Preparation method of composite nanofiltration membrane based on UiO-66 nanoparticles with different defect degrees

By introducing UiO-66 nanoparticles with different degrees of defects into the nanofiltration membrane, the surface morphology of the polyamide separation layer is controlled, which solves the problem of difficult control of the permeability selectivity of the nanofiltration membrane and achieves high permeability and desalination effects. promote.

CN118767703AActive Publication Date: 2024-10-15TIANJIN POLYTECHNIC UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310344208.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-03
Publication Date
2024-10-15
Estimated Expiration
2043-04-03

AI Technical Summary

Technical Problem

The inherent permeation selectivity of existing nanofiltration membranes is difficult to control. The diffusion rate of reaction monomers and rapid polymerization at the water-organic interface result in uncontrollable membrane surface morphology, which limits the improvement of nanofiltration membrane performance.

Method used

By introducing UiO-66 nanoparticles with different defective degrees as additives, they are dispersed in the piperazine aqueous solution for interfacial polymerization, and the surface morphology of the polyamide separation layer is controlled to improve the permeability of the nanofiltration membrane.

Benefits of technology

A composite nanofiltration membrane with ridged nanostructure was prepared, which significantly improved the pure water flux and Na2SO4 rejection rate, and improved the membrane's permeability and desalination capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767703A_ABST
    Figure CN118767703A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a composite nanofiltration membrane based on UiO-66 nano-particles with different defect degrees, and the preparation method comprises the following steps: 1) mixing terephthalic acid, zirconium chloride, glacial acetic acid, trifluoroacetic acid and N, N-dimethylformamide for reaction to obtain UiO-66 (UiO-66-X) nano-particles with different defect degrees; and 2) dispersing the UiO-66-X nano-particles in an aqueous solution of piperazine, and carrying out interfacial polymerization reaction on the UiO-66-X nano-particles and 1, 3, 5-benzoyl chloride dissolved in normal hexane to prepare the composite nanofiltration membrane with a surface ridge-shaped structure, so that the composite nanofiltration membrane has relatively high permeation flux while a relatively high retention rate of Na2SO4 is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of high-performance nanofiltration membrane materials, and in particular, relates to a method for preparing a composite nanofiltration membrane based on UiO-66 nanoparticles with different defective degrees. Background Art

[0002] Nanofiltration (NF) technology plays a huge role in the fields of seawater desalination, sewage treatment and recycling. Nanofiltration membranes can effectively remove multivalent ions and some small molecular organic matter, and often have better permeation flux than reverse osmosis (RO) membranes. Thin film composite (TFC) membranes prepared based on interfacial polymerization (IP) method are dominant in commercial desalination membranes. However, its inherent permeability selectivity (Trade off) is still the main bottleneck restricting the performance improvement of nanofiltration membranes. The difficult-to-control diffusion rate of reaction monomers and their rapid polymerization reaction at the immiscible water-organic interface are one of the core difficulties faced in improving the performance of nanofiltration membranes.

[0003] The uncontrollability of interfacial polymerization significantly affects the structure of the polyamide separation layer, such as the thickness of the separation layer, pore size, surface morphology, etc. Among them, the membrane surface morphology has been proven to significantly affect the separation performance of the nanofiltration membrane. Generally speaking, a rougher or more wrinkled membrane surface can provide a larger effective permeation area and thus improve the permeability. Previous research results have shown that increasing the permeation area of ​​the nanofiltration membrane surface can increase the flux of the nanofiltration membrane. For example, by adding polyvinyl alcohol (PVA) to the aqueous phase, the diffusion instability of the reaction monomers during the interfacial polymerization process can be increased, thereby preparing a composite nanofiltration membrane with a "Turing" structure with a higher surface roughness. Because the polyamide separation layer on its surface presents a regular bubble or tubular structure, the transmission path of water molecules is optimized, and the increase in the roughness of the membrane surface increases the permeation area, thereby improving the water permeability and water-salt selectivity of the nanofiltration membrane. On the other hand, by increasing the hydrophilicity of the membrane surface and thus enhancing the affinity of water molecules to the membrane surface, the mass transfer resistance can be reduced and the permeability of the membrane can be improved.

[0004] Metal-organic frameworks (MOFs) are an emerging class of porous crystalline materials with high porosity, large surface area, and uniform pore size, making them of great significance in membrane separation technology. In particular, water-stable MOFs with sub-angstrom pore windows have recently been shown to be promising in water treatment. As a typical MOF material, the structural unit of UiO-66 consists of a [Zr6O4(OH)4] metal cluster coordinated with 12 terephthalic acids, which has the highest coordination number among MOF materials. This high-density structural unit ensures a tight woven connection in the framework. UiO-66 can maintain structural stability in solvents such as water, dimethylformamide, benzene, or acetone, and has strong acid resistance and certain alkali resistance. MOF particles with defect properties have been shown to be highly efficient molecular and ion adsorbents due to the specific interactions between molecules / ions with specific functional groups and MOF active sites. Therefore, in the present invention, glacial acetic acid is introduced to limit particle size growth in an in-situ controlled manner, and trifluoroacetic acid, a capping agent, is added to compete with terephthalic acid to prepare UiO-66 nanoparticles with different defects. UiO-66 with different defect levels is dispersed in the aqueous phase to react with piperazine monomer to affect the interfacial polymerization process to complete the regulation of the ridge morphology on the membrane surface, thereby achieving the effect of improving the membrane permeability. Summary of the invention

[0005] The present invention solves the problem of high permeability of nanofiltration membranes in the prior art and proposes a method for preparing a composite nanofiltration membrane based on UiO-66 nanoparticles with different defective degrees. In the present invention, UiO-66 with different defective degrees is used as a nano additive, dispersed in an aqueous solution of piperazine and subjected to interfacial polymerization reaction, to prepare a composite nanofiltration membrane with different polyamide separation layer structures. A general strategy for designing a nanofiltration membrane with an adjustable surface nanostructure to enhance desalination performance by defect modification of MOF particles is proposed. UiO-66 (UiO-66-X) with different defective degrees is used as an aqueous phase additive and dispersed in the aqueous phase, and the surface morphology structure of the nanofiltration membrane is evolved from ridge-like to granular by affecting the diffusion process of the interfacial polymerization reaction. It is particularly pointed out that compared with the polyamide separation layer with a granular surface morphology, the surface permeability area of ​​the polyamide separation layer with a ridge-like nanostructure is significantly increased, so the permeability performance of the nanofiltration membrane can be greatly improved.

[0006] The present invention is achieved by a method for preparing a composite nanofiltration membrane based on UiO-66 nanoparticles with different defective degrees, comprising the following steps:

[0007] (1) UiO-66 (UiO-66-X) nanoparticles with different defective degrees were obtained by mixing zirconium chloride as a metal source, terephthalic acid as an organic ligand, N,N-dimethylformamide as a solvent, glacial acetic acid as a particle size regulator, and trifluoroacetic acid as a capping agent.

[0008] (2) Dispersing UiO-66-X nanoparticles in a piperazine / aqueous phase solution to obtain a UiO-66 / piperazine suspension.

[0009] (3) Interfacial polymerization of the suspension obtained in step (2) and 1,3,5-benzenetricarboxylic acid chloride / n-hexane solution is carried out on the surface of a polysulfone support membrane.

[0010] (4) After the surface of the composite membrane prepared in step (3) is rinsed with n-hexane, it is placed in an oven at a certain temperature for cross-linking and curing treatment to obtain the composite nanofiltration membrane based on UiO-66 nanoparticles with different defective degrees.

[0011] In the present invention, in order to prepare a polyamide separation layer nanostructure with different surface morphologies to improve the permeability of the nanofiltration membrane, UiO-66 nanoparticles with different defect levels are dispersed in a piperazine / water phase solvent and subjected to interfacial polymerization reaction with 1,3,5-benzenetricarboxylic acid chloride dissolved in an oil phase solvent to achieve the preparation of a composite nanofiltration membrane. The advantages of the present invention are: (1) UiO-66 nanoparticles with different defect levels are used as additives for the preparation of composite nanofiltration membranes, and nanocomposite membranes with different surface morphologies are prepared while ensuring that their size does not change significantly; (2) When UiO-66-X is used as an aqueous phase additive, due to the increase in membrane surface roughness and hydrophilicity, the representative nanofiltration membrane with ridge-like nanostructure has a higher pure water flux and Na2SO4 retention rate.

[0012] Furthermore, in the step (1), the volume ratio of dimethylformamide, glacial acetic acid and trifluoroacetic acid is 40:1:0-1, the concentration of terephthalic acid is 0.048 mol / L, and the concentration of zirconium chloride is 0.026 mol / L. The above raw materials are fully stirred and mixed and placed in a polytetrafluoroethylene reactor for high-temperature synthesis. The preferred reaction temperature is 120-200°C and the reaction time is 12-24h.

[0013] Furthermore, the end-capping agent trifluoroacetic acid can be replaced by one of difluoroacetic acid, formic acid, trimesic acid or benzoic acid.

[0014] Furthermore, in the step (2), UiO-66-X nanoparticles are dispersed in the aqueous solution by ultrasound at a concentration of 0.01 to 0.3 w / v.%, piperazine, an aqueous monomer required for the interfacial polymerization reaction, has a concentration of 0.1 to 3 w / v.%, and the solvent is deionized water.

[0015] Furthermore, in the step (3), the residence time of the piperazine / water solution on the polysulfone support layer is 3 to 20 minutes; the concentration of the oil phase monomer 1,3,5-benzenetricarboxylic acid chloride is 0.05 to 0.5 w / v.%, the solvent is n-hexane; and the interfacial polymerization time is 1 minute.

[0016] Furthermore, in the step (4), the oven curing and cross-linking temperature is 50 to 100° C., and the curing time is 5 to 30 minutes.

[0017] The surface of the prepared composite nanofiltration membrane polyamide layer presents two different nanostructures: "ridge-like" and "granular". Under a pressure of 0.4 MPa, the pure water flux reaches 27.5 L·m -2 ·h -1 The retention rate of Na2SO4 is maintained above 97.8%.

[0018] The advantages and positive effects of the present invention are:

[0019] 1. UiO-66 nanoparticles with different defective degrees are used to prepare nanofiltration membranes. Under the premise of ensuring that the crystal size does not change too much, nanocomposite membranes with different surface morphologies can be prepared using UiO-66-X nanoparticles as additives.

[0020] 2. When UiO-66-X is used as an aqueous phase additive, the representative nanofiltration membrane with ridged nanostructure has higher pure water flux and Na2SO4 retention rate due to the increase in membrane surface roughness and hydrophilicity. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions of the specific embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the specific embodiments. Obviously, the drawings described below are some specific embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0022] Figure 1 is a scanning electron microscope image of the nanofiltration membrane prepared according to Comparative Example 5 of the present invention;

[0023] Figure 2 3 is a scanning electron microscope image of the nanofiltration membrane prepared according to Example 1 of the present invention. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] This embodiment provides a method for preparing a composite nanofiltration membrane based on UiO-66 nanoparticles with different defective degrees, characterized in that it comprises the following steps:

[0026] (1) UiO-66 (UiO-66-X) nanoparticles with different defective degrees were obtained by mixing zirconium chloride as a metal source, terephthalic acid as an organic ligand, N,N-dimethylformamide as a solvent, glacial acetic acid as a particle size regulator, and trifluoroacetic acid as a capping agent.

[0027] (2) Dispersing UiO-66-X nanoparticles in a piperazine / aqueous phase solution to obtain a UiO-66 / piperazine suspension.

[0028] (3) Interfacial polymerization of the suspension obtained in step (2) and 1,3,5-benzenetricarboxylic acid chloride / n-hexane solution is carried out on the surface of a polysulfone support membrane.

[0029] (4) After the surface of the composite membrane prepared in step (3) is rinsed with n-hexane, it is placed in an oven at a certain temperature for cross-linking and curing treatment to obtain the composite nanofiltration membrane based on UiO-66 nanoparticles with different defective degrees.

[0030] In the step (1), the end-capping agent trifluoroacetic acid can be replaced by one of difluoroacetic acid, formic acid, trimesic acid or benzoic acid, preferably trifluoroacetic acid; the volume ratio of terephthalic acid, zirconium chloride, glacial acetic acid and trifluoroacetic acid is 40:1:0-1, preferably 40:1:0-0.5; the concentration of terephthalic acid is 0.048 mol / L, and the concentration of zirconium chloride is 0.026 mol / L. After the above raw materials are fully stirred and mixed, they are placed in a polytetrafluoroethylene reactor for high-temperature synthesis, the reaction temperature is 120-200°C, preferably 150°C; the reaction time is 12-24h, preferably 12h.

[0031] In the step (2), UiO-66-X nanoparticles are dispersed in the aqueous solution by ultrasound, with a concentration of 0.01-0.3 w / v.%, preferably 0.1 w / v.%; the concentration of the aqueous monomer piperazine required for the interfacial polymerization reaction is 0.1-3 w / v.%, preferably 1 w / v.%; and the solvent is deionized water.

[0032] In the step (3), the residence time of the piperazine / water solution on the polysulfone support layer is 1 to 20 minutes, preferably 3 minutes; the oil phase monomer is 1,3,5-benzenetricarboxylic acid chloride with a concentration of 0.05 to 0.5 w / v.%, preferably 0.15 w / v.%; the solvent is n-hexane; and the interfacial polymerization time is 10 to 120 seconds, preferably 60 seconds.

[0033] In the step (4), the oven curing and cross-linking temperature is 50-100° C., preferably 65° C.; the curing time is 5-30 minutes, preferably 10 minutes.

[0034] The surface of the prepared composite nanofiltration membrane polyamide layer presents two different nanostructures: "ridge-like" and "granular". Under a pressure of 0.4 MPa, the pure water flux reaches 27.5 L·m -2 ·h -1 The retention rate of Na2SO4 is maintained above 97.8%.

[0035] In order to better understand the above-mentioned embodiments of the present invention, they are further described below with reference to specific examples.

[0036] In the following embodiments and comparative examples:

[0037] Terephthalic acid, analytical grade, was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0038] Zirconium chloride, analytical grade, was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0039] Anhydrous piperazine, analytical grade, was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0040] 1,3,5-Benzenetricarboxylic acid chloride, analytical grade, purchased from Beijing Bailingwei Technology Co., Ltd.;

[0041] n-Hexane, analytical grade, was purchased from Tianjin Kemeiou Chemical Reagent Co., Ltd.;

[0042] Dimethylformamide, analytical grade, was purchased from Tianjin Kemeiou Chemical Reagent Co., Ltd.;

[0043] Glacial acetic acid, analytical grade, was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0044] Trifluoroacetic acid, analytical grade, was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.

[0045] Example 1

[0046] (1) 0.16 g zirconium chloride and 0.12 g terephthalic acid were added to 40 mL dimethylformamide and stirred with a magnetic stirrer until a clear solution was obtained. Then a certain amount of 1 mL glacial acetic acid solution was added and stirred thoroughly to mix. All the solutions were transferred to a polytetrafluoroethylene autoclave and heated at 150 °C for 12 h. After cooling naturally to room temperature, the white precipitate was collected by centrifugation and washed three times with dimethylformamide and glacial acetic acid to remove unreacted terephthalic acid and dimethylformamide molecules trapped in the framework pores. It was dried at 100 °C for 10 hours for use.

[0047] (2) Piperazine was added to water at a concentration of 1 w / v.% as the aqueous phase, and 1,3,5-benzenetricarboxylic acid chloride was added to n-hexane to prepare a solution with a concentration of 0.15 w / v.% as the organic phase. After rinsing the polysulfone support membrane with deionized water, the support membrane was fixed in a customized frame with an effective diameter of 7.5 cm. The prepared UiO-66-X nanoparticles were ultrasonically dispersed in the piperazine / aqueous phase solution at a ratio of 0.1 w / v.%, and the ultrasonic time was 1 min. The aqueous phase solution (10 mL) was poured into the frame, and the top surface (dense layer) of the base membrane was completely immersed for 3 min. The aqueous phase was poured out, and the excess aqueous phase solution on the membrane surface was removed using a rubber roller. Then 10 mL of the organic phase solution was poured in and left for 1 min, and the excess organic phase was discarded. Subsequently, the membrane was placed in an oven at 65°C for 10 min for drying and curing to prepare a composite nanofiltration membrane.

[0048] Example 2

[0049] (1) 0.16 g zirconium chloride and 0.12 g terephthalic acid were added to 40 mL dimethylformamide and stirred by a magnetic stirrer until a clear solution was obtained. Then a quantitative 1 mL glacial acetic acid solution was added and stirred thoroughly to mix. Finally, 0.25 mL trifluoroacetic acid was added to the clear solution, and after rapid stirring for 30 min, all the solution was transferred to a polytetrafluoroethylene autoclave and heated at 150 ° C for 12 h. After cooling naturally to room temperature, the white precipitate was collected by centrifugation and washed three times with dimethylformamide and glacial acetic acid to remove unreacted terephthalic acid and dimethylformamide molecules trapped in the framework pores. It was dried at 100 ° C for 10 hours for use.

[0050] (2) Piperazine was added to water at a concentration of 1 w / v.% as the aqueous phase, and 1,3,5-benzenetricarboxylic acid chloride was added to n-hexane to prepare a solution with a concentration of 0.15 w / v.% as the organic phase. After rinsing the polysulfone support membrane with deionized water, the support membrane was fixed in a customized frame with an effective diameter of 7.5 cm. The prepared UiO-66-X nanoparticles were ultrasonically dispersed in the piperazine / aqueous phase solution at a ratio of 0.1 w / v.%, and the ultrasonic time was 1 min. The aqueous phase solution (10 mL) was poured into the frame, and the top surface (dense layer) of the base membrane was completely immersed for 3 min. The aqueous phase was poured out, and the excess aqueous phase solution on the membrane surface was removed using a rubber roller. Then 10 mL of the organic phase solution was poured in and left for 1 min, and the excess organic phase was discarded. Subsequently, the membrane was placed in an oven at 65°C for 10 min for drying and curing to prepare a composite nanofiltration membrane.

[0051] Example 3

[0052] A composite nanofiltration membrane was prepared in the same manner as in Example 2, except that the amount of trifluoroacetic acid added in step (1) of Example 2 was changed to 0.5 mL.

[0053] Example 4

[0054] A composite nanofiltration membrane was prepared in the same manner as in Example 2, except that the amount of trifluoroacetic acid added in step (1) of Example 2 was changed to 1 mL.

[0055] Comparative Example 1

[0056] A composite nanofiltration membrane was prepared in the same manner as in Example 1, except that the UiO-66 prepared in step (2) of Example 1 was added to the 1,3,5-benzenetricarboxylic acid chloride / oil phase solution.

[0057] Comparative Example 2

[0058] A composite nanofiltration membrane was prepared in the same manner as in Example 2, except that the UiO-66 prepared in step (2) of Example 2 was added to the 1,3,5-benzenetricarboxylic acid chloride / oil phase solution.

[0059] Comparative Example 3

[0060] A composite nanofiltration membrane was prepared in the same manner as in Example 3, except that the UiO-66 prepared in step (2) of Example 3 was added to the 1,3,5-benzenetricarboxylic acid chloride / oil phase solution.

[0061] Comparative Example 4

[0062] A composite nanofiltration membrane was prepared in the same manner as in Example 4, except that the UiO-66 prepared in step (2) of Example 4 was added to the 1,3,5-benzenetricarboxylic acid chloride / oil phase solution.

[0063] Comparative Example 5

[0064] Piperazine was added to water at a concentration of 1 w / v.% as the aqueous phase, and 1,3,5-benzenetricarboxylic acid chloride was added to n-hexane to prepare a solution with a concentration of 0.15 w / v.% as the organic phase. After rinsing the polysulfone support membrane with deionized water, the support membrane was fixed in a customized frame with an effective diameter of 7.5 cm. The aqueous phase solution (10 mL) was poured into the frame, and the top surface (dense layer) of the base membrane was completely immersed for 3 minutes. The aqueous phase was poured out, and the excess aqueous phase solution on the membrane surface was removed using a rubber roller. Then 10 mL of the organic phase solution was poured in and left for 1 minute, and the excess organic phase was discarded. Subsequently, the membrane was placed in an oven at 65°C for 10 minutes for drying and curing to prepare a composite nanofiltration membrane.

[0065] Performance Testing

[0066] In the present invention, deionized water and Na2SO4 aqueous solution were used to test the membrane flux and salt retention performance of the composite nanofiltration membranes prepared in Examples 1-4 and Comparative Examples 1-5. Specifically, the membrane separation performance test was carried out at 0.4 MPa with a 1 g / L Na2SO4 solution, and the concentrations of the filtrate and feed solution were tested using a conductivity meter. The results are shown in Table 1 below.

[0067] Table 1 Separation performance and characterization results of composite nanofiltration membrane

[0068]

[0069] As can be seen from Table 1, the pure water flux and the retention rate of Na2SO4 through the membrane are used to evaluate the desalination performance of the nanofiltration membrane. The comparison between Examples 1-4 and Comparative Examples 1-4 shows that due to the difference in the addition of UiO-66-X nanoparticles in the aqueous phase and the oil phase solvent, the permeability of the Example 1-4 membrane prepared by adding UiO-66-X in the aqueous phase is much greater than that of the Comparative Example 1-4 membrane (Example 3: 27.5 L·m -2 ·h -1 ; Comparative Example 3: 19.7 L·m -2 ·h -1 The permeability of the membranes of Comparative Examples 1-4 was only slightly improved compared with the membranes of the comparative examples (17.8-22.3 L·m -2 ·h -1 ), while the performance of the membranes of Examples 1-4 was more significantly improved (22.2 to 27.5 L·m -2 ·h -1). Moreover, compared with the membranes of comparative examples 1-4, the polyamide layer with a ridge structure in the membranes of embodiments 1-4 has a rougher membrane surface (roughness of embodiment 3: 86.16nm), and therefore has a larger effective permeation area. The difference in the surface morphology of the polyamide layer is caused by the difference in the influence of UiO-66-X nanoparticles with different degrees of defects on the interfacial polymerization process. The membranes of all comparative examples and embodiments have good hydrophilicity. Compared with comparative example 5, the addition of UiO-66-X effectively reduces the contact angle of the membrane. The reduction in the water contact angle of the membranes of comparative examples 1-4 is due to the increase in the roughness of the membrane surface. The membranes of embodiments 1-4 also have a lower water contact angle because there are ligand defects in UiO-66-X, and the exposure of the metal center makes the particles have a better affinity with water. The enhancement of the wettability of the membrane surface also contributes to the improvement of the permeability performance of the membrane.

Claims

1. A method for preparing a composite nanofiltration membrane based on UiO-66 nanoparticles with different defective degrees, characterized in that: The steps include: (1) UiO-66 (UiO-66-X) nanoparticles with different defective degrees were obtained by mixing zirconium chloride as a metal source, terephthalic acid as an organic ligand, N,N-dimethylformamide as a solvent, glacial acetic acid as a particle size regulator, and trifluoroacetic acid as a capping agent. (2) Dispersing UiO-66-X nanoparticles in a piperazine / aqueous phase solution to obtain a UiO-66 / piperazine suspension. (3) Interfacial polymerization of the suspension obtained in step (2) and 1,3,5-benzenetricarboxylic acid chloride / n-hexane solution is carried out on the surface of a polysulfone support membrane. (4) After the surface of the composite membrane prepared in step (3) is rinsed with n-hexane, it is placed in an oven at a certain temperature for cross-linking and curing treatment to obtain the composite nanofiltration membrane based on UiO-66 nanoparticles with different defective degrees.

2. The method for preparing a composite nanofiltration membrane based on UiO-66 nanoparticles with different defective degrees according to claim 1, characterized in that: In the step (1), the volume ratio of dimethylformamide, glacial acetic acid and trifluoroacetic acid is 40:1:0-1, the concentration of terephthalic acid is 0.048 mol / L, the concentration of zirconium chloride is 0.026 mol / L, and the preparation is carried out by a hydrothermal reaction method.

3. The method for preparing a composite nanofiltration membrane based on UiO-66 nanoparticles with different defective degrees according to claim 1, characterized in that: In the step (2), UiO-66-X nanoparticles are dispersed in an aqueous solution by ultrasound at a concentration of 0.01 to 0.3 w / v.%; the concentration of the aqueous monomer piperazine required for the interfacial polymerization reaction is 1 w / v.%, and the solvent is deionized water.

4. The method for preparing a composite nanofiltration membrane based on UiO-66 nanoparticles with different defective degrees according to claim 1, characterized in that: In the step (3), the oil phase monomer is trimesoyl chloride, the concentration of which is 0.15 w / v.%, the solvent is n-hexane, and the interfacial polymerization time is 1 min.

5. The method for preparing a composite nanofiltration membrane based on UiO-66 nanoparticles with different defective degrees according to claim 1, characterized in that: In the step (4), the oven curing and cross-linking temperature is 50 to 100° C., and the curing time is 5 to 30 minutes. The surface of the prepared composite nanofiltration membrane polyamide layer presents two different nanostructures: "ridge-like" and "granular". Under a pressure of 0.4 MPa, the pure water flux reaches 27.5 L·m -2 ·h -1 The retention rate of Na2SO4 is maintained above 97.8%.

6. A composite nanofiltration membrane based on UiO-66 nanoparticles with different degrees of defectivity, characterized in that: A composite nanofiltration membrane based on UiO-66 nanoparticles with different defective degrees, prepared by the preparation method described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Preparation method of super-hydrophobic super-oleophylic lithium air battery composite diaphragm

    CN114191996A

  • Preparation method of UiO-66-based nanoparticle composite nanofiltration membrane and product thereof

    CN115382399A

  • Arresting gear

    KR1020230135425A