Heterojunction photocatalyst composite material as well as preparation method and application thereof
The La(OH)CO3/Ni2+-Al3+-LDHs composite material was prepared by hydrothermal method and biological template method, which solved the problem of carrier recombination and dispersion, improved the photocatalytic degradation efficiency of phenol, and achieved efficient phenol removal.
Patent Information
- Application Number
- CN202410771644.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-15
- Publication Date
- 2024-10-15
AI Technical Summary
Existing photocatalysts have carrier recombination problems when treating phenol wastewater, resulting in low degradation efficiency, and the combination of La(OH)CO3 and Ni2+-Al3+-LDHs is difficult to achieve uniform dispersion, affecting the photocatalytic performance.
Basic La(OH)CO3 was prepared by hydrothermal method as the substrate, and ultrathin Ni2+-Al3+-LDHs was synthesized in situ using biological template method. The hydrolysis time and urea concentration were controlled to prepare triangular heart-shaped La(OH)CO3 to achieve La( The heterojunction structure of OH)CO3/Ni2+-Al3+-LDHs composite material increases the specific surface area and active sites, and inhibits carrier recombination.
Significantly improve the photocatalytic degradation rate of phenol, the specific surface area and photocurrent performance of La(OH)CO3/Ni2+-Al3+-LDHs composite material, optimize the photocatalytic efficiency, and enhance the removal ability of phenol.
Smart Images

Figure CN118767926A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of catalysts, and in particular relates to a heterojunction photocatalyst composite material and a preparation method and application thereof. Background Art
[0002] It is very important to effectively treat phenol in wastewater. At present, the treatment methods for phenol-containing wastewater at home and abroad mainly include three categories: physical method, chemical method, biological method and photocatalytic oxidation. Photocatalytic oxidation is one of the most effective methods at present. It can not only degrade phenol in wastewater but also degrade most organic compounds in wastewater. This method has the characteristics of low reaction conditions and no secondary pollution of degradation products, which breaks the limitations of traditional methods and is one of the most popular degradation technologies at present. Its main driving force is the active groups generated during the degradation process, such as superoxide radicals (·O 2+ ) and hydroxyl radicals (·OH), especially the hydroxyl radicals (·OH) with stronger oxidizing ability, which can degrade most of the difficult-to-degrade organic pollutants and is considered to be a promising method.
[0003] Lanthanum carbonate hydroxide (La(OH)CO3) has rarely been reported for photocatalytic applications, but has been widely studied as a luminescent material due to its high fluorescence efficiency. The photogenerated charge carriers in La(OH)CO3 will have a relatively long lifetime. 3+ Lanthanum carbonate hydroxide (La(OH)CO3) is easily generated in an alkaline environment. Density functional theory (DFT) optimization of the electronic structure of La(OH)CO3 shows that the main contributors to the highest occupied valence band (VB) and the lowest unoccupied conduction band (CB) are O-2p and La-4f atomic orbitals, respectively. Since La(OH)CO3 usually lacks electrons in the 4f orbital, they have a strong affinity for electron-rich organic matter. It can be expected that La(OH)CO3 can be used as an adsorbent for removing organic waste from water, which makes the material exhibit excellent photocatalytic performance.
[0004] At the same time, La(OH)CO3, as a heterogeneous structure, can accelerate the reaction and consume photogenerated charges, especially photogenerated holes, in time, thereby avoiding photocorrosion of the photocatalytic system and improving the stability of the photocatalytic system. However, due to its small specific surface area, carriers are easy to recombine, and the morphology of La(OH)CO3 is easy to change during the preparation process, making its preparation more difficult.
[0005] Layered double hydroxides (LDHs), also known as hydrotalcite-like compounds, are a special type of two-dimensional layered functional nanomaterials consisting of positively charged metal hydroxide layers and exchangeable anions ([M 2+ 1-x M 3+x (OH)2](A n- ) x / n ·mH2O). Among them, M 2+ is a divalent metal cation, M 3+ A is a trivalent metal cation. n- The special structure of LDHs makes it possible to adjust the chemical composition of the main layer plate, the charge density and distribution of the main layer plate, the type and quantity of the intercalated guest anions, low production cost and easy synthesis, which is conducive to obtaining a large specific surface area, pore size and more active functional sites, and has a high adsorption capacity. It is considered to be a promising photocatalytic material. The unique structure and properties of LDH have led to its potential applications in ion exchangers, adsorbents, two-dimensional (2D) solid reactors, heterogeneous catalysts, and electro- and photoactive materials, etc., which have been widely studied.
[0006] The results of using LDHs to treat water containing organic pollutants showed that LDHs maintained its photocatalytic activity in three photocatalytic experiments and was considered to be a photocatalyst with high activity, long-term durability and excellent applicability. 2+ -Al 3+ -LDHs are usually flower-like nanospheres with large specific surface area, which are easy to combine with other semiconductors and are good photocatalysts. 2+ -Al 3+ -LDHs agglomerate more seriously and its carriers are easy to recombine.
[0007] Studies have shown that the removal rate of Ni is higher when the photocatalyst and adsorbent are organically combined for the treatment of wastewater containing phenolic compounds and organic dyes. 2+ -Al 3+ -LDHs and La(OH)CO3 are combined to increase its specific surface area, increase the efficiency of carrier separation, and reduce the recombination of photogenerated electrons and electron holes, thereby improving the degradation rate of phenol. By preparing ultra-thin LDHs heterojunctions and then conducting a mechanism study of photocatalytic performance, it was found that ultra-thin LDHs have good photocatalytic performance. Studies have shown that after LDHs are ultra-thin, the specific surface area can be significantly increased, more active sites can be exposed, and the migration distance of carriers in the material can be shortened. Atoms are more likely to escape from the lattice to form holes, thereby improving the conductivity.
[0008] Therefore, we should not only 2+ -Al 3+ -LDHs combines with La(OH)CO3 and also reacts with Ni 2+ -Al 3+-LDHs are ultra-thin, so the combination of the two is somewhat difficult.
[0009] Since there are a large number of hydroxyl groups on the surface of LDHs, the sheets can form hydrogen bonds through the hydroxyl groups on the surface, making LDHs easy to agglomerate, so Ni 2+ -Al 3+ -LDHs always appear as aggregated nanoflowers, which affects the photocatalytic performance. However, it is precisely because the surface of LDHs sheets carries a large number of hydroxyl groups and positive charges that LDHs nanosheets are easily combined with other nanomaterials. In order to solve the problem of easy aggregation of LDHs, the bio-template method is used to use La(OH)CO3 as the substrate, and then ultra-thin Ni is synthesized in situ on La(OH)CO3 by controlling time and temperature. 2+ -Al 3+ -LDHs. Based on ZnCo2O4, ZnAl-LDH / ZnCo2O4 composite materials were synthesized by hydrothermal method. Studies have shown that the adsorption of Congo red and doxycycline by the composite materials is optimal under acidic and neutral conditions, respectively. However, different morphologies will be produced when preparing La(OH)CO3. By controlling the hydrolysis time, reaction temperature, time and urea ratio, it was found that only the hydrolysis time and urea concentration need to be controlled to successfully prepare blocky triangular heart-shaped La(OH)CO3. During the hydrolysis process, urea provides a small amount of CO3 in the alkaline system. 2- and OH - ions to control the growth rate of La(OH)CO3, and the length of the hydrolysis time to control the growth shape of La(OH)CO3. If the hydrolysis time is too short, rod-shaped La(OH)CO3 will be generated. By studying parameters such as chelating agents, reaction temperature, and reaction time, pointed spherical and triangular heart-shaped La(OH)CO3 were successfully prepared. It was found that the triangular heart La(OH)CO3 has higher crystallinity and higher area ratio adsorption capacity. Summary of the invention
[0010] In order to comprehensively solve the above problems, the present invention provides a method for preparing a heterojunction photocatalyst composite material. By controlling the hydrolysis time, rod-shaped and triangular heart-shaped La(OH)CO3 are successfully prepared. Because the triangular heart-shaped La(OH)CO3 has a larger area ratio adsorption capacity, the triangular heart-shaped La(OH)CO3 as a substrate is more conducive to Ni 2 + -Al 3+ -LDHs are ultra-thin, making Ni 2+ -Al 3+ -LDHs sheets are evenly dispersed between sheets.
[0011] Therefore, the present invention first adopts the hydrothermal synthesis method to prepare the basic La(OH)CO3 as the substrate, and then uses the biological template method principle to control certain conditions to prepare the ultra-thin Ni 2+ -Al 3+ -LDHs, under visible light irradiation, La(OH)CO3 / Ni 2+ -Al 3+ -LDHs composite photocatalyst for the photocatalytic degradation of phenol, and found that La(OH)CO3 / Ni 2+ -Al 3+ -LDHs composite photocatalyst has a large specific surface area, a low bandgap, excellent photocurrent performance, exposes more active sites, inhibits the recombination of carriers and has excellent photocatalytic efficiency. 2+ -Al 3+ -LDHs were compared, with a focus on La(OH)CO3 / Ni 2+ -Al 3+ -LDHs composites to improve the photocatalytic performance of the possible mechanism. In summary, a series of characterization methods proved that La(OH)CO3 / Ni 2+ -Al 3+ -LDHs composites were successfully constructed.
[0012] In order to achieve the above object, the specific technical solution of the present invention is:
[0013] A heterojunction photocatalyst composite material, comprising: La(OH)CO3 / Ni 2+ -Al 3+ -LDHs.
[0014] A method for preparing a heterojunction photocatalyst composite material, comprising:
[0015] Step 1: Using La(NO3)3·6H2O and H2NCONH2 as raw materials, La(OH)CO3 was synthesized by hydrothermal method;
[0016] Step 2: Using Ni(NO3)2·6H2O, Al(NO3)3·9H2O and H2NCONH2 as raw materials, a Ni(NO3)2-Al(NO3)3-CO(NH2)2 mixed solution was prepared;
[0017] Step 3: Add La(OH)CO3 to the Ni(NO3)2-Al(NO3)3-CO(NH2)2 mixed solution, reflux and rapidly stir, and filter and recover La(OH)CO3 / Ni 2+ -Al 3+ -LDHs composites.
[0018] Preferably, step 1 comprises:
[0019] a) Step 1.1: Dissolve La(NO3)3·6H2O and H2NCONH2 in deionized water;
[0020] Step 1.2: Place the mixed solution obtained in step 1.1 in an ultrasonic bath and stir until it is completely dispersed; transfer the mixed solution to a magnetic heating stirrer at 98°C for 8h;
[0021] Step 1.3: After the reaction is completed, filter, wash with deionized water and anhydrous ethanol three times, and dry at room temperature.
[0022] Preferably, in step 1.1, La(NO3)3·6H2O is 4.8715 g, H2NCONH2 is 2.027 g, and deionized water is 500 mL.
[0023] Preferably, step 2 comprises:
[0024] Step 2.1: Dissolve Ni(NO3)2·6H2O and Al(NO3)3·9H2O in a 500 mL three-necked flask to obtain a mixed solution with a total metal cation concentration of 50 mM;
[0025] Step 2.2: Add 3.7538 g of H2NCONH2 into the flask to form
[0026] A mixed solution of Ni(NO3)2-Al(NO3)3-CO(NH2)2.
[0027] Preferably, in step 2.1, Ni 2+ / Al 3+ The molar ratio is 3:1.
[0028] Preferably, in step 3, the reflux temperature is 98° C. and the time is 8 h.
[0029] A heterojunction photocatalyst composite material is used for photocatalytic degradation of phenol.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1.La(OH)CO3 / Ni 2+ -Al 3+ -LDHs clearance rates of phenol were 2+ -Al 3+ -LDHs and La(OH)CO3 are 5.86 and 1.91 times higher.
[0032] La(OH)CO3 / Ni 2+ -Al 3+-LDHs catalysts have a large specific surface area, a low bandgap, expose more active sites, inhibit the recombination of carriers and minimize interface resistance, so they have excellent photocatalytic performance;
[0033] 2. Due to La(OH)CO3 and Ni 2+ -Al 3+ The presence of oxygen vacancies between -LDHs and the formation of S-scheme heterojunctions lead to the improvement of photocatalytic activity. In addition, through the analysis of the photocatalytic mechanism, it was determined that the main active participant of the reaction is ·O2 - and ·OH;
[0034] 3.La(OH)CO3 / Ni 2+ -Al 3+ -LDHs composite materials have the advantages of simple synthesis, low cost, high removal rate, excellent photocatalytic efficiency and stability, and can effectively remove phenol-containing wastewater. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention.
[0036] In the attached picture:
[0037] Figure 1 The figure is a flow chart of the method of the present invention.
[0038] Figure 2 SEM images: (a) Ni 2+ -Al 3+ -LDHs, (b)La(OH)CO3, (c)
[0039] La(OH)CO3 / Ni 2+ -Al 3+ -LDHs, (d)La(OH)CO3.
[0040] Figure 3 La(OH)CO3 / Ni 2+ -Al 3+ -Elemental surface scan of LDHs (the left picture shows the distribution of O, Al, Ni, and La elements, and the lower right corner shows La(OH)CO3 / Ni 2+ -Al 3+ -LDHs corresponding energy spectrum) and its corresponding SEM image (upper right)
[0041] Figure 4 La(OH)CO3 / Ni 2+ -Al 3+-LDHs transmission electron microscopy (c), (f), high-resolution transmission electron microscopy (a), (b), (d), and selected area electron diffraction image (e).
[0042] Figure 5 La(OH)CO3 / Ni 2+ -Al 3+ -XRD pattern of LDHs heterojunction (◆LDHs,*La(OH)CO3,).
[0043] Figure 6 (a)La(OH)CO3 / Ni 2+ -Al 3+ -LDHs, (b)Ni-Al-LDHs and (c)
[0044] Infrared spectrum of La(OH)CO3.
[0045] Figure 7 .La(OH)CO3 / Ni 2+ -Al 3+ -XPS high-resolution spectrum of LDHs
[0046] Figure 8 .Ni 2+ -Al 3+ -LDHs,La(OH)CO3 and La(OH)CO3 / Ni 2+ -Al 3+ -N2 adsorption–desorption isotherms and BJH pore size distribution curves of LDHs (inset).
[0047] Fig. 9 .Degradation rate of phenol by different photocatalysts under visible light irradiation at different times.
[0048] Fig.10 . Kinetic study on photocatalytic degradation of phenol by different photocatalysts.
[0049] Fig.11 .Ni 2+ -Al 3+ -LDHs, La(OH)CO3 and La(OH)CO3 / Ni 2+ -Al 3+ -UV diffuse reflectance spectrum of LDHs(S3) (a); Ni 2+ -Al 3+ -LDHs(b), La(OH)CO3(c) and La(OH)CO3 / Ni 2+ -Al 3+ -Bandgap curve of LDHs(d);
[0050] La(OH)CO3 / Ni2+ -Al 3+ -LDHs,La(OH)CO3 and Ni 2+ -Al 3+ -Transient photocurrent response of LDHs(e); Ni 2+ -Al 3+ -LDHs,La(OH)CO3 and La(OH)CO3 / Ni 2+ -Al 3+ -EIS spectrum of LDHs(f).
[0051] Fig.12 .La(OH)CO3 / Ni 2+ -Al 3+ ESR and EPR graphs of -LDHs: (a) DMPO-·OH, (b) DMPO-·O 2- ,(c)TEMPO-h + and (d) OVs.
[0052] Fig.13 .(a)Ni 2+ -Al 3+ -Mott-Schottky plot of LDHs and (b) La(OH)CO3
[0053] Fig.14 La(OH)CO3 / Ni 2+ -Al 3+ Schematic diagram of the possible photocatalytic degradation mechanism of -LDHs photocatalyst under visible light irradiation: S-type heterojunction. DETAILED DESCRIPTION
[0054] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments, but the embodiments are not intended to limit the present invention.
[0055] like Figure 1-Figure 14 , a heterojunction photocatalyst composite material, composed of: La(OH)CO3 / Ni 2+ -Al 3+ -LDHs.
[0056] Preparation Materials:
[0057] Nickel nitrate hexahydrate (Ni(NO3)2·6H2O), aluminum nitrate nonahydrate (Al(NO3)3·9H2O), urea (H2NCONH2), ethanol (C2H6O), lanthanum nitrate (La(NO3)3·6H2O), sodium persulfate (Na2S2O), polyethylene glycol 6000, potassium bromide (KBr), and phenol (C6H6O) were all reagents provided by Sinopharm Chemical Reagent Co., Ltd. They were all analytical grade reagents and did not require further purification.
[0058] A method for preparing a heterojunction photocatalyst composite material, comprising:
[0059] Step 1: Using La(NO3)3·6H2O and H2NCONH2 as raw materials, La(OH)CO3 is synthesized by hydrothermal method. It includes:
[0060] Step 1.1: Dissolve 4.8715 g La(NO3)3·6H2O and 2.027 g H2NCONH2 in 500 mL deionized water to a concentration of 90 mM.
[0061] Step 1.2: Place the mixed solution obtained in step 1.1 in an ultrasonic bath and stir until it is completely dispersed; transfer the mixed solution to a magnetic heating stirrer at 98°C for 8h;
[0062] Step 1.3: After the reaction is completed, filter, wash with deionized water and anhydrous ethanol three times, and dry at room temperature.
[0063] Step 2: Using Ni(NO3)2·6H2O, Al(NO3)3·9H2O and H2NCONH2 as raw materials, preparing a Ni(NO3)2-Al(NO3)3-CO(NH2)2 mixed solution; comprising:
[0064] Step 2.1: Dissolve 5.4525 g Ni(NO3)2·6H2O and 2.3446 g Al(NO3)3·9H2O in a 500 mL three-necked flask to obtain a total metal cation concentration of 50 mM (Ni 2+ / Al 3+ A mixed solution of 37.5 / 12.5) in a molar ratio of 37.5 / 12.5;
[0065] Step 2.2: Add 3.7538 g of H2NCONH2 into the above flask to form a mixed solution of Ni(NO3)2-Al(NO3)3-CO(NH2)2.
[0066] Step 3: Add 1.5 g / L La(OH)CO3 to a total metal cation concentration of 50 mM (Ni 2+ / Al 3+The solid product was recovered by rapid filtration and washed with deionized water and anhydrous ethanol for several times to obtain La(OH)CO3 / Ni(NO3)2-Al(NO3)3-CO(NH2)2 mixed solution with a molar ratio of 37.5 / 12.5) at 98°C for 8 hours. 2+ -Al 3+ -LDHs composites.
[0067] A heterojunction photocatalyst composite material is used for photocatalytic degradation of phenol and phenol-containing wastewater.
[0068] Phenol was used as a model compound, representing a typical water pollutant, to investigate the photocatalytic activity of the catalyst. Accurately measure 20.00 ml of the prepared phenol solution (10 μg / mL) and place it in a 20 ml quartz tube, add 0.0238 g of Na2S2O8, and then add 0.0060 g of the photocatalyst (La(OH)CO3 / Ni 2+ -Al 3+ -LDHs), firstly dark light adsorption was carried out in a quartz tube for 30 min, and then La(OH)CO3 / Ni 2+ -Al 3+ After the adsorption of phenol by -LDHs reached saturation, a visible light catalytic degradation experiment was carried out under continuous magnetic stirring. The light source was a 300W medium mercury lamp (λ=420nm), and a cutoff filter was used as a visible light radiation source. After the sample in the quartz tube was centrifuged at regular intervals, the supernatant in the centrifuge tube was extracted with a needle filter, and its absorbance was measured using a visible ultraviolet spectrometer. The same method was used to measure the absorbance of the supernatant of the product obtained at different times to investigate the effect of reaction time on the degradation of phenol.
[0069] experiment:
[0070] 1. Characterization of Samples
[0071] 1.1 Microscopic surface morphology and elemental analysis
[0072] Scanning electron microscope (SEM) images of pure Ni 2+ -Al 3+ -LDHs, La(OH)CO3 and La(OH)CO3 / Ni 2+ -Al 3+ -LDHs composites.
[0073] like Figure 2 (a) shows that pure Ni 2+ -Al 3+-LDHs have a three-dimensional structure that is flower-like and spherical with stacked nanosheets. They have a large specific surface area, but the agglomeration between them is serious and this advantage cannot be fully utilized.
[0074] Pure La(OH)CO3 Figure 2 As shown in (b) and 2(d), it is mainly composed of triangular heart-shaped (diameter 1-2um) and rod-shaped. The difference in morphology is mainly due to the large difference in hydrolysis time. It can be seen from the figure that the triangular heart-shaped La(OH)CO3 has a higher area ratio adsorption capacity, which is more conducive to the ultra-thin Ni 2+ -Al 3+ -LDHs uniform dispersion, so we choose the triangle heart-shaped La(OH)CO3 as the substrate. And the triangle heart-shaped La(OH)CO3 large and uniform crystals prevent Ni 2+ -Al 3+ -Aggregation of LDHs.
[0075] Ultra-thin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs composite material SEM images Figure 2 As shown in (c), Ni 2+ -Al 3+ -LDHs were originally grown on La(OH)CO3 in a vertical gradient manner, which not only retained the original morphology of La(OH)CO3, but also made Ni 2+ -Al 3 + -LDHs agglomeration is greatly reduced. 2+ -Al 3+ -LDHs are significantly thinner, and Ni 2+ -Al 3+ -LDHs are evenly covered on the surface of La(OH)CO3, increasing the specific surface area of the composite material, exposing more active sites, and improving the photocatalytic efficiency of the composite material. Therefore, ultra-thin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs composite material. The ultrathin La(OH)CO3 / Ni 2+ -Al 3+ One of the reasons why -LDHs composites have excellent photocatalytic performance is that they increase the specific surface area and expose more active sites.
[0076] Ultrathin La(OH)CO3 / Ni 2+ -Al 3+ - Synthesis of LDHs materials, such as Figure 3As shown in the figure, Ni, Al, La and O exist simultaneously and are evenly distributed, indicating that the composite material La(OH)CO3 / Ni 2+ -Al 3+ -LDHs built successfully.
[0077] Figure 4 (a) It shows that the two catalysts are closely connected, which is conducive to the flow of electrons and improves the electron transfer rate.
[0078] like Figure 4 (b) La(OH)CO3 / Ni was further characterized by HRTEM. 2+ -Al 3+ -LDHs composite, the observed lattice spacing is 0.231 nm, which is attributed to the reflection of the hexagonal phase (015) of LDHs.
[0079] like Figure 4 (d), the observed lattice spacing is 0.344 nm, which is attributed to the reflection of the (300) La(OH)CO3 hexagonal phase, indicating that the HRTEM results are consistent with the XRD observations.
[0080] like Figure 4 (c) and Figure 4 As shown in (f), La(OH)CO3 was used as the substrate to generate ultrathin Ni 2+ -Al 3+ -LDHs, which is consistent with the assumption.
[0081] like Figure 4 As shown in (e), selected area electron diffraction (SAED) analysis provides the 2+ -Al 3+ - Further understanding of the structure of LDHs materials. Individual nanosheets show hexagonal arrangement, confirming that La(OH)CO3 and Ni 2 + -Al 3+ -Single crystal properties of LDHs.
[0082] 1.2X-ray diffraction test
[0083] For La(OH)CO3 / Ni 2+ -Al 3+ -LDHs composites were subjected to X-ray diffraction analysis to more effectively detect the crystal plane information of the prepared catalyst. Figure 5 shown.
[0084] The diffraction peaks marked with diamonds are from Ni 2+ -Al 3+-LDHs, these peaks correspond to the diffraction peaks of hydrotalcite. The typical peaks are located at 11.72°, 23.57°, 35.12°, 39.71° and 47.27°, which correspond to the (003), (006), (012), (015) and (018) crystal planes. The diffraction peaks are narrow and strong, indicating that the sample has a high degree of crystallinity and a layered structure. Ni 2+ -Al 3+ The (003) reflection basal spacing (d) of -LDHs is 0.797 nm, which is calculated by d=(d003+2d006+3d009) / 3. 2+ -Al 3+ -LDHs have good crystallinity, which can be proved by the sharp diffraction peaks. It is consistent with the material (PDF#15-0087) card, indicating that Ni 2+ -Al 3+ -LDHs. The diffraction peaks marked by snowflakes are from La(OH)CO3, and these peaks correspond to the diffraction peaks of La(OH)CO3. The typical peaks are located at 17.61°, 24.36°, 30.28°, 35.84° and 42.97°, which are related to the (002), (300), (302), (004) and (330) crystal planes. It is consistent with the card (PDF#26-0815) of the material, hexagonal phase, lattice constants a=b=1.262nm, c=1.003nm, and no other impurity peaks, indicating that the phase purity is high.
[0085] The XRD spectrum of the composite material shows that the La(OH)CO3 / Ni 2+ -Al 3+ -LDHs consist of a hexagonal phase.
[0086] 1.3 Fourier transform infrared spectroscopy
[0087] FT-IR spectroscopy was used to analyze the structural changes and types that occupied these materials.
[0088] Ni 2+ -Al 3+ -LDHs, La(OH)CO3 and La(OH)CO3 / Ni 2+ -Al 3+ -LDHs at 4000-500cm -1 FT-IR spectra in the range Figure 6 The distribution is obvious. Figure 6 As shown in (c), La(OH)CO3 has a wavelength of 3616 and 3483 cm -1There are two small peaks at the bottom, which are caused by the stretching vibration of OH in water and the bending vibration of HOH. The CO3 of La(OH)CO3 2- The ion appears at 1074 cm -1 (v1), 775-868cm -1 (v2), 1396-1649cm -1 (v3) and 690-730cm -1 (v4) Four eigenmodes.
[0089] like Figure 6 As shown in (b), Ni 2+ -Al 3+ -LDHs at 3462cm -1 There is a broad absorption peak at the center, which is a unique absorption peak of hydrotalcite-like and is related to the stretching vibration and bending vibration of the interlayer H2O molecules and the OH of the hydroxyl-OH group. -1 The sharp band at is caused by the bending vibrations of carbonate ions embedded in the lamellar structure. Additional peaks are found at lower wavenumbers, about 766 and 564 cm -1 , which are related to the Al-O and Ni-O vibrations in the LDH lattice, respectively. Figure 6 As shown in (a), La(OH)CO3 / Ni 2+ -Al 3+ The FT-IR spectrum of the -LDHs catalyst showed a peak at 3462 cm -1 A broad absorption peak centered at 1382 cm -1 The centered band and a V1 vibration peak appear simultaneously at 1074 cm -1 This is related to the disordered structure of the LDH interlayer space, which causes the interlayer carbonate ions to move from D 3h Symmetric transformation to C 2v In addition, 1637 and 856 cm -1 The peaks at and are attributed to the symmetric stretching vibration (ν3) and out-of-plane deformation (ν2) of metal carbonates, which are the characteristics of La(OH)CO3 in the composite. 2+ -Al 3+ -LDHs composite heterojunction was successfully prepared.
[0090] 1.4XPS analysis
[0091] In order to determine the ultrathin La(OH)CO3 / Ni 2+ -Al 3+-LDHs catalytic material surface chemical composition and element valence state, XPS study was carried out. XPS spectrum confirmed the presence of C, O, Si, Ag, Ni elements ( Figure 7 (a)). Figure 7 As shown in the Al2P spectrum (b), the peaks at 74.5eV, 70.7eV, and 68.1eV are all attributed to Al 3+ , but 70.7eV and 68.1eV are attributed to the metal ion Al in LDHs 3+ The peak at 74.5 eV is attributed to Al in aluminum hydroxide. 3+ ; Ni2p high resolution XPS spectrum ( Figure 7 (c) shows that the peak at 851.1 eV in the Ni2p spectrum is due to the Ni δ+ 2p 3 / 2 It is a component of the nickel-phosphorus bond. Ultra-thin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs consists of two peaks with binding energies of 855.7eV and 873.1eV, which belong to the Ni2p3 / 2 energy level and Ni2p1 / 2 energy level, respectively, and belong to the hydroxylated Ni-O groups in the bulk layer. At the same time, 861.6 and 879.4 are two satellite peaks corresponding to the Ni2p3 / 2 and Ni2p1 / 2 energy levels, respectively, indicating the presence of high-spin divalent states in Ni; Figure 7 The La3d spectrum of (d) shows that it is a typical La 3+ The compound has two binding energies consisting of 851.9 eV and 835 eV peaks, which belong to the La3d 3 / 2 energy level and La3d 5 / 2 energy level, respectively, with an energy difference of 16.9 eV, which is similar to La 3+ The characteristic peaks of O1s are exactly the same. Figure 7 (e) shows that the deconvolution is divided into three different peaks, 531.3 eV belongs to OH in the metal layer, 529.2 eV belongs to CO3 2- The oxygen in the root ion, 533.1eV belongs to the oxygen in the interlayer water molecules; the C1s spectrum is as follows Figure 7 (f) shows that the peak at 284.4 eV is generated by CC, the peak at 286.4 eV is generated by CO, and the peak at 288.7 eV is generated by C=O. These changes in binding energy indicate that La(OH)CO3 and Ni 2 + -Al 3+ -LDHs form a heterojunction rather than a passive physical mixture. 2+ -Al 3+ -LDHs composite photocatalyst provides a theoretical basis for the formation of heterojunction.
[0092] 1.5BET Results
[0093] Pure Ni 2+ -Al 3+ -LDHs, La(OH)CO3 and ultrathin La(OH)CO3 / Ni 2+ -Al 3+ N2 adsorption-desorption isotherms of -LDHs composites and BJH pore size distribution curves at different reaction times (inset). Figure 8 As shown. 2+ -Al 3 + -LDHs, La(OH)CO3 and ultrathin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs composites have obvious hysteresis loops, so the nitrogen isotherms are all type IV, indicating that these photocatalysts contain mesoporous and microporous substances. 2+ -Al 3+ -LDHs(137.05m 2 / g) and pure La(OH)CO3(2.29867m 2 / g) compared with ultra-thin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs photocatalyst has a relatively high specific surface area (SBET) (124.916 m 2 / g), as shown in Table 1, the results are as expected. The results show that under visible light irradiation, the composite material can provide more active sites for photocatalytic degradation of pollutants.
[0094] Table 1 BET surface areas of Ni 2+ -Al 3+ -LDHs,La(OH)CO3 and La(OH)CO3 / Ni 2+ -Al 3+ -LDHs samples.
[0095]
[0096] 2. Photocatalytic degradation of phenol
[0097] For ultra-thin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs photocatalytic behavior of phenol and Ni 2+ -Al 3+ The degradation performance of phenol by -LDHs and La(OH)CO3 was compared. The results showed that the presence of the catalyst significantly enhanced the photodegradation of phenol.
[0098] La(OH)CO3 / Ni 2+ -Al 3+ -LDHs photocatalytic activity is significantly higher than that of ultrathin Ni 2+ -Al 3+ -LDHs and La(OH)CO3.
[0099] Vislight irradiation and ultrathin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs, La(OH)CO3 and Ni 2+ -Al 3+ The photodegradation kinetics of phenol was monitored by the change of phenol concentration (C) relative to the initial concentration (C0) under the action of -LDHs catalyst. Fig. 9 ). The degradation effect of the catalyst on phenol solution under dark reaction conditions was demonstrated.
[0100] It can be seen that under the dark reaction environment, from 0 to 30 min, the concentration of the phenol solution showed a certain downward trend, and there was no obvious change in the concentration of the phenol solution as time went on. After 30 minutes of dark exposure, the adsorption between the catalyst and the phenol solution reached equilibrium, so all subsequent studies were conducted on the basis of 30 minutes of dark application. As a control, the experiment was repeated in the absence of any photocatalyst. In the absence of a catalyst, 10 μg / mL of phenol was not degraded under 160 min of illumination, indicating that the photolysis reaction contributed little to the degradation of phenol. However, the La(OH)CO3 catalyst greatly promoted the photodegradation. In particular, Ni 2+ and Al 3+ Doped La(OH)CO3 materials (ultra-thin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs) significantly improved the photocatalytic performance and almost completely decomposed phenol within 160 min, which was comparable to La(OH)CO3 and Ni 2+ -Al 3+ -LDHs, ultrathin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs have stronger photodegradation ability. It may be La(OH)CO3 and Ni 2+ -Al 3+ The complexation of -LDHs enhances the active sites and promotes their absorption of visible light.
[0101] Quantitative comparison of photocatalytic reaction kinetics ( Fig.10) to gain a deeper understanding of the photocatalytic performance of the three samples. The kinetic model was established using -ln(C / C0)=kt, where k is the degradation rate constant. 2+ -Al 3+ -LDHs and La(OH)CO3 / Ni 2+ -Al 3+ The k of -LDHs(S3) were linearly fitted to 0.00434, 0.00095 and 0.01558min, respectively. -1 , among which ultrathin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs has the largest k, which is 0.01558min -1 , indicating that La(OH)CO3 effectively improves the photocatalytic activity. 2+ -Al 3+ -LDHs heterostructures expose more active sites. Ultrathin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs have a large specific surface area and excellent photocatalytic performance. The observation results are consistent with the photocatalytic decomposition mentioned above.
[0102] 3. Photocatalytic performance and mechanism
[0103] The ultraviolet-visible diffuse reflectance spectroscopy (UV-vis diffuse reflectance spectroscopy) was used to characterize the pure Ni 2+ -Al 3+ -LDHs, La(OH)CO3 and ultrathin La(OH)CO3 / Ni 2+ -Al 3+ The optical properties of -LDHs materials were studied.
[0104] Further understanding of ultrathin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs has a higher structural basis for photocatalytic activity than the other two catalysts. Fig.11 (a) Pure Ni 2+ -Al 3+ -LDHs has two absorption bands in the ultraviolet region and visible light region, in the range of 325-400nm and 550-700nm respectively. Pure La(OH)CO3 only absorbs ultraviolet light, but ultraviolet light only accounts for 1 / 4 of the full spectrum, so La(OH)CO3 has little utilization of the spectrum. However, Ni 2+ -Al 3+ -LDHs doping significantly improves the ultrathin La(OH)CO3 / Ni 2+ -Al 3+-LDHs light absorption range, which may be due to the formation of heterojunction in the composites.
[0105] Therefore, the enhancement of the visible light absorption range can provide more photogenerated carriers for photocatalytic performance. The Kubelka-Munk formula is used to measure the band gap of the semiconductor. Since the semiconductor band gap width is Fig.11 (b) Fig.11 (c) and Fig.11 (d) shows the intercept of the tangent part on the x-axis, so Ni 2+ -Al 3+ -LDHs, La(OH)CO3 and ultrathin La(OH)CO3 / Ni 2+ -Al 3 + -LDHs have band gap energies of 2.31eV, 2.25eV, and 2.12eV, respectively. According to the solid energy band theory and photocatalytic mechanism, Ni 2 + -Al 3+ -LDHs addition significantly reduced the ultra-thin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs have a low bandgap, which is the reason for their higher visible light PCA, making them more conducive to improving photocatalytic performance.
[0106] In addition, ultrathin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs have a high specific surface area, which makes them highly adsorbable to organic molecules and provides a promising target for photoinduced e - 、-h + It provides more active sites. 2+ -Al 3+ -LDHs, La(OH)CO3 and ultra-thin
[0107] La(OH)CO3 / Ni 2+ -Al 3+ The photocurrent and electrochemical impedance spectroscopy (EIS) tests of -LDHs further confirmed the 2+ -Al 3+ -LDHs-bound heterostructures had the highest charge separation efficiency.
[0108] like Fig.11 As shown in (e), Ni 2+ -Al 3+ -LDHs, La(OH)CO3 and ultrathin La(OH)CO3 / Ni 2+ -Al 3+The photocurrent intensity of the -LDHs composite material during 30s cycling on and off. Essentially, the lower transient photocurrent response signal indicates that the recombination of electrons and holes is faster. The results show that compared with pure Ni 2+ -Al 3+ -LDHs and La(OH)CO3, ultra-thin La(OH)CO3 / Ni 2 + -Al 3+ -LDHs materials have higher photocurrent density.
[0109] Therefore, ultrathin La(OH)CO3 / Ni 2+ -Al 3+ The significantly enhanced photocatalytic activity of -LDHs is also attributed to the increased electron separation and improved charge transfer kinetics under irradiation. 2+ -Al 3+ The growth of heterojunction in the -LDHs complex suppresses the recombination of photogenerated electron-hole pairs while enabling the smooth separation of photogenerated carriers.
[0110] EIS is particularly used to study the transfer resistance and separation rate of photogenerated carriers in semiconductors. The minimum transfer and separation resistance of photoexcited carriers is represented by a shorter radius. Fig.11 (f) shows that compared with pure Ni 2+ -Al 3+ -LDHs and La(OH)CO3, ultra-thin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs component has the weakest curve radius. 2+ -Al 3+ -LDHs catalysts have minimal interfacial resistance, large photogenerated carrier transfer rate and slow electron-hole pair complexation.
[0111] Based on these results, three steps involved in the decomposition mechanism were deduced. Initially, phenol molecules were adsorbed on the LDH surface. Second, phenol was photocatalytically decomposed into CO2, H2O, and ions under visible light irradiation. Third, inorganic molecules and ions were absorbed by LDHs as photocatalytic products.
[0112] The absorption of photons by the catalyst and the resulting e - and h + The transfer of is the main factor controlling the photocatalytic reaction related to the electronic structure of the material. Generally, the photon absorption of the photocatalyst depends on the e - / h +The mobility of the photocatalyst surface affects the possibility of reaching the reaction site. Based on the photocatalytic experimental results, this paper proposes and discusses the ultrathin La(OH)CO3 / Ni 2+ -Al 3+ Potential mechanism of phenol decomposition by -LDHs ( Fig.14 ).
[0113] Electron spin resonance (ESR) was used to study the ultrathin
[0114] La(OH)CO3 / Ni 2+ -Al 3+ -LDHs samples·O 2+ and ·OH active species concentration. Fig.12 As shown in Figure 2, no signal was detected for the sample in the dark, indicating that no reaction species were produced without light excitation. After 10 min of illumination, the observed ESR signal was attributed to the ultrathin La(OH)CO3 / Ni composite material. 2+ -Al 3+ -O on LDHs samples 2+ and ·OH radicals. At the same time, Fig.12 TEMPO-h + The signal is very strong in dark conditions, but decreases with longer periods of light exposure.
[0115] The results showed that: ·OH, ·O 2+ and h + All of them play an important role in the photocatalytic process. Combining the active species capture and ESR measurement results, it is further concluded that ·OH, ·O 2- and h + All of them are involved in the photocatalytic degradation of phenol. In addition, the ultrathin La(OH)CO3 / Ni 2+ -Al 3+ -The presence of oxygen vacancies (OVs) in LDHs samples ( Fig.12 d). Under visible light irradiation, paramagnetic OVs with g = 2.004 are assigned to the electrons trapped on the OVs, confirming the existence of OVs and the ultrathin La(OH)CO3 / Ni 2+ -Al 3+ -The effective generation of active species in the LDHs photocatalyst. If the OVs concentration in the photocatalyst is high enough, a free OVs band can theoretically be induced below the conduction band. More surface OVs will produce more photocatalytic active centers, which is beneficial to capture photogenerated electrons, prevent the recombination of photogenerated electron-hole pairs, and ultimately improve the photocatalytic performance.
[0116] By Mott-Schottky plot and measuring Ni 2+ -Al3+ The flat band potentials of -LDHs and La(OH)CO3 confirm the heterojunction type of the composite. Fig.13 (a,b) are Ni 2+ -Al 3+ -LDHs and La(OH)CO3 Mott-Schottky curves. As shown in the figure, the sample curve has a positive slope, indicating that Ni 2+ -Al 3+ -LDHs and La(OH)CO3 are both typical n-type semiconductors. The flat band potentials relative to Hg / Hg2Cl2 are -0.78eV and -0.63eV respectively. To obtain the standard hydrogen electrode, we use the formula E NHE =E Hg / Hg2Cl2 +0.059*pH-E0 Hg / Hg2Cl2 To evaluate E NHE Among them, E 0 Hg / Hg2Cl2 About 0.241ev, Na2SO4 electrolyte solution pH is 5.0. Ni 2+ -Al 3+ The CB potentials of -LDHs and La(OH)CO3 are -0.539eV and -0.389eV, respectively. Fig.11 It can be seen that the energy band of La(OH)CO3 is 2.25eV, while Ni 2+ -Al 3+ The band energy of -LDHs is 2.31eV. Using equation E VB =Eg+E CB Calculate Ni 2+ -Al 3+ The VB potentials of -LDHs and La(OH)CO3 are 1.771eV and 1.861eV, respectively. Finally, the clear band structures of these photocatalysts are shown in Figure 2. Fig.13 shown.
[0117] Active species capture and ESR (DMPO-·OH, DMPO-·O2 - TEMPO-h + and OVs) experiments and the results of flat band potential show that ultrathin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs composites are likely to have OVs-modified s-type heterojunctions ( Fig.14 ). The S-type heterojunction consists of an oxidized photocatalyst (OP) and a reduced photocatalyst (RP), which can be used to vividly describe the transfer path of electrons from low to high positions, which is similar to the "steps" of a ladder in macroscopic terms. La(OH)CO3 and Ni 2+ -Al 3+There is charge transfer at the interface of -LDHs. Photogenerated electrons are transferred from the CB of La(OH)CO3 to Ni 2+ -Al 3+ -VB of LDHs, inhibiting the rapid recombination rate and prolonging the carrier lifetime, thereby improving the photocatalytic activity.
[0118] It is worth mentioning that the obtained ultrathin La(OH)CO3 / Ni 2+ -Al 3+ -The OVs in LDHs may play a role in the CB of La(OH)CO3 and Ni 2+ -Al 3+ -LDHs VB bridge, thereby accelerating the electron transfer rate. Due to the presence of VOs and La(OH)CO3 and Ni 2+ -Al 3+ -LDHs form an S-scheme heterojunction on Ni 2+ -Al 3+ The strong photogenerated electrons e are retained in the CB(RP) of -LDHs and the VB(OP) of La(OH)CO3. - and hole h + .
[0119] Because you 2+ -Al 3+ -LDHs have a more negative CB potential than the standard reduction potential, so Ni 2+ -Al 3+ -Photoelectrons on LDHs CB - Can generate O2 with adsorbed O2 - Since the VB potential of La(OH)CO3 is greater than the standard oxidation potential, it can oxidize H2O / OH - OH- in the , produces ·OH. It is very likely that part of ·O2 - The other part directly degrades phenol, and the other part reacts with water in the solution to generate ·OH. + It can also directly oxidize phenol into small molecule intermediates.
[0120] The photocatalytic degradation mechanism of phenol by La(OH)CO3 / Ni2+-Al3+-LDHs is described as follows:
[0121] Sample La(OH)CO3 / Ni2+-Al3+-LDHs+phenol→sample
[0122] La(OH)CO3 / Ni2+-Al3+-LDHs (adsorption and desorption).
[0123] La(OH)CO3+hν→La(OH)CO3(e -+h + ).
[0124] Ni 2+ -Al 3+ -LDHs+hν→Ni 2+ -Al 3+ -LDHs(e - +h + ).
[0125] La(OH)CO3(e)→VOs(e - ) → Ni 2+ -Al 3+ -LDHs(h + ).
[0126] O2+Ni 2+ -Al 3+ -LDHs → ·O2 - .
[0127] O2 - +2H2O→2·OH+2OH - .
[0128] La(OH)CO3(h + )+OH – → ·OH.
[0129] La(OH)CO3(h + )+H2O→·OH+H + .
[0130] Phenol + active species (·O2 - ,h + ,·OH)→small molecular,H2O and CO2.
[0131] 4. Conclusion
[0132] In this study, a hydrothermal method was used to prepare ultra-La(OH)CO3 / Ni with high catalytic performance and high crystallinity. 2+ -Al 3+ -LDHs composite heterojunctions were fabricated and their physicochemical properties and photocatalytic degradation of phenol were evaluated. Ultrathin Ni 2+ -Al 3+ -LDHs, and for ultrathin Ni 2+ -Al 3+ -LDHs were uniformly loaded. Through a series of characterization techniques, ultrathin La(OH)CO3 / Ni 2+ -Al 3+-LDHs heterojunction. At the same time, the photocatalytic analysis shows that the ultra-thin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs heterojunction has a significantly better photocatalytic degradation efficiency for phenol than pure La(OH)CO3 and pure Ni 2+ -Al 3+ -LDHs. The reason is that ultra-thin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs photocatalyst has a larger SSA (124.916 m2 / g) and a narrower band gap (2.12 eV), which promotes the separation of photogenerated electron-hole pairs. 2+ -Al 3+ -LDHs, strong photoelectrons - and hole h + The presence of VOs and the formation of an s-type heterojunction were detected. The photogenerated electrons were transferred from the CB of La(OH)CO3 to Ni 2+ -Al 3+ -LDHs VB, inhibits the recombination rate of carriers, prolongs the carrier lifetime, and thus improves the photocatalytic activity. This paper provides a convenient and concise synthesis method, and the research results show that ultrathin La(OH)CO3 / Ni 2+ -Al 3+ -LDHs has the advantages of non-toxicity, low cost and high removal capacity. It is a promising photocatalyst for the degradation of phenol-containing wastewater in wastewater, providing a useful method for the photocatalytic degradation of organic wastewater.
[0133] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A heterojunction photocatalyst composite material, characterized in that: Composition: <h2 style=";text-align:left;direction:ltr">La(OH)CO3 / Ni<h2 style=";text-align:left;direction:ltr"> 2+ <h2 style=";text-align:left;direction:ltr"> -Al<h2 style=";text-align:left;direction:ltr"> 3+ <h2 style=";text-align:left;direction:ltr"> -LDHs.
2. A method for preparing a heterojunction photocatalyst composite material, characterized in that: include Step 1: Using La(NO3)3·6H2O and H2NCONH2 as raw materials, La(OH)CO3 was synthesized by hydrothermal method; Step 2: Using Ni(NO3)2·6H2O, Al(NO3)3·9H2O and H2NCONH2 as raw materials, a Ni(NO3)2-Al(NO3)3-CO(NH2)2 mixed solution was prepared; Step 3: Add La(OH)CO3 to the Ni(NO3)2-Al(NO3)3-CO(NH2)2 mixed solution, reflux and stir rapidly, and filter and recover La(OH)CO3 / Ni 2+ -Al 3+ -LDHs composites.
3. The method for preparing a heterojunction photocatalyst composite material according to claim 2, characterized in that: Step 1 includes: Step 1.1: Dissolve La(NO3)3·6H2O and H2NCONH2 in deionized water; Step 1.2: Place the mixed solution obtained in step 1.1 in an ultrasonic bath and stir until it is completely dispersed; transfer the mixed solution to a magnetic heating stirrer at 98°C for 8h; Step 1.3: After the reaction is completed, filter, wash with deionized water and anhydrous ethanol three times, and dry at room temperature.
4. The method for preparing a heterojunction photocatalyst composite material according to claim 3, characterized in that: In step 1.1, La(NO3)3·6H2O is 4.8715 g, H2NCONH2 is 2.027 g, and deionized water is 500 mL.
5. The method for preparing a heterojunction photocatalyst composite material according to claim 4, characterized in that: Step 2 includes: Step 2.1: Dissolve Ni(NO3)2·6H2O and Al(NO3)3·9H2O in a 500 mL three-necked flask to obtain a mixed solution with a total metal cation concentration of 50 mM; Step 2.2: Add 3.7538 g of H2NCONH2 into the flask to form a mixed solution of Ni(NO3)2-Al(NO3)3-CO(NH2)2.
6. The method for preparing a heterojunction photocatalyst composite material according to claim 5, characterized in that: Step 2.1 Ni 2+ / Al 3+ The molar ratio is 3:
1.
7. The method for preparing a heterojunction photocatalyst composite material according to claim 6, characterized in that: In step 3, the reflux temperature is 98° C. and the time is 8 h.
8. The heterojunction photocatalyst composite material according to claim 1, characterized in that: Applied to the photocatalytic degradation of phenol.