Alumina carrier with core-shell structure and preparation method thereof
By adopting a core-shell structure and a gradient distribution of flaky pseudo-boehmite in the alumina carrier, an "eggshell-albumin-yolk" structure is formed, which solves the problem of existing alumina carriers in the pore channels of heavy and residual oil hydrogenation treatment. The problems of structural unsuitability and decreased activity have been solved, and the effective treatment of heavy metal content and residual oil and the stability of catalyst activity have been achieved.
Patent Information
- Application Number
- CN202310356024.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-04-06
AI Technical Summary
The existing alumina carrier has the problem that the pore structure is not conducive to reactant diffusion and metal deposition in the hydrogenation treatment of heavy and residual oil, resulting in reduced catalyst activity. Moreover, the conventional pore expansion method is complicated and difficult to form a gradient pore structure.
Using an alumina carrier with a core-shell structure, the "eggshell-albumin-yolk" structure is formed through the gradient distribution of flaky pseudo-boehmite, which regulates the size and distribution of the pores, improves the adaptability of the pore structure of the carrier, and is suitable for high metal content Hydrotreating of heavy and residual oil.
It achieves the gradient distribution of macropore content and pore size, improves the diffusion capacity of reactants, enhances the activity stability and resistance to metal deposition of the catalyst, and is suitable for the hydrogenation of heavy metal content and residual oil.
Smart Images

Figure CN118767902A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of alumina material synthesis, and specifically relates to an alumina carrier with a core-shell structure and a preparation method thereof. Background Art
[0002] At present, with the increasing heaviness and inferiority of crude oil, oil refining enterprises are faced with a large number of heavy and residual oil processing and utilization problems. Heavy and residual oil molecules have complex three-dimensional structures, and sulfur-containing polycyclic aromatic hydrocarbon side chains often form steric hindrances, which prevent the sulfur atoms in the five- and six-membered rings from being adsorbed by the active centers of the catalyst. In the process of catalytic hydrogenation, heavy oil macromolecules are adsorbed and deposited on the surface or pores of the catalyst, which increases the diffusion resistance in the reaction and causes the apparent activity of the catalyst to decrease. At the same time, heavy and residual oils contain more coke precursors, which will generate coke and deposit in the pores under certain conditions, causing the active centers of the catalyst to be poisoned. Diffusion in the catalyst becomes a controlling factor in the catalytic hydrogenation process of heavy and residual oils. Therefore, the catalytic hydrogenation of heavy and residual oils requires macroporous catalysts with larger pore sizes and pore volumes to accommodate more carbon deposits, metal deposits, etc., and reduce the diffusion resistance encountered by macromolecular reactions. The large pore size and pore volume of the catalyst mainly rely on the corresponding large pore size and large pore volume carrier.
[0003] Alumina is a commonly used catalyst carrier in the petrochemical industry. It has always been the most widely used and largest-volume catalytic carrier due to its good mechanical stability, easy control of specific surface area and pore structure, and low price and availability. However, the pores of conventional alumina carriers are relatively small. In order to meet the needs of heavy residue hydroprocessing, the "pore expansion" method is usually used to improve the pore structure of the alumina carrier.
[0004] CN107913691A discloses an alumina carrier containing macropores and a preparation method thereof. The method firstly adds pseudo-boehmite powder and sesbania powder into a kneader and mixes them evenly, then prepares a styrene-butadiene rubber emulsion with a particle size of 10-500nm, and adds an organic acid or an inorganic acid thereto; then adds the acid solution containing the styrene-butadiene rubber emulsion into the pseudo-boehmite powder and sesbania powder and kneads them evenly, and then extrudes, forms, dries, and roasts to obtain an alumina carrier containing macropores. The preparation process of the styrene-butadiene rubber emulsion of the pore-enlarging agent in the method is relatively complicated, and in addition, no gradient pores are formed between the surface and the interior of the carrier, which is not conducive to the diffusion of the residual oil reactant molecules into the interior.
[0005] CN104646008A discloses a catalyst for demetallization of inferior heavy oil by hydrodesulfurization and a preparation method thereof. The catalyst uses alumina as a carrier, and group VIII and VIB elements, especially Ni-Mo, as active components. The catalyst has a pore volume of 0.61-0.70 mL / g and a specific surface area of 155-200 m 2 / g, and the average pore diameter is 13.0-18.0nm. The preparation method of the catalyst is to treat the carrier particles after forming and calcining with an acid solution with continuously increasing concentration. Although this method can make the average pore diameter of the final catalyst gradually increase along the radial direction of the catalyst particles from the center to the outer surface, this treatment method is difficult to form larger pores on the carrier surface. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention provides an alumina carrier with a core-shell structure and a preparation method thereof. The macropore content and pore size of the alumina carrier of the present invention present a gradient distribution of an "eggshell-egg white-egg yolk" structure, and the alumina carrier is suitable for the hydroprocessing process of heavy residue oil with high metal (Ni, V) content.
[0007] The core-shell structured alumina carrier of the present invention is a three-layer spherical structure of "eggshell-egg white-yolk", wherein the "eggshell" layer is a flaky alumina crystal aggregate, and the "egg white" and "egg yolk" layers are a mixed phase of a flaky alumina crystal aggregate and a granular alumina aggregate, wherein the mass ratio of the flaky alumina crystal aggregate to the granular alumina aggregate in the "egg white" layer is 0.1:1-0.3:1; the mass ratio of the flaky alumina crystal aggregate to the granular alumina aggregate in the "egg yolk" layer is 0.4:1-1.4:1; the thickness of the "eggshell" layer is 0.2r-0.5r, the thickness of the "egg white" layer is 0.3r-0.6r, and the thickness of the "egg yolk" layer is the remainder, wherein r is the radius of the alumina carrier, i.e., the straight-line distance from the center of the sphere to the outer surface.
[0008] In the alumina carrier with a core-shell structure of the present invention, the flaky alumina grains have a size of 100-800nm and a thickness of 25-80nm; the grain size of the granular alumina grains is 20-100nm.
[0009] The diameter of the alumina carrier with a core-shell structure of the present invention is 2 mm to 10 mm.
[0010] The specific surface area of the core-shell alumina carrier of the present invention is 160-300m 2 / g, the pore volume is 0.8-1.2mL / g, the pore content with a diameter of 10-20nm accounts for 40%-60% of the total pore volume, the pore content with a diameter of 50-100nm accounts for 10%-20% of the total pore volume, and the content of pores with a diameter greater than 100nm accounts for 8%-15% of the total pore volume.
[0011] The method for preparing the core-shell structured alumina carrier of the present invention comprises the following contents: (1) Calcinate aluminum nitrate. After calcination, the material is crushed and screened. The screened material is mixed with an aqueous solution of propylene oxide, and then hydrothermally treated. After treatment, the material is filtered, washed, and dried to obtain flaky pseudo-boehmite P1. (2) Mix pseudo-boehmite P2 with the flaky pseudo-boehmite P1 obtained in step (1) to obtain a mixed material H1, and through rolling ball forming, obtain a spherical precursor S1. (3) Mix pseudo-boehmite P2 with the flaky pseudo-boehmite P1 obtained in step (1) to obtain a mixed material H2, and then mix the spherical precursor S1 with the mixed material H2 and continue rolling ball forming to obtain a spherical precursor S2. (4) Mix the flaky pseudo-boehmite P1 with the spherical precursor S2, perform rolling ball forming, and then dry and calcine to obtain a core-shell structured alumina support.
[0012] In the method of the present invention, the pseudo-boehmite P1 prepared in step (1) has the following properties: 1.0 < P1 ≤ 1.3, 1.1 < P2 ≤ 1.5, P1 = D(120) / D(031), P2 = D(120) / D(020); the D(120) represents the grain size of the crystal plane corresponding to the (120) peak in the XRD pattern of the pseudo-boehmite crystal grains, and D(120) is 75 - 105 Å; D(031) represents the grain size of the crystal plane corresponding to the (031) peak in the XRD pattern of the pseudo-boehmite crystal grains, and D(031) is 70 - 90 Å; D(020) represents the grain size of the crystal plane corresponding to the (020) peak in the XRD pattern of the pseudo-boehmite crystal grains, and D(020) is 60 - 70 Å; the 120 peak refers to the characteristic peak with 2θ of 25.5 - 29.9º in the XRD pattern; the 031 peak refers to the characteristic peak with 2θ of 36.3 - 40.5º in the XRD pattern; the 020 peak refers to the characteristic peak with 2θ of 12.0 - 16.2º in the XRD pattern, D = Kλ / (Bcosθ), where K is the Scherrer constant, λ is the diffraction wavelength of the target material, B is the half-peak width of the diffraction peak, and θ is the diffraction angle.
[0013] In the method of the present invention, the calcination temperature in step (1) is 450 - 650°C, and the calcination time is 4 - 8 hours.
[0014] In the method of the present invention, the crushing particle size of the material in step (1) is greater than 100 mesh, preferably greater than 200 mesh.
[0015] In the method of the present invention, the mass percentage concentration of the aqueous solution of propylene oxide in step (1) is 2.5% - 12%, preferably 4% - 8%, and the mass ratio of the amount of the aqueous solution of propylene oxide used to the mass of the powder material is 3:1 - 10:1, preferably 4:1 - 8:1.
[0016] In the method of the present invention, the hydrothermal treatment in step (1) is carried out in a sealed container, which is preferably an autoclave. The hydrothermal treatment temperature is 110-180° C., preferably 120-160° C., and the treatment time is 4-8 hours. During the hydrothermal treatment, the pressure in the sealed container is autogenous pressure.
[0017] In the method of the present invention, the drying temperature in step (1) is 100-160° C., and the drying time is 2-8 hours.
[0018] In the method of the present invention, the pseudo-boehmite P2 particles described in step (2) are generally in granular form and may be a commercially available product or pseudo-boehmite prepared by methods such as acid precipitation, alkali precipitation, alcohol aluminum hydrolysis, etc., preferably pseudo-boehmite having a pore size greater than 10 nm.
[0019] In the method of the present invention, the mass ratio of the flaky pseudo-boehmite P1 to the pseudo-boehmite P2 in step (2) is 1:9-1:4.
[0020] In the method of the present invention, the ball forming in step (2) is carried out in a turntable forming machine, and the rotation operating conditions of the turntable forming machine are: the inclination angle of the turntable is 40-70°, the rotation speed of the turntable is 10-30rpm; the forming time of the material in the turntable is 10-120min. The radius of the spherical precursor S1 is 0.2r-0.5r, wherein r is the radius of the final spherical alumina material, that is, the straight-line distance from the center of the sphere to the outer surface. During the ball forming process, an aqueous solution containing a gelling agent is sprayed into the material; the aqueous solution containing a gelling agent is one or a mixture of nitric acid, phosphoric acid, oxalic acid, and acetic acid aqueous solutions, and the concentration of the solution is 1wt%-3wt%, preferably an acetic acid aqueous solution.
[0021] In the method of the present invention, the mass ratio of the flaky pseudo-boehmite P1 to the pseudo-boehmite P2 in step (3) is 3:2-3:7.
[0022] In the method of the present invention, the ball forming in step (3) is carried out in a turntable forming machine, and the rotation operating conditions of the turntable forming machine are: the inclination angle of the turntable is 40-70°, the rotation speed of the turntable is 10-30rpm; the forming time of the material in the turntable is 10-120min. The radius of the spherical precursor S2 is 0.5r-0.8r, wherein r is the radius of the final spherical alumina material, that is, the straight-line distance from the center of the sphere to the outer surface. During the ball forming process, an aqueous solution containing a gelling agent is sprayed into the material; the aqueous solution containing a gelling agent is one or a mixture of aqueous solutions of nitric acid, phosphoric acid, oxalic acid, and acetic acid, and the concentration of the solution is 1wt%-3wt%, preferably an acetic acid aqueous solution.
[0023] In the method of the present invention, the ball forming in step (4) is carried out in a turntable forming machine, and the rotating operating conditions of the turntable forming machine are: the inclination angle of the turntable is 40-70°, the rotation speed of the turntable is 10-30rpm; the forming time of the material in the turntable is 10-60min, and the final sphere diameter is adjusted as needed, generally 5-10mm. During the ball forming process, an aqueous solution containing a peptizing agent is sprayed into the material; the aqueous solution containing a peptizing agent is one or a mixture of aqueous solutions of nitric acid, phosphoric acid, oxalic acid, and acetic acid, and the mass concentration of the solution is 1%-3%, preferably an aqueous solution of acetic acid.
[0024] In the method of the present invention, the drying time in step (4) is 1-8 hours, preferably 2-6 hours, and the drying temperature is 60°C-180°C, preferably 80°C-150°C; the roasting temperature is 350-800°C, preferably 500-650°C, and the roasting time is 2-6 hours, preferably 2-4 hours.
[0025] The core-shell alumina carrier of the present invention is suitable for the hydroprocessing process of heavy oil and residual oil, and is particularly suitable for the hydroprocessing process of heavy oil and residual oil with high metal (Ni, V) content.
[0026] The present invention also provides a hydroprocessing catalyst, which comprises the above-mentioned alumina carrier with a core-shell structure.
[0027] Compared with the prior art, the present invention has the following advantages: The present invention uses flaky pseudo-boehmite as a raw material, and controls the pore structure of the alumina carrier by regulating the content of flaky pseudo-boehmite in different radial regions of the carrier. The macropore content and pore size distribution of the alumina carrier prepared by the method are in a gradient distribution of "eggshell-egg white-egg yolk", that is, the surface layer is formed by the accumulation of flaky alumina to form larger pores, the middle layer has a high macropore content and a second pore size, and the core layer is even smaller. The pore structure is conducive to the diffusion of macromolecular reactants into the interior of the carrier, and is particularly suitable for use as a catalyst carrier for heavy residue hydroprocessing with high metal (Ni, V) content. The hydroprocessing catalyst prepared with the alumina as a carrier has larger surface pores and strong resistance to metal deposition. The surface pores are not easily blocked and deactivated by metal and carbon deposition, which is conducive to the diffusion of reactants into the interior of the catalyst, thereby improving the reaction activity inside the corresponding catalyst and improving the activity stability of the catalyst. The method has a simple process for preparing flaky pseudo-boehmite. The prepared pseudo-boehmite flaky grains have a regular structure, the pores formed by the accumulation of flaky grains are open, the content of 50-150nm pores is high, and the flaky grains have good strength. The pores formed by the accumulation are not easy to collapse during the molding process, so that the pores formed by the accumulation of flaky grains are well retained in the carrier, thereby increasing the content of macropores in the carrier. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] FIG. 1 is a SEM image of the flaky pseudo-boehmite P1-1 prepared in Example 1.
[0029] FIG. 2 is an XRD spectrum of the flaky pseudo-boehmite P1-1 prepared in Example 1.
[0030] FIG3 is a SEM image of material P1-6 prepared in Comparative Example 3. Implementation
[0031] The technical scheme and technical effect of the present invention are further described below in conjunction with the embodiments, but are not limited to the following embodiments. In the present invention, wt% represents mass fraction.
[0032] BET method: N2 physical adsorption-desorption was used to characterize the pore structure of the carriers of the embodiment and the comparative example. The specific operation was as follows: The pore structure of the sample was characterized by using an ASAP-2420 N2 physical adsorption-desorption instrument. A small amount of sample was vacuum treated at 300°C for 3-4 hours, and finally the product was placed under liquid nitrogen low temperature (-200°C) for nitrogen adsorption-desorption test. The specific surface area was obtained according to the BET equation, and the pore volume and the distribution rate of pore diameters below 30nm were obtained according to the BJH model.
[0033] Scanning electron microscopy was used to characterize the microstructure of the alumina carrier. The specific operation was as follows: a JSM-7500F scanning electron microscope was used to characterize the microstructure of the carrier, with an accelerating voltage of 5 KV, an accelerating current of 20 µA, and a working distance of 8 mm.
[0034] X-ray diffraction (XRD) analysis was performed on a D / max-2500 fully automatic rotating target X-ray diffractometer produced by Rigaku Corporation, Japan, using a Cu target, Kα radiation source, graphite monochromator, tube voltage of 40 kV, and tube current of 80 mA.
[0035] Mercury intrusion method: A mercury intrusion instrument was used to characterize the pore diameter distribution of the carriers of the embodiment and the comparative example. The specific operation is as follows: The pore distribution of the sample was characterized using the American Micromeritics AutoPore 9500 fully automatic mercury intrusion instrument. After the sample was dried, it was weighed and loaded into the dilatometer, and degassed for 30 minutes under the vacuum conditions given by the instrument, and then loaded with mercury. The dilatometer was then placed in an autoclave and vented. Then, a pressure increase and pressure reduction test was performed. The mercury contact angle was 130°, and the mercury interfacial tension was 0.485N.cm -1 The distribution rate of pores with a diameter of more than 100 nm is measured by mercury intrusion porosimetry.
[0036] The most probable pore size determination: Take the material pore size as the horizontal coordinate and the rate of change of pore volume with pore size as the vertical coordinate to obtain the pore size differential distribution curve. The peak value in the curve is the most probable pore size.
[0037] In the present invention, the method for determining the average pore size of the different layers from the outer surface layer of the catalyst particles to the central core, i.e., "eggshell-egg white-yolk", is as follows: first, the pore volume, specific surface area and average pore diameter of the sample are determined by the low temperature nitrogen adsorption method (BET), and then a certain amount of the sample is taken and placed in a catalyst abrasion tester, and the sample is polished, and a certain amount of quartz sand is added to increase the wear rate. When the particle size of the sample is reduced to a certain extent after polishing, the weight loss of the sample is measured and its pore structure is measured again. From the relationship that the total pore volume and specific surface area of the sample are equal to the sum of each part, the pore volume and specific surface area of the polished part can be calculated, and 20-80 samples are measured at the same time to calculate the average pore diameter. In this way, the average pore diameter of different layers from the outer surface layer to the central core is determined.
[0038] Preparation of flake pseudo-boehmite material P1: Example 1
[0039] (1) Weigh an appropriate amount of aluminum nitrate and place it in a crucible and calcine it at 500℃ for 5.5 hours. Crushing, screening out particles larger than 200 mesh; (2) Weigh 100 g of the sieved particles and add 5.5% propylene oxide aqueous solution. 610 g, magnetically stirred for 30 minutes, then the mixture was transferred into an autoclave, sealed and heated at 145°C for 5.3 hours, and after cooling, the solid material was filtered, washed, and dried at 120°C for 4 hours to obtain pseudo-boehmite P1-1. The microstructure of the sample was observed by scanning electron microscopy to be a stack of flaky grains with a size of 120-650 nm and a thickness of 25-55 nm. The scanning electron microscopy image is shown in FIG. Figure 1 , XRD spectrum see Figure 2 , P1=1.07, P2=1.45, D(120) is 90Å, D(031) is 84Å, and D(020) is 62Å. Example 2
[0040] The same as Example 1, except that the calcination temperature of aluminum nitrate in step (1) is 550°C and the calcination time is 6.5 hours. In step (2), the concentration of propylene oxide is 6.3%, the amount of solution is 530 g, the hydrothermal treatment temperature is 130°C, and the treatment time is 6.0 hours, to obtain pseudo-boehmite P1-2. The microstructure of the sample is observed by scanning electron microscopy to be a stack of flaky grains, the size of the flaky grains is 140-680nm, the thickness is 30-65nm, P1=1.10, P2=1.41, D(120) is 87Å, D(031) is 79Å, and D(020) is 62Å. Example 3
[0041] The same as Example 1, except that the calcination temperature of aluminum nitrate in step (1) is 450°C and the calcination time is 7.5 hours. In step (2), the concentration of propylene oxide is 7.7%, the amount of solution is 410 g, the hydrothermal treatment temperature is 125°C, and the treatment time is 7.5 hours, to obtain pseudo-boehmite P1-3. The microstructure of the sample is observed by scanning electron microscopy to be a stack of flaky grains, the size of the flaky grains is 135-700nm, the thickness is 30-60nm, P1=1.14, P2=1.31, D(120) is 87Å, D(031) is 76Å, and D(020) is 66Å. Example 4
[0042] The same as Example 1, except that the calcination temperature of aluminum nitrate in step (1) is 650°C and the calcination time is 4.5 hours. In step (2), the concentration of propylene oxide is 4.2%, the amount of solution is 740 g, the hydrothermal treatment temperature is 155°C, and the treatment time is 4 hours, to obtain pseudo-boehmite P1-4. The microstructure of the sample is observed by scanning electron microscopy to be a stack of flaky grains, the size of the flaky grains is 125-650nm, the thickness is 25-65nm, P1=1.18, P2=1.36, D(120) is 87Å, D(031) is 74Å, and D(020) is 64Å.
[0043] Comparative Example 1 The same as Example 1, except that the propylene oxide in step (2) was replaced by the same amount of ethylene oxide, no lamellar grains were observed in the microstructure of the material P1-5 after hydrothermal treatment, P1=1.06, P2=1.49, D(120) was 61Å, D(031) was 58Å, and D(020) was 41Å.
[0044] Comparative Example 2 The same as Example 1, except that the aluminum nitrate in step (1) is replaced by aluminum sulfate, and the solid material particles are dissolved after hydrothermal treatment, and the product is not separated.
[0045] Comparative Example 3 The same as Example 1, except that the aluminum nitrate in step (1) was replaced by aluminum chloride. No lamellar grains were observed in the microstructure of the material P1-6 after hydrothermal treatment. The scanning electron microscope image shows: Figure 3 , P1=1.16, P2=1.63, D(120) is 81Å, D(031) is 70Å, and D(020) is 50Å.
[0046] Preparation of core-shell structure alumina materials: Example 5
[0047] Weigh 15 g of the flaky pseudo-boehmite P1-1 prepared in Example 1 and 100 g of the pseudo-boehmite Aluminium stone P2 (prepared by aluminium sulfate-sodium aluminate method, with a most probable pore size of 12.5 nm) was mixed evenly, and the mixed material was placed in a turntable molding machine for full mixing, and the inclination angle of the turntable was adjusted to 50°, and the speed of the turntable was adjusted to 15 rpm; an acetic acid aqueous solution with a mass concentration of 1% was sprayed onto the material in the turntable through a sprayer, and after mixing and contacting, the material was molded in the turntable for 30 minutes, and a spherical precursor S1 with a diameter of 2.0-3.0 mm was obtained; (2) Weigh 100 g of the flaky pseudo-boehmite P1-1 prepared in Example 1 and 125 g of the pseudo-boehmite P2, mix the above materials evenly, place the mixed materials and the spherical precursor S1 prepared in step (1) in a turntable molding machine for thorough mixing, adjust the inclination angle of the turntable to 45°, and the speed of the turntable to 12 rpm. Spray an acetic acid aqueous solution with a mass concentration of 1.2% onto the materials in the turntable through a sprayer. After mixing and contacting, the materials are molded in the turntable for 25 min to obtain a spherical precursor S2 with a diameter of 4 to 5 mm. (3) The flaky pseudo-boehmite P1-1 prepared in Example 1 and the spherical precursor S2 prepared in step (2) were placed in a turntable molding machine and mixed thoroughly. The inclination angle of the turntable was adjusted to 40° and the rotation speed of the turntable was 10 rpm. An acetic acid aqueous solution with a mass concentration of 1.3% was sprayed onto the materials in the turntable through a sprayer. After mixed contact, the materials were molded in the turntable for 20 minutes to obtain spherical materials with a diameter of 6 to 8 mm. The obtained spherical materials were dried at 120°C for 4 hours and calcined at 650°C for 4 hours to obtain a core-shell structured spherical alumina carrier S-1. The carrier properties are shown in Table 1. Example 6
[0048] The same as Example 5, except that the flaky pseudo-boehmite P1-1 in step (1), step (2) and step (3) is replaced by flaky pseudo-boehmite P1-2. The amount of pseudo-boehmite P2 added in step (1) is 70 g, and the amount of pseudo-boehmite P2 added in step (2) is 150 g, to obtain a core-shell structured spherical alumina carrier S-2. The carrier properties are shown in Table 1. Example 7
[0049] The same as Example 5, except that the flaky pseudo-boehmite P1-1 in step (1), step (2) and step (3) is replaced by flaky pseudo-boehmite P1-3. The amount of pseudo-boehmite P2 added in step (1) is 82 g, and the amount of pseudo-boehmite P2 added in step (2) is 82 g, to obtain a core-shell structured spherical alumina carrier S-3, the properties of which are shown in Table 1. Example 8
[0050] The same as Example 5, except that the flaky pseudo-boehmite P1-1 in step (1), step (2) and step (3) is replaced with flaky pseudo-boehmite P1-4. The amount of pseudo-boehmite P2 added in step (1) is 62 g, and the amount of pseudo-boehmite P2 added in step (2) is 185 g, to obtain a core-shell structured spherical alumina carrier S-4, the properties of which are shown in Table 1.
[0051] Comparative Example 4 The same as Example 5, except that the flaky pseudo-boehmite P1-1 used in step (1), step (2) and step (3) is replaced by material P1-5 prepared in comparative example 1, to obtain a comparative spherical alumina carrier S-5. The properties of the carrier are shown in Table 1.
[0052] Comparative Example 5 The same as Example 5, except that the flaky pseudo-boehmite P1-1 used in step (1), step (2) and step (3) is replaced by material P1-6 prepared in comparative example 3, to obtain a comparative spherical alumina carrier S-6. The properties of the carrier are shown in Table 1.
[0053] Table 1 Alumina support properties Example 5 Example 6 Example 7 Example 8 Comparative Example 4 Comparative Example 5 Carrier S-1 S-2 S-3 S-4 S-5 S-6 <![CDATA[Specific surface area, m 2 / g]]> 187 206 172 220 163 168 Pore volume, mL / g 0.93 0.91 0.89 0.94 0.76 0.78 10-20nm pore content, v% 47.3 49.6 44.2 53.1 60.1 62.4 50-100nm pore content, v% 16.2 14.1 18.6 12.5 7.1 4.9 Pore content greater than 100nm, v% 8.7 8.3 9.2 8.9 2.1 2.4 Thickness of the "yolk" layer, r 0.30 0.40 0.30 0.45 — — Thickness of the "protein" layer, r 0.45 0.40 0.45 0.35 — — Thickness of the "eggshell" layer, r 0.25 0.20 0.25 0.20 — — From the data in Table 1, it can be seen that the alumina carrier prepared by the method of the present invention using flaky pseudo-boehmite as raw material has a higher content of pores of 50-100nm and larger than 100nm, indicating that the pores formed by the accumulation of flaky pseudo-boehmite grains help to increase the macropore content of the carrier and regulate the pore structure. The alumina carrier prepared in the comparative example has a lower content of pores of 50-100nm and larger than 100nm. Example 9
[0054] Weigh 50 grams of the alumina carriers prepared in Examples 5-8 and Comparative Examples 4-5 respectively, and impregnate the alumina carriers in a saturated impregnation manner with a Mo-Ni-P impregnation solution having a molybdenum oxide concentration of 9.7 g / 100 mL and a nickel oxide concentration of 2.4 g / 100 mL. The impregnated materials are dried at 120°C for 6 hours, and the dried materials are calcined in air at 450°C for 6 hours to obtain hydrodemetallization catalysts Cat-1, Cat-2, Cat-3, Cat-4 and comparative hydrodemetallization catalysts Cat-5 and Cat-6.
[0055] Using a vacuum residue as raw material, the metal (Ni+V) content in the raw oil is 232μg / g. The catalytic performance of catalysts Cat-1-Cat-6 was evaluated in a fixed-bed residue hydrogenation reactor. The reaction conditions are as follows: reaction temperature is 385℃, hydrogen partial pressure is 13.5MPa, liquid hourly volume space velocity is 0.45h -1 , the hydrogen-to-oil volume ratio is 780. After 1000 hours of reaction, the content of each impurity in the generated oil is determined, and the impurity removal rate is calculated. The evaluation results are shown in Table 2.
[0056] Table 2 Comparison of catalyst hydrogenation performance Catalyst No. Cat-1 Cat-2 Cat-3 Cat-4 Cat-5 Cat-6 Relative demetallization rate, % 137 129 131 135 100 96 It can be seen from the data in Table 2 that the hydrodemetallization catalyst prepared with the alumina of the present invention as a carrier is particularly suitable for use as a catalyst carrier for hydrotreating heavy residue oil with a high metal (Ni+V) impurity content, and the hydrodemetallization catalyst prepared with the alumina as a carrier has a high hydrodemetallization activity.
Claims
1. A core-shell alumina carrier, characterized in that: The carrier has a "shell - protein - yolk" three - layer spherical structure. The "shell" layer is an aggregate of flaky alumina grains, and the "protein" and "yolk" layers are a mixed phase of an aggregate of flaky alumina grains and an aggregate of granular alumina. Among them, the mass ratio of the aggregate of flaky alumina grains to the aggregate of granular alumina in the "protein" layer is 0.1:1 - 0.3:1; the mass ratio of the aggregate of flaky alumina grains to the aggregate of granular alumina in the "yolk" layer is 0.4:1 - 1.4:1; the thickness of the "shell" layer is 0.2r - 0.5r, the thickness of the "protein" layer is 0.3r - 0.6r, and the thickness of the "yolk" layer is the remainder, where r is the radius of the alumina carrier, that is, the straight - line distance from the center of the sphere to the outer surface.
2. The core-shell alumina carrier according to claim 1, characterized in that: The size of the flaky alumina grains is 100 - 800 nm, and the thickness is 25 - 80 nm; the grain size of the granular alumina grains is 20 - 100 nm.
3. The core-shell alumina carrier according to claim 1, characterized in that: The diameter of the alumina carrier with a core - shell structure is 2 mm - 10 mm.
4. The core-shell alumina carrier according to claim 1, characterized in that: Specific surface area is 160-300m 2 / g, the pore volume is 0.8-1.2mL / g, the pore content with a diameter of 10-20nm accounts for 40%-60% of the total pore volume, the content of pores with a diameter of 50-100nm accounts for 10%-20% of the total pore volume, and the content of pores with a diameter greater than 100nm accounts for 8%-15% of the total pore volume.
5. A preparation method of the alumina carrier with a core - shell structure according to any one of claims 1 - 4, comprising the following steps: (1) Calcinate aluminum nitrate. After calcination, the material is crushed and screened. The screened material is mixed with an aqueous solution of propylene oxide, and then hydrothermally treated. After treatment, the material is filtered, washed, and dried to obtain flaky pseudoboehmite P1; (2) Mix pseudoboehmite P2 with the flaky pseudoboehmite P1 obtained in step (1) to obtain a mixed material H1, and then form it into spherical precursors S1 by rolling - ball forming; (3) Mix pseudoboehmite P2 with the flaky pseudoboehmite P1 obtained in step (1) to obtain a mixed material H2, and then mix the spherical precursor S1 with the mixed material H2 and continue rolling - ball forming to obtain spherical precursors S2; (4) Mix the flaky pseudoboehmite P1 with the spherical precursor S2, perform rolling - ball forming, and then dry and calcine to obtain the alumina carrier with a core - shell structure.
6. The method according to claim 5, characterized in that: The pseudoboehmite P1 prepared in step (1) has the following properties: 1.0 < P1 ≤ 1.3, 1.1 < P2 ≤ 1.5, P1 = D(120) / D(031), P2 = D(120) / D(020); where D(120) represents the grain size of the crystal plane corresponding to the (120) peak in the XRD pattern of the pseudoboehmite grains, and D(120) is 75 - 105 Å; D(031) represents the grain size of the crystal plane corresponding to the (031) peak in the XRD pattern of the pseudoboehmite grains, and D(031) is 70 - 90 Å; D(020) represents the grain size of the crystal plane corresponding to the (020) peak in the XRD pattern of the pseudoboehmite grains, and D(020) is 60 - 70 Å; the 120 - peak refers to the characteristic peak with 2θ of 25.5 - 29.9º in the XRD pattern; the 031 - peak refers to the characteristic peak with 2θ of 36.3 - 40.5º in the XRD pattern; the 020 - peak refers to the characteristic peak with 2θ of 12.0 - 16.2º in the XRD pattern, and D = Kλ / (Bcosθ), where K is the Scherrer constant, λ is the diffraction wavelength of the target material, B is the half - peak width of the diffraction peak, and θ is the diffraction angle.
7. The method according to claim 5, characterized in that: The calcination temperature in step (1) is 450-650° C. and the calcination time is 4-8 hours.
8. The method according to claim 5, characterized in that: The particle size of the material crushed in step (1) is greater than 100 mesh, preferably greater than 200 mesh.
9. The method according to claim 5, characterized in that: The mass percentage concentration of the propylene oxide aqueous solution in step (1) is 2.5%-12%, preferably 4%-8%, and the mass ratio of the propylene oxide aqueous solution to the powder material is 3:1-10:1, preferably 4:1-8:
1.
10. The method according to claim 5, characterized in that: The hydrothermal treatment in step (1) is carried out in a sealed container at a temperature of 110-180° C., preferably 120-160° C., for 4-8 hours. During the hydrothermal treatment, the pressure in the sealed container is autogenous pressure.
11. The method according to claim 5, characterized in that: The drying temperature in step (1) is 100-160° C., and the drying time is 2-8 hours.
12. The method according to claim 5, characterized in that: The pseudo-boehmite P2 particles in step (2) are in granular form, preferably pseudo-boehmite with a pore size greater than 10 nm.
13. The method according to claim 5, characterized in that: The mass ratio of the flaky pseudo-boehmite P1 to the pseudo-boehmite P2 in step (2) is 1:9-1:
4.
14. The method according to claim 5, characterized in that: The ball forming in step (2) is carried out in a turntable forming machine, and the rotation operating conditions of the turntable forming machine are: the inclination angle of the turntable is 40-70°, the rotation speed of the turntable is 10-30 rpm; the forming time of the material in the turntable is 10-120 min; the radius of the spherical precursor S1 is 0.2r-0.5r, where r is the radius of the final spherical alumina material, that is, the straight-line distance from the center of the sphere to the outer surface.
15. The method according to claim 5, characterized in that: The mass ratio of the flaky pseudo-boehmite P1 to the pseudo-boehmite P2 in step (3) is 3:2-3:
7.
16. The method according to claim 5, characterized in that: The ball forming in step (3) is carried out in a rotating disk forming machine, and the rotating operation conditions of the rotating disk forming machine are: the inclination angle of the rotating disk is 40-70°, the rotating speed of the rotating disk is 10-30 rpm; the forming time of the material in the rotating disk is 10-120 min. The radius of the spherical precursor S2 is 0.5r-0.8r, where r is the radius of the final spherical alumina material, that is, the straight-line distance from the center of the sphere to the outer surface.
17. The method according to claim 5, characterized in that: The ball forming in step (4) is carried out in a turntable forming machine, and the rotation operating conditions of the turntable forming machine are: the inclination angle of the turntable is 40-70°, the rotation speed of the turntable is 10-30 rpm; the forming time of the material in the turntable is 10-60 minutes, and the final sphere diameter is 5-10 mm.
18. The method according to claim 5, characterized in that: The drying time in step (4) is 1-8 hours, and the drying temperature is 60°C-180°C; the roasting temperature is 350-800°C, and the roasting time is 2-6 hours.
19. Use of the core-shell alumina carrier according to any one of claims 1 to 4 in the hydroprocessing process of heavy oil and residual oil.
20. A hydroprocessing catalyst, characterized in that: The catalyst comprises an alumina carrier with a core-shell structure according to any one of claims 1 to 4.
Citation Information
Patent Citations
Heavy oil hydrogenation catalyst and preparation method thereof
CN106140180A
High-dispersion particle catalyst applied to synthesis of hydrogen peroxide as well as preparation method and application thereof
CN107008492A
Aluminum oxide and preparation method thereof
CN110937618A
Alumina carrier with core-shell structure as well as preparation and application thereof
CN111715200A
Highly-dispersed particulate catalyst for use in hydrogen peroxide synthesis, preparation method therefor and application thereof
WO2017128946A1
Cited By
Modified alumina ball filler based on pore size gradient distribution and method for preparing the same