Preparation method of water-based hexagonal boron nitride high-temperature release agent

By the preparation method of modified hexagonal boron nitride, the problem of insufficient lubrication performance and adhesion of aqueous hexagonal boron nitride release agent at high temperature was solved, and water-based hexagonal boron nitride with excellent lubricity and high temperature adhesion was prepared. High-temperature mold release agent improves the flatness and mold release effect of the product.

CN119040058AActive Publication Date: 2024-11-29LIAONING BORON TECH CO LTD

Patent Information

Application Number
CN202411261158.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-29
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

The existing aqueous hexagonal boron nitride release agents have insufficient lubricating performance and adhesion at high temperatures, resulting in poor product flatness and mold release effect.

Method used

By the preparation method of modified hexagonal boron nitride, hydroxylated hexagonal boron nitride is carboxylated using γ-aminopropyltriethoxysilane and succinic anhydride, and is carboxylated with functional fillers and amino acid sodium tripolyphosphate. The grafting reaction was carried out to form modified hexagonal boron nitride, combined with a binder and a defoaming agent, and prepared a water-based hexagonal boron nitride high-temperature release agent.

Benefits of technology

The modified hexagonal boron nitride high-temperature release agent exhibits excellent lubricity and adhesion at high temperatures, forming a uniform lubricating film, reducing the friction coefficient, and improving the flatness and mold release effect of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the field of high-temperature release agents, and discloses a preparation method of a water-based hexagonal boron nitride high-temperature release agent which comprises the following components in parts by weight: 25-40 parts of modified hexagonal boron nitride, 35-65 parts of softened water, 10-25 parts of a binder and 0.3-0.5 part of a defoaming agent. The modified hexagonal boron nitride is prepared by carrying out carboxylation treatment on hydroxylated hexagonal boron nitride by using gamma-aminopropyltriethoxysilane and butanedioic anhydride, mixing the carboxylated hexagonal boron nitride with a functional filler, and then carrying out grafting reaction on the mixture and aminated sodium tripolyphosphate; wherein the functional filler is prepared by taking graphite-phase carbon nitride as a carrier to grow silicon dioxide nanoparticles in situ; the preparation method of the water-based hexagonal boron nitride high-temperature release agent comprises the following steps: weighing the raw materials in parts by weight, carrying out ball milling on the modified hexagonal boron nitride, adding softened water, stirring and dispersing, grinding by a high-speed dispersion machine after the dispersion is finished to obtain a mixture, and then adding the binder and the defoaming agent into the mixture and continuously stirring to prepare the water-based hexagonal boron nitride high-temperature release agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-temperature release agents, and in particular relates to a method for preparing a water-based hexagonal boron nitride high-temperature release agent. Background Art

[0002] In the field of metal and non-metal forming and processing, the emergence of molds has accelerated the efficiency of material forming. However, the qualified rate of material forming mainly depends on the release agent, which is a layer of functional material applied between the product and the mold. Its main function is to smoothly demold the product and ensure that the surface of the product is flat and smooth without scratches and other traces. There are many types of release agents, which are classified by solvents, mainly including: water-based release agents, oil-based release agents, and powder release agents. In the field of high-temperature processing, the release agent needs to have high lubricity and non-decomposition at high temperatures.

[0003] The prior art selects water-based hexagonal boron nitride as a demoulding agent. The water-based hexagonal boron nitride demoulding agent mainly relies on the poor wettability of molten metal to hexagonal boron nitride and the lamellar structure of hexagonal boron nitride. Hexagonal boron nitride has chemical inertness and high surface energy. Its dispersibility in the lubricating medium is poor and it is easy to agglomerate during the sliding process, which reduces its lubrication performance. At the same time, due to the different electronegativity of boron atoms and nitrogen atoms, extremely strong polarity is generated between the lamellar layers of hexagonal boron nitride, which can inhibit the slippage between the layers and reduce the friction reduction and anti-wear performance of hexagonal boron nitride. In addition, due to the low viscosity of water, it is difficult to form an elastic fluid dynamic lubrication film between the substrates, and there is a problem of a large friction coefficient, which affects the flatness of the product. Summary of the invention

[0004] In order to solve the deficiencies mentioned in the above background technology, the purpose of the present invention is to provide a method for preparing a water-based hexagonal boron nitride high-temperature release agent. By adding modified hexagonal boron nitride, the release agent is endowed with excellent lubricity and high-temperature adhesion, and the release effect is good.

[0005] The purpose of the present invention can be achieved through the following technical solutions: A method for preparing a water-based hexagonal boron nitride high-temperature mold release agent, wherein the water-based hexagonal boron nitride high-temperature mold release agent comprises the following components in parts by weight: 25-40 parts of modified hexagonal boron nitride, 35-65 parts of softened water, 10-25 parts of a binder, and 0.3-0.5 parts of a defoaming agent; The modified hexagonal boron nitride is prepared by carboxylating hydroxylated hexagonal boron nitride with γ-aminopropyltriethoxysilane and succinic anhydride, mixing the hydroxylated hexagonal boron nitride with a functional filler, and then grafting the hydroxylated hexagonal boron nitride with ammoniated sodium tripolyphosphate, wherein the functional filler is prepared by in-situ growth of silicon dioxide nanoparticles using graphite phase carbon nitride as a carrier; The preparation method of the water-based hexagonal boron nitride high-temperature release agent comprises the following steps: Weigh each raw material by weight, ball-mill the modified hexagonal boron nitride to 3-5 μm in a ball mill, add softened water and stir and disperse for 1.5-2 h. After dispersion, grind it in a high-speed disperser for 4-6 h to obtain a mixture with a fineness of 1-5 μm, then add a binder and a defoamer to the mixture and continue stirring for 0.5-1 h to prepare a water-based hexagonal boron nitride high-temperature release agent.

[0006] Preferably, the binder is one or more combinations of aluminum dihydrogen phosphate, aluminum sol, and aluminum sulfate.

[0007] Preferably, the defoamer is a silicone defoamer.

[0008] Preferably, the preparation method of the modified hexagonal boron nitride comprises the following steps: (1) Put hexagonal boron nitride in a reactor, add sodium hydroxide solution and stir for 42-48 hours, centrifuge, wash and dry to prepare hydroxylated hexagonal boron nitride; (2) ultrasonically dispersing graphite phase carbon nitride in deionized water, then adding anhydrous citric acid and continuing ultrasonication for 1.5 to 2 hours to prepare protonated graphite phase carbon nitride; (3) Sodium silicate was placed in a reactor, deionized water was added and mixed, ethanol was slowly added and the temperature was raised to 75-85°C, protonated graphite carbon nitride was added, the pH value of the system was adjusted to 5-6 with concentrated sulfuric acid solution, and ethanol was added. The reaction was stopped when the reaction temperature was maintained at 75-85°C, and the supernatant was discarded after aging for 1-2 hours, and the mixture was washed with deionized water and ethanol, and dried in a freeze dryer to prepare a functionalized filler; (4) γ-aminopropyltriethoxysilane and succinic anhydride are placed in N,N-dimethylformamide and stirred at 75-90°C for 2-5 hours to form a mixed solution, hydroxylated hexagonal boron nitride and functionalized filler are ultrasonically dispersed in N,N-dimethylformamide, deionized water is added and mixed, and then added to the mixed solution and stirred for 4-6 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried to prepare a carboxylated composite material; (5) dissolving sodium tripolyphosphate and γ-aminopropyltriethoxysilane in toluene solvent, reacting at 65-75° C. for 5-6 hours, and after the reaction is completed, centrifuging, washing, and drying to prepare aminated sodium tripolyphosphate; (6) The carboxyl composite material is ultrasonically dispersed in deionized water to obtain a dispersion, and deionized water, 1-ethyl-(3-dimethylaminopropyl) carbodiimide and N-hydroxysuccinimide are mixed to obtain a mixed solution. The mixed solution is added to the dispersion and allowed to stand for 0.5 to 1 h. Aminated sodium tripolyphosphate is then added and stirred at 30 to 50 °C for 5 to 6 h. After the reaction is completed, the modified hexagonal boron nitride is prepared by centrifugation, washing and drying.

[0009] Preferably, in step (3), the mass ratio of sodium silicate to protonated graphite phase carbon nitride is 20:3-7.

[0010] Preferably, in step (4), the mass ratio of γ-aminopropyltriethoxysilane, succinic anhydride, hydroxylated hexagonal boron nitride and functionalized filler is 7-10:9-12:1-3:0.5-1.

[0011] Preferably, in step (5), the mass ratio of sodium tripolyphosphate to γ-aminopropyltriethoxysilane is 1:1.4-2.

[0012] Preferably, in step (6), the mass ratio of 1-ethyl-(3-dimethylaminopropyl)carbodiimide to N-hydroxysuccinimide is 7.5-8.5:1.

[0013] Beneficial effects of the present invention: The present invention uses sodium hydroxide solution to hydroxylate hexagonal boron nitride, and uses citric acid to protonate graphite phase carbon nitride to form a positive charge center, and then SiO3, a precursor of silicon dioxide, is used to 2- The silicon dioxide nanoparticles are adsorbed on the surface of graphite carbon nitride by electrostatic attraction, and then the silicon dioxide nanoparticles are in-situ grown on the surface of graphite carbon nitride to form a functionalized filler. The addition of the functionalized filler can give the release agent excellent high temperature resistance, chemical stability and lubricity, and has sufficient adsorption strength at high temperature, and can form a complete and uniform lubricating film during the deformation of the product. The present invention further uses γ-aminopropyltriethoxysilane and succinic anhydride to carboxylate the hydroxylated hexagonal boron nitride and the functionalized filler, and at the same time uses γ-aminopropyltriethoxysilane to amino-modify sodium tripolyphosphate and then performs an amidation reaction with the carboxylated composite material. The introduced sodium phosphate group has stronger water solubility. The sodium tripolyphosphate, hexagonal boron nitride and the functionalized filler are firmly bonded through chemical bonds, and can be dispersed more evenly in the matrix. The modified hexagonal boron nitride can reduce its surface polarity and inhibit its agglomeration in the matrix, thereby reducing its interlayer friction. DETAILED DESCRIPTION

[0014] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0015] Example 1 A method for preparing modified hexagonal boron nitride comprises the following steps: (1) 2.5 g of hexagonal boron nitride was placed in a reactor, a sodium hydroxide solution with a mass concentration of 40% was added and stirred for 48 hours, and then centrifuged, washed and dried to prepare hydroxylated hexagonal boron nitride; (2) 5 g of graphite carbon nitride was ultrasonically dispersed in 100 mL of deionized water, and then 35.7 g of anhydrous citric acid was added and ultrasonicated for 2 h to prepare protonated graphite carbon nitride; (3) 40 g of sodium silicate was placed in a reactor, 120 mL of deionized water was added and mixed, 10 mL of ethanol was slowly added and the temperature was raised to 80 °C, 10.5 g of protonated graphite carbon nitride was added, the pH value of the system was adjusted to 6 with concentrated sulfuric acid solution, and then 80 mL of ethanol was added. The reaction was stopped when the reaction temperature was maintained at 80 °C, and the supernatant was discarded after aging for 2 h, and the mixture was washed with deionized water and ethanol, and dried in a freeze dryer to prepare a functionalized filler; (4) 7.3 g of γ-aminopropyltriethoxysilane and 9.5 g of succinic anhydride were dissolved in 100 mL of N, N-dimethylformamide and stirred at 85 °C for 4 h to form a mixed solution. 2.6 g of hydroxylated hexagonal boron nitride and 0.7 g of functionalized filler were ultrasonically dispersed in 100 mL of N, N-dimethylformamide, 10 mL of deionized water was added and mixed, and then added to the mixed solution and stirred for 5 h. After the reaction was completed, the mixture was centrifuged, washed and dried to prepare a carboxylated composite material. (5) 4 g of sodium tripolyphosphate and 6.4 g of γ-aminopropyltriethoxysilane were dissolved in 50 mL of toluene solvent and reacted at 70° C. for 6 h. After the reaction was completed, the mixture was centrifuged, washed, and dried to prepare aminated sodium tripolyphosphate; (6) 1.5 g of the carboxylated composite material was ultrasonically dispersed in 150 mL of deionized water to obtain a dispersion, 60 mL of deionized water, 4 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 0.5 g of N-hydroxysuccinimide were mixed evenly to obtain a mixed solution, the mixed solution was added to the dispersion, allowed to stand for 0.5 h, and then 6.5 g of amino sodium tripolyphosphate was added. The mixture was stirred and reacted at 45 °C for 6 h. After the reaction was completed, the mixture was centrifuged, washed and dried to obtain modified hexagonal boron nitride.

[0016] Example 2 A water-based hexagonal boron nitride high-temperature release agent comprises the following components in parts by weight: 27 parts of the modified hexagonal boron nitride prepared in Example 1, 35 parts of softened water, 12 parts of a binder aluminum dihydrogen phosphate, and 0.3 parts of Deqian defoamer 6800.

[0017] The preparation method of the water-based hexagonal boron nitride high-temperature release agent comprises the following steps: Weigh each raw material by weight, ball-mill the modified hexagonal boron nitride to 3-5 μm in a ball mill, add softened water and stir and disperse for 2 h. After dispersion, grind it in a high-speed disperser for 5 h to obtain a mixture with a fineness of 1-5 μm, then add a binder and a defoamer to the mixture and continue stirring for 1 h to prepare a water-based hexagonal boron nitride high-temperature release agent.

[0018] Example 3 A water-based hexagonal boron nitride high-temperature release agent comprises the following components in parts by weight: 35 parts of the modified hexagonal boron nitride prepared in Example 1, 52 parts of softened water, 17 parts of aluminum dihydrogen phosphate as a binder, and 0.4 parts of Deqian defoamer 6800.

[0019] The preparation method of the above-mentioned water-based hexagonal boron nitride high-temperature release agent is the same as that of Example 2.

[0020] Example 4 A water-based hexagonal boron nitride high-temperature release agent comprises the following components in parts by weight: 40 parts of the modified hexagonal boron nitride prepared in Example 1, 63 parts of softened water, 24 parts of aluminum dihydrogen phosphate as a binder, and 0.5 parts of Deqian defoamer 6800.

[0021] The preparation method of the above-mentioned water-based hexagonal boron nitride high-temperature release agent is the same as that of Example 2.

[0022] Comparative Example 1 A method for preparing modified hexagonal boron nitride comprises the following steps: (1) 2.5 g of hexagonal boron nitride was placed in a reactor, a sodium hydroxide solution with a mass concentration of 40% was added and stirred for 48 hours, and then centrifuged, washed and dried to prepare hydroxylated hexagonal boron nitride; (2) 7.3 g of γ-aminopropyltriethoxysilane and 9.5 g of succinic anhydride were dissolved in 100 mL of N, N-dimethylformamide and stirred at 85 °C for 4 h to form a mixed solution. 2.6 g of hydroxylated hexagonal boron nitride and 0.7 g of nano-silicon dioxide were ultrasonically dispersed in 100 mL of N, N-dimethylformamide, 10 mL of deionized water was added and mixed, and then added to the mixed solution and stirred for 5 h. After the reaction was completed, the mixture was centrifuged, washed and dried to prepare a carboxylated composite material. (3) 4 g of sodium tripolyphosphate and 6.4 g of γ-aminopropyltriethoxysilane were dissolved in 50 mL of toluene solvent and reacted at 70° C. for 6 h. After the reaction was completed, the mixture was centrifuged, washed, and dried to prepare aminated sodium tripolyphosphate; (4) 1.5 g of the carboxylated composite material was ultrasonically dispersed in 150 mL of deionized water to obtain a dispersion, 60 mL of deionized water, 4 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 0.5 g of N-hydroxysuccinimide were mixed evenly to obtain a mixed solution, the mixed solution was added to the dispersion, allowed to stand for 0.5 h, and then 6.5 g of amino sodium tripolyphosphate was added. The mixture was stirred and reacted at 45 °C for 6 h. After the reaction was completed, the mixture was centrifuged, washed and dried to obtain modified hexagonal boron nitride.

[0023] Comparative Example 2 A water-based hexagonal boron nitride high-temperature release agent comprises the following components in parts by weight: 40 parts of modified hexagonal boron nitride prepared in Comparative Example 1, 63 parts of softened water, 24 parts of binder aluminum dihydrogen phosphate, and 0.5 parts of Deqian defoamer 6800.

[0024] The preparation method of the above-mentioned water-based hexagonal boron nitride high-temperature release agent is the same as that of Example 2.

[0025] Comparative Example 3 A water-based hexagonal boron nitride high-temperature release agent comprises the following components in parts by weight: 30 parts of hexagonal boron nitride, 7 parts of nano-silicon dioxide, 3 parts of graphite phase carbon nitride, 2 parts of sodium tripolyphosphate, 63 parts of softened water, 24 parts of binder aluminum dihydrogen phosphate, and 0.5 parts of Deqian defoamer 6800.

[0026] The preparation method of the above-mentioned water-based hexagonal boron nitride high-temperature release agent is the same as that of Example 2.

[0027] Performance Testing The release agents prepared in Examples 2-4 and Comparative Examples 2-3 were tested for performance: (1) High-temperature adhesion performance test: Using Q-235 as a test piece, the release agents prepared in Examples 2-4 and Comparative Examples 2-3 were tested for adhesion performance at different temperatures. The data results are shown in Table 1.

[0028] (2) Lubrication performance test: Using SUS-304 as a test piece, the friction coefficient of the release agents prepared in Examples 2-4 and Comparative Examples 2-3 was measured, and the data results are shown in Table 1.

[0029] Table 1 Test results of sample performance.

[0030] As can be seen from the data in Table 1, the release agent prepared in Examples 2-4 of the present invention has sufficient adsorption strength at high temperature, and has a low friction coefficient, and has good lubrication and demoulding performance. In Comparative Example 2, the functional filler is replaced by nano-silicon dioxide in equal amounts, and the measured adhesion at high temperature is significantly reduced compared with Examples 2-4, and the friction coefficient is slightly lower than that of Examples 2-4, indicating that the addition of graphite phase carbon nitride can improve the high-temperature adhesion and lubricity of the release agent. In Comparative Example 3, hexagonal boron nitride, nano-silicon dioxide and graphite phase carbon nitride are simply mixed, and the measured friction coefficient is higher than that of Examples 2-4, and the high-temperature adhesion is slightly lower than that of Examples 2-4, because its poor water solubility and dispersibility in the matrix lead to reduced performance.

[0031] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0032] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A method for preparing a water-based hexagonal boron nitride high-temperature release agent, characterized in that: The water-based hexagonal boron nitride high-temperature release agent comprises the following components in parts by weight: 25-40 parts of modified hexagonal boron nitride, 35-65 parts of softened water, 10-25 parts of a binder, and 0.3-0.5 parts of a defoamer; The modified hexagonal boron nitride is prepared by carboxylating hydroxylated hexagonal boron nitride with γ-aminopropyltriethoxysilane and succinic anhydride, mixing the hydroxylated hexagonal boron nitride with a functional filler, and then grafting the hydroxylated hexagonal boron nitride with ammoniated sodium tripolyphosphate, wherein the functional filler is prepared by in-situ growth of silicon dioxide nanoparticles using graphite phase carbon nitride as a carrier; The preparation method of the water-based hexagonal boron nitride high-temperature release agent comprises the following steps: Weigh each raw material by weight, ball-mill the modified hexagonal boron nitride to 3-5 μm in a ball mill, add softened water and stir and disperse for 1.5-2 h. After dispersion, grind it in a high-speed disperser for 4-6 h to obtain a mixture with a fineness of 1-5 μm, then add a binder and a defoamer to the mixture and continue stirring for 0.5-1 h to prepare a water-based hexagonal boron nitride high-temperature release agent.

2. The method for preparing the water-based hexagonal boron nitride high-temperature release agent according to claim 1, characterized in that: The binder is one or more combinations of aluminum dihydrogen phosphate, aluminum sol, and aluminum sulfate.

3. The method for preparing the water-based hexagonal boron nitride high-temperature release agent according to claim 1, characterized in that: The defoamer is an organosilicon defoamer.

4. The method for preparing the water-based hexagonal boron nitride high-temperature release agent according to claim 1, characterized in that: The preparation method of the modified hexagonal boron nitride comprises the following steps: (1) Put hexagonal boron nitride in a reactor, add sodium hydroxide solution and stir for 42-48 hours, centrifuge, wash and dry to prepare hydroxylated hexagonal boron nitride; (2) ultrasonically dispersing graphite phase carbon nitride in deionized water, then adding anhydrous citric acid and continuing ultrasonication for 1.5 to 2 hours to prepare protonated graphite phase carbon nitride; (3) Sodium silicate was placed in a reactor, deionized water was added and mixed, ethanol was slowly added and the temperature was raised to 75-85°C, protonated graphite carbon nitride was added, the pH value of the system was adjusted to 5-6 with concentrated sulfuric acid solution, and ethanol was added. The reaction was stopped when the reaction temperature was maintained at 75-85°C, and the supernatant was discarded after aging for 1-2 hours, and the mixture was washed with deionized water and ethanol, and dried in a freeze dryer to prepare a functionalized filler; (4) γ-aminopropyltriethoxysilane and succinic anhydride are placed in N,N-dimethylformamide and stirred at 75-90°C for 2-5 hours to form a mixed solution, hydroxylated hexagonal boron nitride and functionalized filler are ultrasonically dispersed in N,N-dimethylformamide, deionized water is added and mixed, and then added to the mixed solution and stirred for 4-6 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried to prepare a carboxylated composite material; (5) dissolving sodium tripolyphosphate and γ-aminopropyltriethoxysilane in toluene solvent, reacting at 65-75° C. for 5-6 hours, and after the reaction is completed, centrifuging, washing, and drying to prepare aminated sodium tripolyphosphate; (6) The carboxyl composite material is ultrasonically dispersed in deionized water to obtain a dispersion, and deionized water, 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide are mixed to obtain a mixed solution. The mixed solution is added to the dispersion and allowed to stand for 0.5 to 1 h. Aminated sodium tripolyphosphate is then added and stirred at 30 to 50 °C for 5 to 6 h. After the reaction is completed, the modified hexagonal boron nitride is prepared by centrifugation, washing and drying.

5. The method for preparing the water-based hexagonal boron nitride high-temperature release agent according to claim 4, characterized in that: In the step (3), the mass ratio of sodium silicate to protonated graphite phase carbon nitride is 20:3-7.

6. The method for preparing a water-based hexagonal boron nitride high-temperature release agent according to claim 4, characterized in that: In the step (4), the mass ratio of γ-aminopropyltriethoxysilane, succinic anhydride, hydroxylated hexagonal boron nitride and functionalized filler is 7-10:9-12:1-3:0.5-1.

7. The method for preparing a water-based hexagonal boron nitride high-temperature release agent according to claim 4, characterized in that: In the step (5), the mass ratio of sodium tripolyphosphate to γ-aminopropyltriethoxysilane is 1:1.4-2.

8. The method for preparing a water-based hexagonal boron nitride high-temperature release agent according to claim 4, characterized in that: In the step (6), the mass ratio of 1-ethyl-(3-dimethylaminopropyl)carbodiimide to N-hydroxysuccinimide is 7.5-8.5:1.

Citation Information

Patent Citations

  • Non-graphite type lubricant for hot die forging of metal and preparation method of non-graphite type lubricant

    CN102533423A

  • Hexagonal boron nitride base slide plate lubricant and preparation method thereof

    CN103509641A

  • Ultraviolet-resistant molybdenum disulfide dry-film lubricant for self-locking nut and preparation method of lubricant

    CN106590855A

  • Aqueous boron nitride coating capable of binding at low temperature and being used at high temperature

    CN109021628A

  • Durable paint used for glass forming die demoulding

    CN109897408A

Cited By

  • High-temperature release agent and preparation method thereof

    CN120865985A

  • Method for reinforcing outer surface of casting in precision valve body pouring