Rubber composition, rubber compound and preparation method thereof
React with white carbon black by using 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde in the rubber composition and chain with rubber molecular Cross-linking, combined with anti-aging agent and anti-coke agent, solves the problems of high-temperature heat generation and difficult processing of rubber compositions, achieves low heat generation, high hardness and wear resistance, simplifies the mixing process and extends the service life.
Patent Information
- Application Number
- CN202411021280.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-26
AI Technical Summary
The existing rubber compositions have high heat generation performance at high temperatures and have high requirements for mixing processes and processing equipment, which leads to the charring of the rubber and affects the service life and production efficiency of the tire.
1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde is used as a multifunctional additive to reduce heat generation by reacting with white carbon black, and The rubber molecular chain is directly involved in cross-linking during vulcanization to avoid constant temperature mixing control. At the same time, anti-aging agents, stearic acid, zinc oxide, promoters and anti-coke agents are added to delay aging and control the vulcanization rate.
It significantly reduces the heat generation performance of the rubber composition, improves its processability and hardness, wear resistance and tear resistance of vulcanized rubber, simplifies the mixing process, reduces the requirements for processing equipment, and extends vulcanized rubber The service life is avoided from premature scorching of the glue.
Smart Images

Figure BDA0004969066830000061 
Figure BDA0004969066830000071 
Figure BDA0004969066830000091
Abstract
Description
Technical Field
[0001] The present invention relates to the field of rubber technology, and in particular to a rubber composition, a rubber compound and a preparation method thereof. Background Art
[0002] At present, the requirements for heat generation performance of tires for different purposes, including engineering tires, aircraft tires, all-steel tires and passenger car tires, are getting higher and higher. Since rubber is a poor conductor of heat, as the tire speed and load gradually increase, the temperature inside the rubber compound also increases, resulting in problems such as heat delamination caused by failure to dissipate heat in time, belt puncture caused by groove bottom cracking, and shoulder and crown voids caused by high heat generation. Therefore, the low heat generation performance of tire rubber has always been the focus of research. As for the way to reduce the heat generation of rubber, currently, white carbon black and silane coupling agents are mainly used to replace traditional reinforcing filler carbon black, which has derived a series of white carbon black dispersants, modified SBR and modified BR materials that improve the dispersion of white carbon black and reduce the heat generation of rubber. Silane coupling agent can react with white carbon black at one end and release sulfur at the other end to participate in the vulcanization cross-linking reaction and connect with the rubber molecular chain, thereby improving the dispersion of white carbon black and reducing the heat generation of the rubber. However, since silane coupling agent contains sulfur element, it has high requirements for the mixing processing temperature of the rubber compound. If the mixing processing temperature is too high, the silane coupling agent will release sulfur element prematurely to participate in the cross-linking reaction. As the amount of white carbon black and silane coupling agent gradually increases, the requirements for mixing technology and processing equipment are getting higher and higher.
[0003] The Chinese patent application with the patent application publication number CN116410524A proposes a low-heat tread rubber for engineering tires and a preparation method thereof, which uses a high content of white carbon black in the formula to reduce the heat generation performance of the rubber material, and adds a high content of silane coupling agent to not only improve the anti-reversion, tearing performance and flexural performance of the rubber material, but also improve the physical properties of the engineering tire radial tire, thereby extending the service life of the tire, reducing costs and improving benefits. It mainly reduces the heat generation of the vulcanized rubber by adding white carbon black and silane coupling agent, but the mixing process after adding the silane coupling agent is strictly required, that is, the temperature of the silanization reaction cannot be too high, otherwise it will cause the sulfur in the silane to be released, resulting in premature cross-linking of the rubber material, thereby causing the rubber material to be scorched prematurely and cannot be used.
[0004] The Chinese patent application with patent application publication number CN115678122A proposes a tread rubber, preparation method, application and low heat build-up load-bearing radial tire of a low heat build-up tire, which mainly provides the rubber with suitable low heat build-up performance by adding white carbon black and silane coupling agent and adjusting the appropriate ratio of the two.
[0005] A Chinese patent application with patent application publication number CN102746536A proposes a formula for low heat generation aviation tire tread rubber. The tread rubber is made of 1# smoke sheet rubber as the main material, and is mixed with medium-super wear-resistant carbon black, highly dispersed white carbon black, white carbon black dispersant, silane coupling agent, heat stabilizer HS-80, thermal conductivity enhancer TB-S and anti-vulcanization reversion agent WK-901 as auxiliary materials. White carbon black and silane coupling agent are still added to reduce the heat generation of the rubber.
[0006] All of the above methods reduce the heat generation of the rubber compound by adding white carbon black and silane coupling agent, but there is still a lack of additives that can replace the silane coupling agent to improve the dispersion of white carbon black and simplify the mixing process. Summary of the invention
[0007] The main purpose of the present invention is to provide a rubber composition, a mixed rubber and a preparation method thereof, so as to solve the problems in the prior art of high heat generation of the rubber material and high requirements on the mixing process and processing equipment.
[0008] To achieve the above-mentioned object, according to one aspect of the present invention, a rubber composition is provided, which comprises, by weight, 50 to 90 parts of natural rubber, 10 to 50 parts of styrene-butadiene rubber, 5 to 30 parts of carbon black, 15 to 60 parts of white carbon black, 1.8 to 10.5 parts of 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde, 2.3 to 9 parts of an antioxidant, 1 to 2.5 parts of stearic acid, 1.5 to 5 parts of zinc oxide, 1 to 4 parts of an accelerator, 1 to 3 parts of sulfur and 0.1 to 0.2 parts of a scorch retarder.
[0009] Furthermore, the rubber composition comprises, by weight: 55 to 90 parts of natural rubber, 15 to 45 parts of styrene-butadiene rubber, 8 to 25 parts of carbon black, 15 to 55 parts of white carbon black, 3.5 to 7.0 parts of 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde, 2.6 to 6 parts of antioxidant, 1.5 to 2 parts of stearic acid, 2 to 5 parts of zinc oxide, 1.1 to 3.6 parts of accelerator, 1 to 2.5 parts of sulfur and 0.1 to 0.2 parts of scorch retarder.
[0010] Furthermore, the styrene-butadiene rubber is solution-polymerized styrene-butadiene rubber SOL 5251H; and / or the brand of carbon black is selected from any one or more of N115, N121, N134, N110, N234 and N220; and / or the brand of white carbon black is selected from any one or more of Z1165MP, Z200MP, Z1115MP and VN3; and / or the anti-scorch agent is anti-scorch agent CTP.
[0011] Furthermore, the antioxidant is selected from any one or more of antioxidant wax, antioxidant RD and antioxidant 4020.
[0012] Furthermore, the antioxidant is a combination of antioxidant wax, antioxidant RD and antioxidant 4020, and the mass ratio of antioxidant wax, antioxidant RD and antioxidant 4020 is 0.8-1.5:0.5-2.5:1-2.5, preferably 0.8-1.5:0.6-2.0:1.2-2.5.
[0013] Furthermore, the accelerator is a NS accelerator and / or a diphenylguanidine accelerator.
[0014] Furthermore, the accelerator is a combination of an NS accelerator and a diphenylguanidine accelerator, and the mass ratio of the NS accelerator to the diphenylguanidine accelerator is 0.5-2:0.5-2, preferably 0.5-1.8:0.6-1.8.
[0015] According to another aspect of the present invention, a rubber mix is provided, which is obtained by mixing a rubber composition, and the rubber composition is the rubber composition mentioned above.
[0016] According to another aspect of the present invention, there is provided a method for preparing the above-mentioned rubber mix, the method comprising: step S1, mixing natural rubber, styrene-butadiene rubber, carbon black, white carbon black, zinc oxide, stearic acid, antioxidant, 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde in one stage and performing the first batch of mixing to obtain a first masterbatch; step S2, mixing the first masterbatch in two stages and performing the second batch of mixing to obtain a second masterbatch; and step S3, mixing the second masterbatch, sulfur, accelerator and scorch retarder in the third batch of mixing to obtain a rubber mix.
[0017] Furthermore, the speed of the first mixing is 42-48 rpm, and / or the time of the first mixing is 2-5 min, and / or the temperature of the first row of rubber is 160-165° C.; and / or the speed of the second mixing is 40-45 rpm, and / or the time of the second mixing is 2-4 min, and / or the temperature of the second row of rubber is 155-160° C.; and / or the speed of the final mixing is 28-32 rpm, and / or the time of the final mixing is 1.5-3 min, and / or the temperature of the third row of rubber is 100-110° C.
[0018] By applying the technical solution of the present invention, the rubber composition of the present application is mainly prepared by adding a multifunctional additive, namely 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde, which has two alkoxy groups at both ends of its molecular chain, which can react with the hydroxyl groups on the surface of silica respectively, thereby reducing the surface polarity of silica, and further improving the dispersion of silica, that is, reducing the heat generation of the rubber composition. At the same time, the 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde molecular chain contains conjugated olefins and methyl substituents, that is, it contains active α-H and carbon-carbon double bonds. During vulcanization, its α carbon atom can directly participate in the cross-linking reaction process between rubber and sulfur, so there is no need for special constant temperature mixing control of the mixing process, thereby greatly improving the processability of the rubber composition; adding antioxidants can delay rubber aging, thereby extending the service life of the vulcanized rubber; adding stearic acid, zinc oxide, accelerators, and sulfur can promote the cross-linking reaction process between them and the rubber molecular chain, thereby forming a three-dimensional network structure and accelerating vulcanization, thereby improving the hardness, wear resistance and tear resistance of the vulcanized rubber; adding anti-scorching agents can control the vulcanization rate and prevent the rubber composition from scorching prematurely, thereby improving the quality of the vulcanized rubber. In addition, the rubber composition of the present invention not only has low heat generation, but is also easy to process, i.e., there is no need to maintain a constant temperature mixing time during mixing. At the same time, the rubber composition of the present invention has low requirements on the cooling performance of the processing equipment, whether the rotation speed can be automatically adjusted, and other performances, and even if a traditional internal mixer is used for mixing, a good mixing effect can be achieved.
[0019] Specific implementation methods
[0020] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0021] As analyzed in the background technology of this application, the prior art has problems such as high heat generation of rubber and high requirements for mixing technology and processing equipment. In order to solve the above problems, this application provides a rubber composition, a mixed rubber and a preparation method thereof.
[0022] In a typical embodiment of the present application, a rubber composition is provided, which includes, by weight, 50 to 90 parts of natural rubber, 10 to 50 parts of styrene-butadiene rubber, 5 to 30 parts of carbon black, 15 to 60 parts of white carbon black, 1.8 to 10.5 parts of 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde, 2.3 to 9 parts of an antioxidant, 1 to 2.5 parts of stearic acid, 1.5 to 5 parts of zinc oxide, 1 to 4 parts of an accelerator, 1 to 3 parts of sulfur and 0.1 to 0.2 parts of a scorch retarder.
[0023] The rubber composition of the present application is mainly prepared by adding a multifunctional additive, namely 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde, which has two alkoxy groups at both ends of its molecular chain, which can react with the hydroxyl groups on the surface of silica respectively, thereby reducing the surface polarity of silica, and then improving the dispersion of silica, that is, reducing the heat generation of the rubber composition. At the same time, the 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde molecular chain contains conjugated olefins and methyl substituents, that is, it contains active α-H and carbon-carbon double bonds. During vulcanization, its α carbon atom can directly participate in the cross-linking reaction process between rubber and sulfur, so there is no need for special constant temperature mixing control of the mixing process, thereby greatly improving the processability of the rubber composition; adding antioxidants can delay rubber aging, thereby extending the service life of the vulcanized rubber; adding stearic acid, zinc oxide, accelerators, and sulfur can promote the cross-linking reaction process between them and the rubber molecular chain, thereby forming a three-dimensional network structure and accelerating vulcanization, thereby improving the hardness, wear resistance and tear resistance of the vulcanized rubber; adding anti-scorching agents can control the vulcanization rate and prevent the rubber composition from scorching prematurely, thereby improving the quality of the vulcanized rubber. In addition, the rubber composition of the present invention not only has low heat generation, but is also easy to process, i.e., there is no need to maintain a constant temperature mixing time during mixing. At the same time, the rubber composition of the present invention has low requirements on the cooling performance of the processing equipment, whether the rotation speed can be automatically adjusted, and other performances, and even if a traditional internal mixer is used for mixing, a good mixing effect can be achieved.
[0024] In one embodiment of the present application, the rubber composition includes, by weight: 55 to 90 parts of natural rubber, 15 to 45 parts of styrene-butadiene rubber, 8 to 25 parts of carbon black, 15 to 55 parts of white carbon black, 3.5 to 7.0 parts of 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde, 2.6 to 6 parts of antioxidant, 1.5 to 2 parts of stearic acid, 2 to 5 parts of zinc oxide, 1.1 to 3.6 parts of accelerator, 1 to 2.5 parts of sulfur and 0.1 to 0.2 parts of scorch retarder.
[0025] The component contents of the rubber composition are preferably within the above ranges, which helps to further enhance the synergistic effect of the components, thereby improving the dispersibility of silica, reducing the heat generation of the rubber composition, and improving the processability of the rubber.
[0026] In one embodiment of the present application, the styrene-butadiene rubber is solution-polymerized styrene-butadiene rubber SOL 5251H; and / or the brand of carbon black is selected from any one or more of N115, N121, N134, N110, N234 and N220; and / or the brand of white carbon black is selected from any one or more of Z1165MP, Z200MP, Z1115MP and VN3; and / or the anti-scorch agent is anti-scorch agent CTP.
[0027] The type of styrene-butadiene rubber is preferably within the above range, which is helpful for mixing and vulcanization, thereby improving the processing performance of the rubber composition; the type of carbon black is preferably within the above range, which is helpful for improving the hardness and conductivity of the vulcanized rubber. The type of white carbon black is preferably within the above range, which is helpful for improving the reaction effect with 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde, thereby reducing the heat generation of the rubber composition; the type of scorch retarder is preferably within the above range, which is helpful for controlling the vulcanization rate and avoiding premature scorching of the rubber composition as much as possible, thereby improving the quality of the vulcanized rubber.
[0028] In one embodiment of the present application, the antioxidant is selected from any one or more of antioxidant wax, antioxidant RD and antioxidant 4020.
[0029] The type of antioxidant is preferably within the above range, which helps to delay the aging of the vulcanized rubber, thereby helping to extend the service life of the vulcanized rubber. At the same time, the above preferred antioxidant helps to reduce costs.
[0030] In one embodiment of the present application, the antioxidant is a combination of antioxidant wax, antioxidant RD and antioxidant 4020, and the mass ratio of antioxidant wax, antioxidant RD and antioxidant 4020 is 0.8-1.5:0.5-2.5:1-2.5, preferably 0.8-1.5:0.6-2.0:1.2-2.5.
[0031] The preferred antioxidant is a combination of antioxidant wax, antioxidant RD and antioxidant 4020 and controlling their mass ratio within the above range, which helps to further improve the coordination effect of functional groups between different types of antioxidants, thereby helping to inhibit the breakage of rubber molecular chains and further improve the service life of the vulcanized rubber.
[0032] In one embodiment of the present application, the accelerator is a NS accelerator and / or a diphenylguanidine accelerator.
[0033] The preferred accelerators are of the above types, which help to accelerate the vulcanization reaction between sulfur and rubber molecules to form a uniform and stable cross-linked structure, thereby helping to improve the hardness, abrasion resistance and tear strength of the vulcanized rubber.
[0034] In one embodiment of the present application, the accelerator is a combination of an NS accelerator and a diphenylguanidine accelerator, and the mass ratio of the NS accelerator to the diphenylguanidine accelerator is 0.5-2:0.5-2, preferably 0.5-1.8:0.6-1.8.
[0035] Preferably, the accelerator is a combination of NS accelerator and diphenylguanidine accelerator and controlling their mass ratio within the above range helps to further improve the vulcanization uniformity and form a uniform and stable cross-linked structure, thereby helping to improve the hardness, wear resistance and tear strength of the vulcanized rubber.
[0036] In another typical embodiment of the present application, a rubber mix is provided, which is obtained by mixing a rubber composition, and the rubber composition is the rubber composition mentioned above.
[0037] The rubber compound obtained by mixing the rubber composition not only has low heat generation and is easy to process, but also has high hardness, wear resistance, tear strength and other properties.
[0038] In another typical embodiment of the present application, a method for preparing the above-mentioned rubber mixture is provided, and the preparation method comprises: step S1, mixing natural rubber, styrene-butadiene rubber, carbon black, white carbon black, zinc oxide, stearic acid, antioxidant, and 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde in a first stage and a first batch of rubber to obtain a first masterbatch; step S2, mixing the first masterbatch in a second stage and a second batch of rubber to obtain a second masterbatch; and step S3, finally mixing the second masterbatch, sulfur, an accelerator, and a scorch retarder in a third batch of rubber to obtain a rubber mixture.
[0039] The present application uniformly disperses carbon black, white carbon black, zinc oxide, stearic acid, antioxidant, 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethyl acetaldehyde into natural rubber and styrene-butadiene rubber through a first-stage mixing, forming a masterbatch with good dispersibility and plasticity, which is beneficial to subsequent processing, and during the first-stage mixing, there is no need to perform constant temperature mixing control, which greatly improves the simple operability of the processing process. After the first-stage masterbatch is mixed in two stages, the dispersion effect of the above-mentioned raw materials can be further enhanced, thereby strengthening the interaction between 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethyl acetaldehyde and white carbon black, thereby improving the heat generation performance of the vulcanized rubber. Adding sulfur, accelerator and anti-scorch agent during the final refining process can make sulfur, accelerator and anti-scorch agent fully and evenly dispersed, while preventing sulfur from undergoing a cross-linking reaction in advance, thereby improving the hardness, wear resistance and tear resistance of the vulcanized rubber. In addition, the mixing process of the present invention is not only simple, but also can meet the processing conditions for preparing low-heat vulcanized rubber, that is, there is no need to maintain a constant temperature mixing time for the reaction of silane and white carbon black during mixing, as in the conventional solution of adding a silane coupling agent. This is attributed to the fact that 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde contains active carbon-carbon double bonds and α carbon atoms, and can directly react with sulfur during the vulcanization of the rubber compound. Its reaction mechanism with sulfur is consistent with the reaction mechanism of diene rubber with sulfur. High temperature during mixing will not cause a cross-linking reaction caused by the release of sulfur elements, instead of participating in the vulcanization reaction in the manner of releasing sulfur elements in conventional silane coupling agents, thereby avoiding the need to control the temperature during mixing not to be too high, and preventing the sulfur elements in conventional silane coupling agents from being released prematurely during mixing, causing the rubber compound to undergo a cross-linking reaction prematurely. Traditional silane coupling agents need to maintain a low temperature and constant temperature mixing time during the mixing process to prevent high temperature mixing from causing premature release of sulfur in the silane coupling agent, which will lead to premature crosslinking and vulcanization reactions, thereby making the rubber material unusable. At the same time, the preparation method of the present invention has low requirements on the cooling performance of the processing equipment, whether it can automatically adjust the speed, and other performances, and even if a traditional internal mixer is used for mixing, a good mixing effect can be achieved.
[0040] In one embodiment of the present application, the speed of the first mixing is 42-48 rpm, and / or the time of the first mixing is 2-5 min, and / or the temperature of the first row of rubber is 160-165°C; and / or the speed of the second mixing is 40-45 rpm, and / or the time of the second mixing is 2-4 min, and / or the temperature of the second row of rubber is 155-160°C; and / or the speed of the final mixing is 28-32 rpm, and / or the time of the final mixing is 1.5-3 min, and / or the temperature of the third row of rubber is 100-110°C.
[0041] It is preferred to control the rotation speed, time and temperature of the first batch of mixing within the above range, which is helpful to improve the dispersibility of carbon black, white carbon black, zinc oxide, stearic acid, antioxidant, 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde in natural rubber and styrene-butadiene rubber, thereby helping to improve the dispersibility and plasticity of the first batch of masterbatch; it is preferred to control the rotation speed, time and temperature of the second batch of mixing within the above range, which is helpful to further strengthen the interaction between 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde and white carbon black, thereby improving the heat generation performance of the vulcanized rubber; it is preferred to control the rotation speed, time and temperature of the third batch of mixing within the above range, which is helpful to promote the full and uniform dispersion of sulfur, accelerator and scorch retarder, and at the same time try to avoid the premature cross-linking reaction of sulfur, thereby helping to improve the strength and wear resistance of the vulcanized rubber.
[0042] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.
[0043] In Examples 1 to 5 and Comparative Example 1 of the present invention, the composition of the rubber composition in parts by weight is shown in Table 1. The rubber compound is prepared by the following preparation method using the rubber composition as a raw material:
[0044] Natural rubber, styrene-butadiene rubber, carbon black, white carbon black, zinc oxide, stearic acid, antioxidant, 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde were added into a GE320 internal mixer for mixing in one stage. The speed of mixing in one stage was 48rpm and the mixing time was 2min. The top bolt was pressed and mixed for 40s. The top bolt was raised and put into place. The top bolt was pressed and the speed was adjusted to 42rpm. Mixing was carried out for 40s. The top bolt was raised and mixed for 40s. Then the unloading door was opened to discharge the first batch of rubber. The temperature of the first batch of rubber was controlled at 160-165℃. The mill was opened to unload the rubber and the rubber was cooled and collected to obtain a masterbatch.
[0045] Add the first-stage masterbatch into a GE320 internal mixer for second-stage mixing. The speed of the second-stage mixing is 45 rpm and the time of the second-stage mixing is 2 min. Press the top bolt and mix for 40 seconds. Lift the top bolt to its place. Press the top bolt and mix for 40 seconds. Lift the top bolt and press the top bolt and mix for 40 seconds. Open the discharge door and discharge the second batch of rubber. The temperature of the second batch of rubber is controlled at 155-160°C. Open the mixer to unload the rubber and cool it to collect the rubber to obtain the second-stage masterbatch.
[0046] The second-stage masterbatch, sulfur, accelerator and anti-scorch agent are added to the GK255 internal mixer for final mixing. The speed of final mixing is 32rpm and the time of final mixing is 1.5min. The top bolt is pressed and mixed for 30s. The top bolt is raised and the top bolt is pressed and mixed for 30s. The top bolt is raised and the top bolt is pressed and mixed for 30s. The unloading door is opened and the third rubber is discharged. The temperature of the third rubber discharge is controlled at 100-110℃. The sheet is unloaded from the mixer and the rubber is cooled and collected to obtain a mixed rubber.
[0047] Table 1
[0048]
[0049]
[0050] Example 6
[0051] The difference from Example 3 is that natural rubber, styrene-butadiene rubber, carbon black, white carbon black, zinc oxide, stearic acid, antioxidant, and 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde are added to a GE320 internal mixer for mixing in one stage, the rotation speed of the mixing in one stage is 42 rpm, and the mixing time in one stage is 5 min; the top bolt is pressed and mixed for 80 s, the top bolt is raised and put into place, the top bolt is pressed and mixed for 80 s, the top bolt is raised, the top bolt is pressed and mixed for 80 s, the top bolt is raised, the top bolt is pressed and mixed for 60 s, and then the unloading door is opened to carry out the first discharge of rubber, and the temperature of the first discharge of rubber is controlled at 160-165°C; the mill is opened to unload the sheet, the rubber is cooled and collected, and a masterbatch is obtained.
[0052] The first stage masterbatch was added into the GE320 internal mixer for second stage mixing, the second stage mixing speed was 40 rpm, the second stage mixing time was 4 min; the top bolt was pressed, mixing was performed for 80 s, the top bolt was raised to the position, the top bolt was pressed and mixed for 80 s, the top bolt was raised, the top bolt was pressed and mixed for 80 s, the discharge door was opened, and the second discharge of rubber was carried out, and the temperature of the second discharge of rubber was controlled at 155-160°C; the mill was opened to unload the sheet, and the rubber was cooled and collected to obtain the second stage masterbatch.
[0053] The second-stage masterbatch, sulfur, accelerator and anti-scorch agent are added to a GK255 internal mixer for final mixing. The speed of the final mixing is 28 rpm and the time of the final mixing is 3 min. The top bolt is pressed and mixed for 60 s. The top bolt is raised and the top bolt is pressed and mixed for 60 s. The top bolt is raised and the top bolt is pressed and mixed for 60 s. The unloading door is opened and the third rubber is discharged. The temperature of the third rubber discharge is controlled at 100-110°C. The sheet is unloaded from the mixer and the rubber is cooled and collected to obtain a mixed rubber.
[0054] Example 7
[0055] The difference from Example 3 is that the antioxidant is a combination of antioxidant wax, antioxidant RD and antioxidant 4020, the mass ratio of antioxidant wax, antioxidant RD and antioxidant 4020 is 0.8:1.2:2.5, and finally a mixed rubber is obtained.
[0056] Example 8
[0057] The difference from Example 3 is that the antioxidant is a combination of antioxidant wax, antioxidant RD and antioxidant 4020, the mass ratio of antioxidant wax, antioxidant RD and antioxidant 4020 is 1.5:1.8:1.2, and finally a mixed rubber is obtained.
[0058] Example 9
[0059] The difference from Example 3 is that the antioxidant is a combination of antioxidant wax, antioxidant RD and antioxidant 4020, the mass ratio of antioxidant wax, antioxidant RD and antioxidant 4020 is 1.5:2.5:0.5, and finally a mixed rubber is obtained.
[0060] Example 10
[0061] The difference from Example 3 is that the accelerator is a combination of NS accelerator and diphenylguanidine accelerator, the mass ratio of NS accelerator to diphenylguanidine accelerator is 0.5:1.3, and finally a rubber compound is obtained.
[0062] Embodiment 11
[0063] The difference from Example 3 is that the accelerator is a combination of NS accelerator and diphenylguanidine accelerator, the mass ratio of the NS accelerator to the diphenylguanidine accelerator is 1.3:0.5, and a rubber compound is finally obtained.
[0064] Example 12
[0065] The difference from Example 3 is that the accelerator is a combination of NS accelerator and diphenylguanidine accelerator, the mass ratio of the NS accelerator to the diphenylguanidine accelerator is 1.7:0.1, and a rubber compound is finally obtained.
[0066] Embodiment 13
[0067] The difference from Example 3 is that the rotation speed of the first stage mixing is 42 rpm, the time of the first stage mixing is 5 min, the temperature of the first stage rubber discharge is 160-165° C., and finally a mixed rubber is obtained.
[0068] Embodiment 14
[0069] The difference from Example 3 is that the rotation speed of the first stage mixing is 35 rpm, the time of the first stage mixing is 6 min, the temperature of the first stage rubber discharge is 148° C., and finally a mixed rubber is obtained.
[0070] Embodiment 15
[0071] The difference from Example 3 is that the rotation speed of the second stage mixing is 45 rpm, the time of the second stage mixing is 2 min, the temperature of the second stage rubber discharge is 155-160° C., and finally a mixed rubber is obtained.
[0072] Example 16
[0073] The difference from Example 3 is that the rotation speed of the second stage mixing is 35 rpm, the time of the second stage mixing is 5 min, the temperature of the second stage rubber discharge is 150° C., and finally a mixed rubber is obtained.
[0074] Embodiment 17
[0075] The difference from Example 3 is that the final refining speed is 28 rpm, the final refining time is 3 min, the temperature of the third row of rubber is 100-110° C., and finally a mixed rubber is obtained.
[0076] Embodiment 18
[0077] The difference from Example 1 is that the final refining speed is 25 rpm, the final refining time is 3 min, the temperature of the third row of rubber is 120° C., and finally a mixed rubber is obtained.
[0078] Comparative Example 1
[0079] The difference from Example 3 is that natural rubber, styrene-butadiene rubber, carbon black, white carbon black, zinc oxide, stearic acid, antioxidant, 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde are added to the GE320 internal mixer for a mixing period, the mixing speed is 48rpm, and the mixing time for one period is 265s; the top bolt is pressed and mixed for 40s, the top bolt is raised and put in place, the silane coupling agent Si69 is added, the top bolt is pressed and mixed for 45s, the top bolt is raised, the top bolt is pressed, and the speed is adjusted to a variable speed automatic control range of 35 ~48rpm, mix at a constant temperature for 60s, raise the top bolt, keep the speed at a variable speed of 35~48rpm, press the top bolt to mix at a constant temperature for 60s, raise the top bolt, keep the speed at a variable speed of 35~48rpm, press the top bolt to mix at a constant temperature for 60s, control the temperature of the rubber compound at 145±3℃ during the whole process, reduce the speed when the temperature is high, and increase the speed when the temperature is low. After 180s of silanization reaction, open the unloading door and carry out the first discharge of rubber. The temperature of the first discharge of rubber is controlled below 150℃; unload the sheet from the mixing mill, cool and collect the rubber to obtain a masterbatch.
[0080] Add the first-stage masterbatch into a GE320 internal mixer for second-stage mixing. The speed of the second-stage mixing is 45 rpm and the time of the second-stage mixing is 2 min. Press the top bolt and mix for 40 seconds. Raise the top bolt to its place. Press the top bolt and mix for 40 seconds. Raise the top bolt and press the top bolt and mix for 40 seconds. Open the discharge door and discharge the second batch of rubber. The temperature of the second batch of rubber is controlled at 145-150°C. Open the mixer to unload the rubber and cool it to collect the rubber to obtain the second-stage masterbatch.
[0081] The second-stage masterbatch, sulfur, accelerator and anti-scorch agent are added to the GK255 internal mixer for final mixing. The speed of final mixing is 32rpm and the time of final mixing is 1.5min. The top bolt is pressed and mixed for 30s. The top bolt is raised and the top bolt is pressed and mixed for 30s. The top bolt is raised and the top bolt is pressed and mixed for 30s. The unloading door is opened and the third rubber is discharged. The temperature of the third rubber discharge is controlled at 100-110℃. The sheet is unloaded from the mixer and the rubber is cooled and collected to obtain a mixed rubber.
[0082] Test Method
[0083] The performance of the mixed rubbers of the above embodiments and comparative examples was tested, and the test results are shown in Table 2 and Table 3.
[0084] Mooney viscosity index test method: Test according to "GB / T 1232.1-2016 Unvulcanized rubber - Determination by disc shear viscometer - Part 1: Determination of Mooney viscosity".
[0085] RPA analysis-Panye effect test conditions: frequency is 10 Hz, temperature is 60°C, and strain is 0.07% to 200%.
[0086] MDR test method: GB / T 16584 "Standard for determination of vulcanization of rubber by rotorless vulcanizer" was used for MDR test, where the temperature was 150°C and the test time was 60 minutes.
[0087] Tensile performance test: The tensile performance test was carried out according to GB / T 528-2009 "Test method for tensile properties of rubber and rubber products", where the vulcanization conditions were 150°C and 30 minutes.
[0088] Thermal oxidative aging performance test: aging conditions are 100℃, 48h, and vulcanization conditions are 150℃, 30min. Among them, M300 / M100=300% elongation / 100% elongation, tensile product retention rate=after aging (tensile strength*elongation at break) / before aging (tensile strength*elongation at break)*100%.
[0089] Filler dispersion state test method: Test according to GB / T 6030-2006 "Rapid comparison method for evaluation of carbon black and carbon black silica dispersion in rubber".
[0090] DMA test method: GABO dynamic thermomechanical analyzer was used for DMA test (dynamic thermomechanical analysis test). The test conditions were tensile mode, dynamic strain of 0.25%, static strain of 7%, frequency of 10 Hz, test temperature range of 30-80 °C, heating rate of 2 °C / min, and the test results were expressed as tanδ@60 °C.
[0091] Table 2
[0092]
[0093]
[0094] Table 3
[0095]
[0096]
[0097] Among them, the amount of 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde in Example 2 is the same as that of the silane coupling agent Si69 in Comparative Example 1. When the amounts of other components and the process are basically the same, the tanδ@60°C value of Comparative Example 1 is significantly greater than that of Example 2. Therefore, compared with Comparative Example 1, the heat generation of the mixed rubber in Example 2 is lower.
[0098] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0099] The rubber composition of the present application is mainly prepared by adding a multifunctional additive, namely 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde, which has two alkoxy groups at both ends of its molecular chain, which can react with the hydroxyl groups on the surface of silica respectively, thereby reducing the surface polarity of silica, and then improving the dispersion of silica, that is, reducing the heat generation of the rubber composition. At the same time, the 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde molecular chain contains conjugated olefins and methyl substituents, that is, it contains active α-H and carbon-carbon double bonds. During vulcanization, its α carbon atom can directly participate in the cross-linking reaction process between rubber and sulfur, so there is no need for special constant temperature mixing control of the mixing process, thereby greatly improving the processability of the rubber composition; adding antioxidants can delay rubber aging, thereby extending the service life of the vulcanized rubber; adding stearic acid, zinc oxide, accelerators, and sulfur can promote the cross-linking reaction process between them and the rubber molecular chain, thereby forming a three-dimensional network structure and accelerating vulcanization, thereby improving the hardness, wear resistance and tear resistance of the vulcanized rubber; adding anti-scorching agents can control the vulcanization rate and prevent the rubber composition from scorching prematurely, thereby improving the quality of the vulcanized rubber. In addition, the rubber composition of the present invention not only has low heat generation, but is also easy to process, i.e., there is no need to maintain a constant temperature mixing time during mixing. At the same time, the rubber composition of the present invention has low requirements on the cooling performance of the processing equipment, whether the rotation speed can be automatically adjusted, and other performances, and even if a traditional internal mixer is used for mixing, a good mixing effect can be achieved.
[0100] The above are only embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A rubber composition, It is characterized in that In parts by weight, the rubber composition comprises: 50-90 parts of natural rubber; 10-50 parts of styrene-butadiene rubber; 5 to 30 parts of carbon black; 15-60 parts of white carbon black; 1.8 to 10.5 parts of 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde; 2.3 to 9 parts of antioxidant; 1-2.5 parts of stearic acid; 1.5 to 5 parts of zinc oxide; 1 to 4 parts of accelerator; 1-3 parts of sulfur; and 0.1 to 0.2 parts of anti-scorch agent.
2. The rubber composition according to claim 1, It is characterized in that In parts by weight, the rubber composition comprises: 55 to 90 parts of the natural rubber; 15 to 45 parts of the styrene-butadiene rubber; 8 to 25 parts of the carbon black; 15 to 55 parts of the white carbon black; 3.5 to 7.0 parts of the 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde; 2.6 to 6 parts of the antioxidant; 1.5 to 2 parts of stearic acid; 2 to 5 parts of the zinc oxide; 1.1 to 3.6 parts of the accelerator; 1 to 2.5 parts of said sulfur; and 0.1 to 0.2 parts of the anti-scorching agent.
3. The rubber composition according to claim 1 or 2, It is characterized in that The styrene butadiene rubber is solution polymerized styrene butadiene SOL5251H; and / or the brand of the carbon black is selected from any one or more of N115, N121, N134, N110, N234 and N220; and / or the brand of the white carbon black is selected from any one or more of Z1165MP, Z200MP, Z1115MP and VN3; and / or the anti-scorch agent is anti-scorch agent CTP.
4. The rubber composition according to any one of claims 1 to 3, It is characterized in that The antioxidant is selected from any one or more of antioxidant wax, antioxidant RD and antioxidant 4020.
5. The rubber composition according to claim 4, It is characterized in that The antioxidant is a combination of antioxidant wax, antioxidant RD and antioxidant 4020, and the mass ratio of the antioxidant wax, the antioxidant RD and the antioxidant 4020 is 0.8-1.5:0.5-2.5:1-2.5, preferably 0.8-1.5:0.6-2.0:1.2-2.
5.
6. The rubber composition according to any one of claims 1 to 5, It is characterized in that The accelerator is a NS accelerator and / or a diphenylguanidine accelerator.
7. The rubber composition according to claim 6, It is characterized in that The accelerator is a combination of an NS accelerator and a diphenylguanidine accelerator, and the mass ratio of the NS accelerator to the diphenylguanidine accelerator is 0.5-2:0.5-2, preferably 0.5-1.8:0.6-1.
8.
8. A rubber compound obtained by mixing a rubber composition. It is characterized in that The rubber composition is the rubber composition according to any one of claims 1 to 7.
9. A method for preparing the rubber compound according to claim 8, It is characterized in that The preparation method comprises: Step S1, mixing and discharging natural rubber, styrene-butadiene rubber, carbon black, white carbon black, zinc oxide, stearic acid, antioxidant, and 1,1,8,8-tetraethoxy-2,7-dimethyl-2T,4T,6T-triethylacetaldehyde in sequence to obtain a masterbatch; Step S2, sequentially performing two-stage mixing and a second batch mixing on the first-stage masterbatch to obtain a two-stage masterbatch; and Step S3, the second-stage masterbatch, sulfur, accelerator and scorch retarder are subjected to final refining and third refining in sequence to obtain the mixed rubber.
10. The preparation method according to claim 9, It is characterized in that The rotation speed of the first mixing stage is 42-48 rpm, and / or the time of the first mixing stage is 2-5 min, and / or the temperature of the first row of rubber is 160-165° C.; and / or, the rotation speed of the second stage mixing is 40-45 rpm, and / or the time of the second stage mixing is 2-4 min, and / or the temperature of the second row of rubber is 155-160° C.; And / or, the rotation speed of the final refining is 28-32 rpm, and / or the time of the final refining is 1.5-3 min, and / or the temperature of the third rubber discharge is 100-110°C.