatly improve the safety and effectiveness of medical vascular stents and greatly reduce the incidence of restenosis in stents. Anticoagulant coating is the most widely studied modification method for improving the anticoagulant performance of stents and reducing restenosis in stents. This method is to coat the drug on the surface or graft it on the surface of the substrate by chemical reaction. These drug coatings require complex and specific targeted modification of the surface, which is complicated to operate and difficult to prepare. For example, the heparin drug coating technology that has been clinically applied requires first obtaining heparin molecules with aldehyde groups at the non-reducing end; the heparin molecules with aldehyde groups at the non-reducing end are subjected to amine-aldehyde condensation reaction with amino compounds to prepare modified heparin, and then the modified heparin molecules are mixed with reactive monomers to undergo polymerization reaction to form polymers; finally, the polymer solution is coated on the surface of the substrate, and the cross-linking groups are cured to form a heparinized coating on the surface. This technology requires multiple chemical reactions and mixing of multiple chemical monomers during the coating preparation process, and it is easy to hide the anticoagulant active sites of heparin. Summary of the invention

[0005] In view of this, the object of the present invention is to provide an anticoagulant vascular stent and a preparation method thereof. The present invention adopts a simple method to prepare an anticoagulant coating on the surface of the stent, does not require too many complicated chemical reactions, and has excellent anticoagulant effect.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing an anticoagulant vascular stent, comprising the following steps:

[0008] The micro-textured stent is subjected to hydroxylation treatment and then immersed in dimethyl sulfoxide for grafting reaction to obtain the anticoagulant vascular stent; the inner surface of the micro-textured stent is provided with U-shaped grooves along the axial direction of the stent, and the U-shaped grooves cover the inner surface of the stent.

[0009] Preferably, the hydroxylation solution used in the hydroxylation treatment is a mixed solution of concentrated sulfuric acid and hydrogen peroxide, the mass fraction of the concentrated sulfuric acid is 98%, the mass fraction of the hydrogen peroxide is 30%, and the volume ratio of concentrated sulfuric acid to hydrogen peroxide in the mixed solution is 7:3 to 3:1.

[0010] Preferably, the hydroxylation treatment is carried out at a temperature of 80 to 85° C. and for a time of 20 to 30 minutes.

[0011] Preferably, the grafting reaction is carried out at a temperature of 60 to 85° C. and for a time of 6 to 12 hours.

[0012] Preferably, the temperature of the grafting reaction is 65°C or 80°C.

[0013] Preferably, after the hydroxylation treatment and the grafting reaction, the obtained scaffold material is washed with water and dried in sequence.

[0014] Preferably, a single U-shaped groove has a width of 40-50 μm and a depth of 20-40 μm.

[0015] Preferably, the method for preparing the micro-textured scaffold comprises the following steps:

[0016] Laser etching a U-shaped groove on the surface of the support substrate to obtain a micro-textured substrate;

[0017] After the micro-textured substrate is heat-treated and formed, laser welding and laser engraving are performed in sequence to obtain the micro-textured bracket.

[0018] Preferably, the heat treatment is performed at a temperature of 580-600° C. and for a time of 20-25 min.

[0019] The present invention provides an anticoagulant vascular stent prepared by the preparation method described in the above technical solution, wherein the inner and outer surfaces of the anticoagulant vascular stent have a dimethyl sulfoxide molecular layer.

[0020] The present invention provides a method for preparing an anticoagulant vascular stent, comprising the following steps: subjecting a micro-textured stent to a hydroxylation treatment, and then immersing the micro-textured stent in dimethyl sulfoxide for a grafting reaction to obtain the anticoagulant vascular stent; the inner surface of the micro-textured stent is provided with a U-shaped groove along the axial direction of the stent, and the U-shaped groove covers the inner surface of the stent. The present invention provides a U-shaped groove along the axial direction of the stent on the inner surface of the stent to form a micro-texture structure, and the shear stress of the stent changes, thereby increasing the blood flow rate and reducing the adhesion of platelets; the present invention forms a dimethyl sulfoxide molecular coating on the surface of the stent through the hydroxylation treatment and grafting reaction, and dimethyl sulfoxide has an anti-platelet activation effect. The preparation method provided by the present invention is simple and efficient, does not require too many complex chemical reactions, and the obtained stent has an excellent anticoagulant effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A schematic diagram of the process of preparing a micro-textured scaffold according to an embodiment of the present invention;

[0022] Figure 2 This is a schematic diagram of the three-dimensional structure of the bracket body in an embodiment of the present invention;

[0023] Figure 3 This is a planar unfolded view of the bracket body in an embodiment of the present invention;

[0024] Figure 4 The inner surface morphology of the micro-textured stent in the embodiment of the present invention is shown in FIG. Figure 4 (a) shows the two-dimensional morphology of the inner surface of the micro-textured scaffold, and (b) shows the three-dimensional morphology of the inner surface of the micro-textured scaffold.

[0025] Figure 5 The apparent contact angle measurement results of the original substrate, the textured substrate and the DMSO-modified substrate obtained according to the method of Example 2;

[0026] Figure 6 The platelet adhesion morphology on different stent surfaces. Figure 6 (a) is the platelet adhesion morphology on the surface of the stent without modified surface, (b) is the platelet adhesion morphology on the surface of the stent with textured surface, and (c) is the platelet adhesion morphology on the surface of the anticoagulant vascular stent (with textured + DMSO surface) obtained in Example 2;

[0027] Figure 7 The platelet adhesion morphology on different stent surfaces. Figure 7 (a) is the platelet adhesion morphology on the surface of the stent without modified surface, (b) is the platelet adhesion morphology on the surface of the stent with textured surface, and (c) is the platelet adhesion morphology on the surface of the anticoagulant vascular stent (with textured + DMSO surface) obtained in Example 3;

[0028] Figure 8The results of platelet CD62p+ expression rate on the surface of different stents. Figure 7 (a) to (e) correspond to the blank control, the scaffold with no modified surface, the scaffold with a textured surface, the scaffold with a textured + DMSO surface in Example 2, and the scaffold with a textured + DMSO surface in Example 3, respectively. DETAILED DESCRIPTION

[0029] The present invention provides a method for preparing an anticoagulant vascular stent, comprising the following steps:

[0030] The micro-textured stent is subjected to hydroxylation treatment and then immersed in dimethyl sulfoxide for grafting reaction to obtain the anticoagulant vascular stent; the inner surface of the micro-textured stent is provided with U-shaped grooves along the axial direction of the stent, and the U-shaped grooves cover the inner surface of the stent.

[0031] In the present invention, the inner surface of the micro-textured stent is provided with U-shaped grooves along the axial direction of the stent, and the U-shaped grooves cover the inner surface of the stent. In the present invention, the width of a single U-shaped groove is preferably 40 to 50 μm, more preferably 45 μm, and the depth is preferably 20 to 40 μm, more preferably 30 μm.

[0032] In the present invention, the method for preparing the micro-textured scaffold preferably comprises the following steps:

[0033] Laser etching a U-shaped groove on the surface of the support substrate to obtain a micro-textured substrate;

[0034] After the micro-textured substrate is heat-treated and formed, laser welding and laser engraving are performed in sequence to obtain the micro-textured bracket.

[0035] Figure 1 Schematic diagram of the process of preparing a micro-textured scaffold according to an embodiment of the present invention.

[0036] In the present invention, the support substrate is preferably a titanium alloy flat substrate. Before laser etching, the support substrate is preferably polished. In the present invention, the parameters of the laser etching preferably include: scanning speed 1000mm / s, pulse frequency 50Hz, pulse width 10μs, power 20W, scanning number 10 times, and scanning spacing of 20μm.

[0037] In the present invention, the temperature of the heat treatment molding is preferably 580-600°C, and the time is preferably 20-25 minutes. The present invention fixes the stent base into a stent shape through heat treatment, specifically, the micro-textured titanium alloy flat plate base is subjected to mold rolling treatment, and the U-shaped groove is located on its inner surface, and then the rolled base is heat treated to be fixed into a circular vascular stent shape to achieve a better circular curvature. The present invention has no special requirements for the parameters of the laser welding, and laser welding can be performed using welding parameters familiar to those skilled in the art. In the present invention, the laser engraving is to engrave the stent into a desired shape. The present invention has no special requirements for the shape of the stent, and a vascular stent of a shape familiar to those skilled in the art can be used. In an embodiment of the present invention, the stent is specifically laser engraved into the following shape: Figure 2-Figure 3 The shape shown in the figure, the stent includes a plurality of supports (i.e., "Z"-shaped annular supports) surrounded by a plurality of sinusoidal annular metal wires with an arc of 60°, and each of the supports is connected by an I-type connector (i.e., a straight connecting rib); wherein the stent with the "Z"-shaped annular support structure effectively combines radial support performance and axial compliance performance, and the I-type connector occupies a small surface area of ​​the stent, reducing the coagulation factor. In an embodiment of the present invention, the inner diameter of the micro-textured stent is 1 cm, the thickness is 0.2 mm, the length is 2 cm, and the length of the straight connecting rib is 1.03 mm.

[0038] The present invention arranges U-shaped grooves on the inner surface of the stent along the axial direction of the stent to form a micro-texture structure, so that the shear stress of the stent changes, the blood flow rate is increased, and the adhesion of platelets is reduced.

[0039] In the present invention, the micro-textured support is preferably cleaned before being subjected to hydroxylation treatment. In the present invention, the cleaning is preferably ultrasonically cleaning the micro-textured support with ethanol and ultrapure water for 10 minutes respectively, and then drying with a hair dryer.

[0040] In the present invention, the hydroxylation solution used in the hydroxylation treatment is preferably a mixed solution of concentrated sulfuric acid and hydrogen peroxide. In the present invention, the mass fraction of the concentrated sulfuric acid is preferably 98%, the mass fraction of the hydrogen peroxide is preferably 30%, and the volume ratio of concentrated sulfuric acid to hydrogen peroxide in the mixed solution is preferably 7:3 to 3:1, more preferably 7:3 or 3:1. In the present invention, the temperature of the hydroxylation treatment is preferably 80 to 85°C, more preferably 80 to 82°C, and the time is preferably 20 to 30 minutes, more preferably 25 to 30 minutes.

[0041] In the present invention, the specific operation of the hydroxylation treatment is preferably:

[0042] Put concentrated sulfuric acid in a beaker, slowly add hydrogen peroxide into the concentrated sulfuric acid, stirring while adding, continue stirring for 3 minutes after the addition is complete, and wait for the mixed solution to cool;

[0043] The obtained mixed solution is heated to 80-85° C. in a water bath, and then the micro-textured scaffold is placed therein for hydroxylation treatment.

[0044] The present invention uses the hydroxylation treatment to make the surface of the stent contain abundant hydroxyl functional groups.

[0045] After the hydroxylation treatment, the present invention preferably sequentially washes and dries the obtained scaffold material. In the present invention, the washing is preferably performed with deionized water to rinse away the excess hydroxylation solution on the scaffold; the drying temperature is preferably 60°C and the drying time is preferably 1 hour.

[0046] In the present invention, the purity of the dimethyl sulfoxide is preferably greater than 99%. The present invention has no special requirements for the amount of dimethyl sulfoxide used, as long as the stent can be completely immersed. In the present invention, the temperature of the grafting reaction is preferably 60 to 85°C, more preferably 65°C or 80°C, and the time is preferably 6 to 12 hours, more preferably 6 to 8 hours. In the present invention, the temperature of the grafting reaction will affect the degree of grafting, that is, the number of dimethyl sulfoxide molecules grafted on the surface. The present invention preferably immerses the hydroxylated stent in a beaker filled with dimethyl sulfoxide, and then places it in a drying oven at a temperature of 60 to 85°C to carry out the grafting reaction.

[0047] In the present invention, the surface of the stent after the hydroxylation treatment contains abundant hydroxyl groups, and the hydroxyl functional groups can react with dimethyl sulfoxide to form a surface molecular layer with dimethyl sulfoxide; at the same time, the reaction change to the dimethyl sulfoxide molecules is very small, which can better ensure the function of dimethyl sulfoxide. In the present invention, the reaction involved in the grafting reaction is: CH3S(O)CH3+OH→(CH3)2S(O)-OH. The present invention forms a dimethyl sulfoxide molecular coating on the surface of the stent through the grafting reaction, and dimethyl sulfoxide has the effect of resisting platelet activation.

[0048] After the grafting reaction, the present invention preferably sequentially washes and dries the obtained scaffold material. In the present invention, the washing is preferably carried out with deionized water, the drying temperature is preferably 80° C., and the drying time is preferably 6 hours.

[0049] The present invention can rapidly prepare an anticoagulant vascular stent with a dimethyl sulfoxide molecular coating, does not require excessive raw materials, and is simple to operate.

[0050] The present invention provides an anticoagulant vascular stent prepared by the preparation method described in the above technical solution, wherein the inner and outer surfaces of the anticoagulant vascular stent have a dimethyl sulfoxide molecular layer. The anticoagulant vascular stent provided by the present invention has the function of inhibiting platelet activation and significantly improving anticoagulant performance.

[0051] In order to further illustrate the present invention, the anticoagulant vascular stent and the preparation method thereof provided by the present invention are described in detail below in conjunction with examples, but they should not be construed as limiting the protection scope of the present invention.

[0052] In the examples, dimethyl sulfoxide was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., AR analytical grade, with a purity of >99%.

[0053] Example 1

[0054] Preparation of micro-textured scaffolds:

[0055] The dimensions of the stent used in the embodiment are as follows: inner diameter 1 cm, thickness 0.2 mm, length 2 cm, straight connecting rib 1.03 mm, arc 60° sinusoidal ring, and its structure is as follows: Figure 2 As shown, the plane expansion diagram is as follows Figure 3 The preparation method is as follows (process as shown Figure 1 shown):

[0056] The vascular stent is made of titanium alloy plate, which is laser cut by ultraviolet pulse laser equipment with the parameters of speed 1000 mm / s, pulse frequency 50 Hz, pulse width 10 μs, and processed into titanium alloy plate with length 25 mm, width 31.9 mm, and thickness 0.2 mm.

[0057] A U-shaped groove was etched on the surface of the titanium alloy plate using an ultraviolet pulse laser device. The parameters were a scanning speed of 1000 mm / s, a pulse frequency of 50 Hz, a pulse width of 10 μs, a power of 20 W, a scanning number of 10 times, and a scanning interval of 20 μm. A micro-textured structure was formed. The width of the U-shaped groove was 45 μm, and the depth was 30 μm, that is, the aspect ratio was 0.67.

[0058] The micro-textured titanium alloy plate was rolled into a round shape using a heat treatment mold at a temperature of 600°C for 20 minutes. Then, a laser automatic welding machine was used for welding with parameters such as a laser wavelength of 1064nm, an output power of 200W, a pulse width of 20ms, and a pulse frequency of 50Hz. The rolled shape was formed into a round tube with an inner diameter of 1cm, and the textured structure was located on the inner surface of the round tube. Finally, a laser micromachining device was used with a parameter of an output power of 100W to carve the round tube into a sinusoidal annular vascular stent with an arc of 60°.

[0059] Figure 4 is the inner surface morphology of the micro-textured scaffold. Figure 4 (a) shows the two-dimensional morphology of the inner surface of the micro-textured scaffold, and (b) shows the three-dimensional morphology of the inner surface of the micro-textured scaffold. It can be seen that the micro-texture is arranged in a U-shaped linear shape, the bottom of the groove is flat, and the U-shaped grooves are evenly distributed.

[0060] Example 2

[0061] The preparation of anticoagulant vascular stent, the steps are as follows:

[0062] The micro-textured scaffold prepared in Example 1 was cleaned by ultrasonic cleaning with ethanol and ultrapure water for 10 min respectively, and then dried with a hair dryer to make its surface clean;

[0063] First, put 98wt% concentrated sulfuric acid into a beaker, and slowly add 30%wt hydrogen peroxide into the concentrated sulfuric acid. The volume ratio of concentrated sulfuric acid to hydrogen peroxide is 7:3. Stir while adding. Stir for 3 minutes and wait for the mixed solution to cool. Heat the mixed solution in an 80℃ water bath, put in the cleaned titanium alloy bracket, and heat for 30 minutes. Take out the titanium alloy bracket, rinse off the excess mixed solution with deionized water, and then put it in a drying oven and dry it at 60℃ for 1h to obtain a hydroxylated bracket;

[0064] The hydroxylated stent is immersed in a beaker of pure dimethyl sulfoxide solution, and then placed in a drying oven for heating at 65°C for 6 hours. The stent is taken out and rinsed with deionized water, and then placed in a drying oven for drying at 80°C for 6 hours to obtain a stent containing a stable dimethyl sulfoxide molecule anticoagulant coating, namely the anticoagulant vascular stent.

[0065] Example 3

[0066] The preparation of anticoagulant vascular stent, the steps are as follows:

[0067] The micro-textured scaffold prepared in Example 1 was cleaned by ultrasonic cleaning with ethanol and ultrapure water for 10 min respectively, and then dried with a hair dryer to make its surface clean;

[0068] First, put 98wt% concentrated sulfuric acid into a beaker, and then slowly add 30wt% hydrogen peroxide into the concentrated sulfuric acid. The volume ratio of concentrated sulfuric acid to hydrogen peroxide is 7:3. Stir while adding. Stir for 3 minutes and wait for the mixed solution to cool. Heat the mixed solution in an 80℃ water bath, put in the cleaned titanium alloy stent, and heat for 30 minutes. Take out the titanium alloy stent, rinse off the excess mixed solution with deionized water, and then put it in a drying oven and dry it at 60℃ for 1h to obtain a hydroxylated stent.

[0069] The hydroxylated stent is immersed in a beaker of pure dimethyl sulfoxide solution, and then placed in a drying oven for heating at 80°C for 6 hours. The stent is taken out and rinsed with deionized water, and then placed in a drying oven for drying at 80°C for 6 hours to obtain a stent containing a stable dimethyl sulfoxide molecule anticoagulant coating, namely the anticoagulant vascular stent.

[0070] Performance testing of anticoagulant vascular stents:

[0071] (1) Contact angle test

[0072] To facilitate the measurement of the contact angle of the anticoagulation coating, the bracket was replaced with a titanium alloy flat substrate (referred to as the original substrate) with a size of 2 cm × 2 cm and a thickness of 2 mm; the titanium alloy flat substrate was laser-etched with U-shaped grooves only in the manner of Example 1 to form a textured substrate; the textured substrate was hydroxylated and grafted with dimethyl sulfoxide in accordance with the methods of Example 2 and Example 3, respectively, to obtain a DMSO-modified substrate. The contact angle of each substrate was tested at room temperature using an optical contact angle meter.

[0073] Figure 5 The following are the apparent contact angle measurement results of the original substrate, the textured substrate and the DMSO modified substrate obtained according to the method of Example 2. Figure 5 It can be seen that the contact angle of the surface modified by DMSO according to the method of Example 2 is increased to 105°, which is a hydrophobic surface. The apparent contact angle of the surface modified by DMSO according to the method of Example 3 is 92.7°.

[0074] (2) Antiplatelet adhesion test

[0075] The anticoagulant vascular stents with anticoagulant coatings obtained in Examples 2 and 3 were subjected to antiplatelet adhesion tests. The anticoagulant vascular stents were placed in a test tube containing platelet-rich plasma, and then the test tubes were placed in a platelet shaking storage box, with the temperature set at 22°C, the shaking frequency at 60 cycles / min, and the shaking for 20 minutes. The surface adhesion results of the anticoagulant coatings of the anticoagulant vascular stents (with textured + DMSO surfaces) obtained in Examples 2 and 3 are as follows: Figure 6 , Figure 7 As shown, it is compared with the original scaffold without laser-etched U-shaped grooves and DMSO modification (i.e., the scaffold without modified surface) and the scaffold only with laser-etched U-shaped grooves but no DMSO modification (i.e., the scaffold with a textured surface).

[0076] Depend on Figure 6 and Figure 7 It can be seen that a large number of activated platelets appear on the surface of the stent without modified surface and the platelets aggregate (the primary stage of thrombosis); a small number of platelets appear on the surface of the stent with textured surface, with irregular shape and enlarged, and the cells are ready to aggregate and adhere to each other. This is because when the platelets pass through the irregular groove surface, the morphology changes greatly after collision activation, and filamentous and lamellar feet are expressed; a small number of platelets adhere to the dimethyl sulfoxide surface of the stent obtained in Example 2 and Example 3, and the number of aggregated adhesion is reduced, which greatly reduces the adhesion of platelets compared to other surfaces. It shows that texture and DMSO modification have the effect of reducing platelet adhesion and aggregation.

[0077] (3) Antiplatelet activation test

[0078] The anticoagulant vascular stent with anticoagulant coating obtained in Examples 2 to 3 was subjected to an antiplatelet activation test. The anticoagulant vascular stent was implanted in a silicone tube, and a peristaltic pump system (Chongqing Jieheng peristaltic pump brand WT-600CA model) was used to perform peristaltic circulation of the silicone tube. The circulating blood used was the blood of experimental mice, and the circulation time was 10 minutes. The expression rate of the platelet activation marker CD62P in the blood was detected using a flow cytometer. The activation results of the stent anticoagulant coating (with a textured + DMSO surface) obtained in Example 2 and Example 3 on platelets are shown as follows, respectively. Figure 8 As shown in (d) and (e), and compared with the original scaffold without laser-etched U-shaped grooves and DMSO modification (i.e., the scaffold without modified surface, Figure 8 (b)), and a scaffold with only laser-etched U-shaped grooves but no DMSO modification (i.e., a scaffold with a textured surface, Figure 8 (c)) for comparison, and set up a blank control ( Figure 8 (a)). Figure 8 Comp-FITC-A represents the FITC-CD3 staining result (fluorescence intensity) in the multicolor antibody after adjustment compensation, and Comp-PE-A represents the PE-CD4 staining result (fluorescence intensity) in the multicolor antibody after adjustment compensation.

[0079] Depend on Figure 8 It can be seen that after the surface modification with dimethyl sulfoxide in Example 2 and Example 3, the expression rate of CD62P in the blood was reduced to 7.74% and 6.33% respectively, and the expression rate of CD62P in the blood after texture modification was 17.5%, and the modification with dimethyl sulfoxide reduced it by 9.76% and 11.17%. Compared with other surfaces, DMSO surface modification greatly reduced the activation effect of platelets, and the effect was the most obvious. The lower the expression rate of platelet marker CD62P, the lower the activation rate of platelets.

[0080] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing an anticoagulant vascular stent, characterized in that: The following steps are involved: The micro-textured stent is subjected to hydroxylation treatment and then immersed in dimethyl sulfoxide for grafting reaction to obtain the anticoagulant vascular stent; the inner surface of the micro-textured stent is provided with U-shaped grooves along the axial direction of the stent, and the U-shaped grooves cover the inner surface of the stent.

2. The preparation method according to claim 1, characterized in that: The hydroxylation solution used in the hydroxylation treatment is a mixed solution of concentrated sulfuric acid and hydrogen peroxide, the mass fraction of the concentrated sulfuric acid is 98%, the mass fraction of the hydrogen peroxide is 30%, and the volume ratio of concentrated sulfuric acid to hydrogen peroxide in the mixed solution is 7:3 to 3:

1.

3. The preparation method according to claim 1 or 2, characterized in that: The temperature of the hydroxylation treatment is 80-85° C. and the time is 20-30 minutes.

4. The preparation method according to claim 1, characterized in that: The grafting reaction temperature is 60-85° C. and the time is 6-12 hours.

5. The preparation method according to claim 4, characterized in that: The temperature of the grafting reaction is 65°C or 80°C.

6. The preparation method according to claim 1, characterized in that: After the hydroxylation treatment and the grafting reaction, the obtained scaffold material is washed with water and dried in sequence.

7. The preparation method according to claim 1, characterized in that: The width of a single U-shaped groove is 40 to 50 μm, and the depth is 20 to 40 μm.

8. The preparation method according to claim 1 or 7, characterized in that: The preparation method of the micro-textured scaffold comprises the following steps: Laser etching a U-shaped groove on the surface of the support substrate to obtain a micro-textured substrate; After the micro-textured substrate is heat-treated and formed, laser welding and laser engraving are performed in sequence to obtain the micro-textured bracket.

9. The preparation method according to claim 8, characterized in that: The heat treatment temperature is 580-600° C. and the time is 20-25 minutes.

10. The anticoagulant vascular stent prepared by the preparation method according to any one of claims 1 to 9, wherein the inner and outer surfaces of the anticoagulant vascular stent have a dimethyl sulfoxide molecular layer.