Preparation method of NiSnO3 modified B doped porous g-C3N4 nanotube composite photocatalyst

The preparation of the composite photocatalyst of the B-doped porous g-C3N4 nanotube modified NiSnO3 was solved, and the specific surface area of ​​the two-dimensional carbon nitride nanosheets was small and the photogenerated charge separation efficiency was low, achieving efficient photocatalytic activity and good cycles Stability, suitable for industrial applications.

CN118892840APending Publication Date: 2024-11-05HARBIN NORMAL UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410921659.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing two-dimensional carbon nitride nanosheets have a small specific surface area and low photogenerating charge separation efficiency, which limits their photocatalytic performance.

Method used

The preparation method of B-doped porous g-C3N4 nanotube composite photocatalyst is prepared by one-step calcination method, and the NiSnO3 nanoparticles are dispersed by ultrasonic to form a composite photocatalyst, which is enhanced. Light absorption capacity and charge separation efficiency.

Benefits of technology

It has achieved efficient visible light decomposition of aquatic hydrogen, with photocatalytic activity of 5632.57μmol·g-1·h-1, with good cycle stability and green environmental protection characteristics, and is suitable for large-scale production and industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892840A_ABST
    Figure CN118892840A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a NiSnO3 modified B doped porous g-C3N4 nanotube composite photocatalyst, and belongs to the field of photocatalyst preparation. The problems that an existing two-dimensional carbon nitride nanosheet is small in specific surface area and low in photo-generated charge separation efficiency are solved. The method comprises the following steps: preparing B-doped porous g-C3N4 nanotubes, and dispersing the B-doped porous g-C3N4 nanotubes in N, N-dimethylformamide; 2, preparing NiSnO3 nano particles, and dispersing the NiSnO3 nano particles in n-hexane; and mixing the NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst with the g-C3N4 nanotube composite photocatalyst. The method has the advantages of easily available raw materials, simple process, low cost, high benefit, no toxicity and no pollution, and is suitable for large-scale production. The composite photocatalyst disclosed by the invention is used as a photocatalyst for decomposing water to produce hydrogen by visible light, the photocatalytic activity of the composite photocatalyst is as high as 5632.57 [mu] mol.g <-1 >. H <-1 >, and the composite photocatalyst shows excellent catalytic activity and good cycle stability and has a wide practical application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of photocatalyst preparation, and specifically relates to a method for preparing a NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst. Background Art

[0002] With the continuous development of science and technology in human society, the world is gradually moving towards urbanization and industrialization. During the development, energy is also consumed in large quantities. The mining and use of non-renewable fossil fuels will cause environmental pollution, inevitably leading to the scarcity of fossil fuel resources and the deterioration of the environment. Photocatalysts can directly use sunlight as a light source to decompose water and release hydrogen. Hydrogen can be used as a convenient high-energy density energy source with high calorific value and pollution-free combustion products.

[0003] Carbon nitride is a two-dimensional non-metallic organic polymer semiconductor material with the advantages of being cheap, readily available, and environmentally friendly, but it has the disadvantages of limited visible light absorption, small specific surface area, and low efficiency of photogenerated charge separation. In recent years, people have proposed a variety of strategies to overcome the above shortcomings to improve photocatalytic performance, including element doping, morphology control, and heterojunction construction.

[0004] Element doping can adjust its light absorption capacity and the recombination rate of photogenerated carriers, thereby improving the photocatalytic activity of the material. Element doping includes metal doping and non-metal doping. Compared with metal doping, non-metal doping can maintain the non-metallic properties of carbon nitride materials. Compared with traditional carbon nitride nanosheets, the longer axial length of carbon nitride nanotubes allows multiple reflections of the incident light, improving the capture of light; and the axial mass transfer process of the nanotubes accelerates the photocatalytic reaction process. However, researchers can only make larger boron-doped micron-sized carbon nitride tubes at present, and there has been no report on the one-step preparation of hollow and porous nanoscale boron-doped carbon nitride nanotubes. Summary of the invention

[0005] The purpose of the present invention is to solve the problems of small specific surface area and low photogenerated charge separation efficiency of existing two-dimensional carbon nitride nanosheets, and to provide a method for preparing NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst.

[0006] A method for preparing NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst, which is carried out according to the following steps:

[0007] 1. Preparation of B-doped porous g-C3N4 nanotubes:

[0008] Urea and m-aminophenylboronic acid are placed in a crucible, and then heated in an oven until they are melted. After melting, the crucible is taken out and naturally cooled to room temperature, and then placed in a muffle furnace for calcination. After the calcination is completed, the crucible is cooled to room temperature to obtain B-doped porous g-C3N4 nanotubes.

[0009] 2. Preparation of NiSnO3 nanoparticles:

[0010] NiCl3·6H2O and K2SnO3·3H2O were dissolved in distilled water respectively, then mixed and stirred for 30 minutes, and then transferred to a high-pressure reactor and subjected to hydrothermal reaction in an oven. The obtained solid was washed, centrifuged, dried, and then calcined in a muffle furnace to obtain NiSnO3 nanoparticles.

[0011] 3. Preparation of NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst:

[0012] The B-doped porous g-C3N4 nanotubes were ultrasonically dispersed in N,N-dimethylformamide to obtain solution A, and the NiSnO3 nanoparticles were ultrasonically dispersed in n-hexane to obtain solution B;

[0013] The above solution A and solution B are mixed and 10 mL of anhydrous ethanol is added. After ultrasonic dispersion for 1 hour, the product is collected by centrifugation, washed and then dispersed in anhydrous ethanol. Finally, the target product is collected by centrifugation, washed and dried to obtain NiSnO3 modified B doped porous g-C3N4 nanotube composite photocatalyst, thus completing the preparation method.

[0014] Furthermore, the amount of urea in step 1 is 10 g, and the amount of m-aminophenylboronic acid is 2.5 mg to 25 mg.

[0015] Furthermore, the heating rate in step 1 is 1 to 5°C / min.

[0016] Furthermore, the calcination temperature in step 1 is 400-600° C., and the calcination time is 2-4 hours.

[0017] Furthermore, the NiCl3·6H2O and K2SnO3·3H2O described in step 2 are respectively dissolved in distilled water: 1 mmol of NiCl3·6H2O and 1 mmol of K2SnO3·3H2O are respectively dissolved in 10 mL of distilled water.

[0018] Furthermore, the hydrothermal reaction in step 2 is carried out at 150-200° C. for 18-24 hours.

[0019] Furthermore, the cleaning, centrifugation and drying in step 2 are as follows: washing with distilled water and anhydrous ethanol for 3 times respectively, then centrifuging at 8000r / min for 5 minutes, and then vacuum drying at 60°C for 6 to 10 hours.

[0020] Furthermore, the calcination temperature in step 2 is 300-350° C., and the calcination time is 2-6 hours.

[0021] Furthermore, in step three, 0.1 g of B-doped porous g-C3N4 nanotubes were ultrasonically dispersed in 15 mL of N,N-dimethylformamide to obtain solution A, and 5 mg to 15 mg of NiSnO3 nanoparticles were ultrasonically dispersed in 15 mL of n-hexane to obtain solution B.

[0022] Furthermore, the ultrasonic dispersion time in step 3 is 30 minutes.

[0023] Furthermore, the washing in step 3: washing with anhydrous ethanol for 2 to 3 times; the dispersing: magnetic stirring for 10 hours.

[0024] Furthermore, the washing and drying in step 3: washing with anhydrous ethanol for 2 to 3 times, and then drying at 60° C. for 12 to 16 hours.

[0025] Furthermore, the centrifugation in step 3 is performed at a speed of 8000 to 10000 r / min for 3 to 5 min.

[0026] The present invention has the following advantages and beneficial effects:

[0027] (1) The present invention prepares a NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst, the raw materials of which are easily available, the process is simple, low-cost, high-efficiency, non-toxic and pollution-free, suitable for large-scale production, and is expected to move towards industrial application and has good application prospects.

[0028] (2) The present invention prepares a NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst. First, a one-step calcination method is used to prepare B-doped porous g-C3N4 nanotubes. While successfully doping B elements into carbon nitride nanotubes, the catalyst surface presents a rich nanopore structure during the calcination process. The nanotube diameter is about 180nm, the tube wall thickness is about 40nm, and a unique one-dimensional tubular structure is formed, which provides a convenient channel for the transfer of photogenerated electrons and effectively inhibits the recombination of photogenerated carriers.

[0029] (3) The present invention prepares a NiSnO3-modified B-doped porous g-C3N4 nanotube composite photocatalyst as a photocatalyst for the decomposition of water to produce hydrogen under visible light, and its photocatalytic activity is as high as 5632.57 μmol·g -1 ·h -1, showing excellent catalytic activity and good cycle stability; NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst has the advantages of wide light absorption range, low electron-hole pair recombination rate, good photocatalytic performance, good stability, green and environmental protection, etc. It can be widely used in the field of photocatalysis, and has good photocatalytic performance and broad practical application prospects.

[0030] (4) NiSnO3 in the present invention has good visible light absorption capacity. The use of NiSnO3 nanoparticles and B-doped porous g-C3N4 nanotubes to compositely construct heterojunctions can not only improve the light absorption performance of the catalyst, but also accelerate the transfer and separation efficiency of charges through the interface effect between NiSnO3 and B-doped porous g-C3N4 nanotubes, which can further improve the photocatalytic activity. This greatly breaks through the bottleneck problems of limited visible light absorption capacity, small specific surface area and low photogenerated charge separation efficiency, making practical application and industrial production possible.

[0031] The invention is suitable for the preparation of NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The SEM images and EDS images of B-doped porous g-C3N4 nanotubes containing different amounts of m-aminophenylboronic acid, wherein part a is the microscopic morphology of boron-doped carbon nitride in Example 3, part b is the microscopic morphology of boron-doped carbon nitride in Example 4, part c is the microscopic morphology of B-doped porous g-C3N4 nanotubes in Example 1, part d is the microscopic morphology of boron-doped carbon nitride in Example 5, part e is the microscopic morphology of boron-doped carbon nitride in Example 5, and part f is the EDS image of B-doped porous g-C3N4 nanotubes in Example 1;

[0033] Figure 2 TEM images of B-doped porous g-C3N4 nanotubes, NiSnO3 nanoparticles and NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalysts, wherein part a is the TEM image of B-doped porous g-C3N4 nanotubes in Example 1, part b is the TEM image of NiSnO3 nanoparticles in Example 1, part c is the TEM image of NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst in Example 1, and part d is the HRTEM image of part c;

[0034] Figure 3 It is a bar chart of the photocatalytic hydrogen production rate of comparative example 1, B-doped porous g-C3N4 nanotubes, NiSnO3 nanoparticles and NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.

[0036] Specific implementation method 1: This implementation method is a method for preparing a NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst, which is carried out in the following steps:

[0037] 1. Preparation of B-doped porous g-C3N4 nanotubes:

[0038] Urea and m-aminophenylboronic acid are placed in a crucible, and then heated in an oven until they are melted. After melting, the crucible is taken out and naturally cooled to room temperature, and then placed in a muffle furnace for calcination. After the calcination is completed, the crucible is cooled to room temperature to obtain B-doped porous g-C3N4 nanotubes.

[0039] 2. Preparation of NiSnO3 nanoparticles:

[0040] NiCl3·6H2O and K2SnO3·3H2O were dissolved in distilled water respectively, then mixed and stirred for 30 minutes, and then transferred to a high-pressure reactor and subjected to hydrothermal reaction in an oven. The obtained solid was washed, centrifuged, dried, and then calcined in a muffle furnace to obtain NiSnO3 nanoparticles.

[0041] 3. Preparation of NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst:

[0042] The B-doped porous g-C3N4 nanotubes were ultrasonically dispersed in N,N-dimethylformamide to obtain solution A, and the NiSnO3 nanoparticles were ultrasonically dispersed in n-hexane to obtain solution B;

[0043] The above solution A and solution B are mixed and 10 mL of anhydrous ethanol is added. After ultrasonic dispersion for 1 hour, the product is collected by centrifugation, washed and then dispersed in anhydrous ethanol. Finally, the target product is collected by centrifugation, washed and dried to obtain NiSnO3 modified B doped porous g-C3N4 nanotube composite photocatalyst, thus completing the preparation method.

[0044] In step 1 of this embodiment, urea and m-aminophenylboric acid are fully ground before being loaded into the crucible, wherein fully ground means that the two are mixed and ground in an agate mortar for 20 to 30 minutes.

[0045] The B-doped porous g-C3N4 nanotubes prepared in step 1 of this embodiment are yellow powder.

[0046] The NiSnO3 nanoparticles prepared in step 2 of this embodiment are green powder.

[0047] The NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst prepared in this embodiment is applied to visible light photocatalytic decomposition of water to produce hydrogen.

[0048] Specific embodiment 2: This embodiment is different from specific embodiment 1 in that the amount of urea in step 1 is 10 g, and the amount of m-aminophenylboronic acid is 2.5 mg to 25 mg. Other steps and parameters are the same as those in specific embodiment 1.

[0049] Specific implementation method three: This implementation method is different from specific implementation method one in that the heating rate in step one is 1-5°C / min. Other steps and parameters are the same as those in specific implementation method one.

[0050] Specific embodiment 4: This embodiment is different from specific embodiment 1 in that the calcination temperature in step 1 is 400-600° C. and the calcination time is 2-4 hours. The other steps and parameters are the same as those in specific embodiment 1.

[0051] Specific embodiment 5: This embodiment is different from specific embodiment 1 in that the NiCl3·6H2O and K2SnO3·3H2O in step 2 are dissolved in distilled water respectively: 1 mmol of NiCl3·6H2O and 1 mmol of K2SnO3·3H2O are dissolved in 10 mL of distilled water respectively. The other steps and parameters are the same as those in specific embodiment 1.

[0052] Specific embodiment 6: This embodiment is different from specific embodiment 1 in that the hydrothermal reaction in step 2 is carried out at 150-200° C. for 18-24 hours. The other steps and parameters are the same as those in specific embodiment 1.

[0053] Specific embodiment 7: This embodiment is different from the specific embodiment 1 in that the cleaning, centrifugation and drying in step 2 are: washing with distilled water and anhydrous ethanol three times respectively, then centrifuging at 8000r / min for 5min, and then vacuum drying at 60°C for 6-10h. The other steps and parameters are the same as those in the specific embodiment 1.

[0054] Specific embodiment 8: This embodiment is different from specific embodiment 1 in that the calcination temperature in step 2 is 300-350° C. and the calcination time is 2-6 hours. Other steps and parameters are the same as those in specific embodiment 1.

[0055] Specific embodiment 9: This embodiment is different from specific embodiment 1 in that in step 3, 0.1 g of B-doped porous g-C3N4 nanotubes are ultrasonically dispersed in 15 mL of N,N-dimethylformamide to obtain solution A, and 5 mg to 15 mg of NiSnO3 nanoparticles are ultrasonically dispersed in 15 mL of n-hexane to obtain solution B. The other steps and parameters are the same as those in specific embodiment 1.

[0056] Specific embodiment 10: This embodiment is different from specific embodiment 1 in that the ultrasonic dispersion time in step 3 is 30 minutes. The other steps and parameters are the same as those in specific embodiment 1.

[0057] Specific implementation eleven: This implementation differs from specific implementation one in that the washing in step three is: washing with anhydrous ethanol for 2 to 3 times; the dispersion is: magnetic stirring for 10 hours. The other steps and parameters are the same as those in specific implementation one.

[0058] Specific embodiment 12: This embodiment differs from specific embodiment 1 in that the washing and drying in step 3 are: washing with anhydrous ethanol for 2 to 3 times, and then drying at 60° C. for 12 to 16 hours. The other steps and parameters are the same as those in specific embodiment 1.

[0059] Specific implementation 13: This implementation is different from specific implementation 1 in that the centrifugation in step 3 is performed at a speed of 8000-10000 r / min for 3-5 min. The other steps and parameters are the same as those in specific implementation 1.

[0060] The beneficial effects of the present invention are verified by the following examples:

[0061] Unless otherwise specified, the reagents, instruments and equipment used in the present invention are conventional reagents, instruments and equipment in the art.

[0062] In this embodiment, the performance test of photocatalytic water decomposition to produce hydrogen is carried out by using a CEL-SPH2N device of Beijing Zhongjiao Jinyuan Company to precipitate hydrogen, and the precipitated hydrogen is analyzed by a GC-7920 gas chromatograph. The experimental device for photocatalytic water decomposition to produce hydrogen includes: carrier gas (argon), propulsion gas (high-purity air), cooling water circulation pump, quartz reactor, magnetic stirrer, 300W xenon lamp (PLS-SXE300 model, Beijing Bofeilai) equipped with UVCUT 420nm filter, and data workstation.

[0063] Embodiment 1:

[0064] A method for preparing NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst, which is carried out according to the following steps:

[0065] 1. Preparation of B-doped porous g-C3N4 nanotubes:

[0066] Urea and m-aminophenylboronic acid are placed in a crucible, and then heated in an oven until they are melted. After melting, they are taken out and naturally cooled to room temperature, and then placed in a muffle furnace for calcination. After the calcination is completed, they are cooled to room temperature to obtain B-doped porous g-C3N4 nanotubes (referred to as BCNT).

[0067] 2. Preparation of NiSnO3 nanoparticles:

[0068] NiCl3·6H2O and K2SnO3·3H2O were dissolved in distilled water respectively, and then mixed and stirred for 30 minutes, and then transferred to a high-pressure reactor and hydrothermally reacted in an oven. The obtained solid was washed, centrifuged and dried, and then calcined in a muffle furnace to obtain NiSnO3 nanoparticles (denoted as NSO);

[0069] 3. Preparation of NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst:

[0070] The B-doped porous g-C3N4 nanotubes were ultrasonically dispersed in N,N-dimethylformamide to obtain solution A, and the NiSnO3 nanoparticles were ultrasonically dispersed in n-hexane to obtain solution B;

[0071] The above solution A and solution B are mixed and 10 mL of anhydrous ethanol is added. After ultrasonic dispersion for 1 hour, the product is collected by centrifugation, washed and then dispersed in anhydrous ethanol. Finally, the target product is collected by centrifugation, washed and dried to obtain NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst (denoted as NSO / BCNT), thus completing the preparation method.

[0072] In step 1 of this embodiment, the amount of urea is 10 g, and the amount of m-aminophenylboronic acid is 15 mg.

[0073] The heating rate in step 1 of this embodiment is 2°C / min.

[0074] The calcination temperature in step 1 of this embodiment is 500° C. and the calcination time is 2 h.

[0075] In step 2 of this embodiment, NiCl3·6H2O and K2SnO3·3H2O are dissolved in distilled water respectively: 1 mmol of NiCl3·6H2O and 1 mmol of K2SnO3·3H2O are dissolved in 10 mL of distilled water respectively.

[0076] The hydrothermal reaction in step 2 of this embodiment: the hydrothermal reaction was carried out at 180° C. for 20 h.

[0077] The cleaning, centrifugation and drying in step 2 of this embodiment are as follows: washing with distilled water and anhydrous ethanol three times each, then centrifuging at 8000 r / min for 5 minutes, and then vacuum drying at 60° C. for 6 hours.

[0078] The calcination temperature in step 2 of this embodiment is 300° C. and the calcination time is 4 hours.

[0079] In step three of this embodiment, 0.1 g of B-doped porous g-C3N4 nanotubes are ultrasonically dispersed in 15 mL of N,N-dimethylformamide to obtain solution A, and 15 mg of NiSnO3 nanoparticles are ultrasonically dispersed in 15 mL of n-hexane to obtain solution B.

[0080] The ultrasonic dispersion time in step 3 of this embodiment is 30 minutes.

[0081] The washing in step 3 of this embodiment is: washing with anhydrous ethanol for 3 times; the dispersion is: magnetic stirring for 10 hours.

[0082] Washing and drying in step 3 of this embodiment: wash with anhydrous ethanol three times, and then dry at 60° C. for 16 hours.

[0083] The centrifugation in step 3 of this embodiment is performed at a speed of 8000 r / min for 5 min.

[0084] The B-doped porous g-C3N4 nanotubes prepared in this example have the following morphology: Figure 1 c and Figure 2 As shown in a. Figure 1 f, proving that element B has been successfully doped into carbon nitride.

[0085] The NiSnO3 nanoparticles prepared in this example have a morphology as shown in FIG. Figure 2 As shown in b.

[0086] The NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst prepared in this example is Figure 2 c and 2d.

[0087] 0.01 g of NiSnO3 modified B doped porous g-C3N4 nanotube composite photocatalyst prepared in this example was placed in a quartz reactor, and 50 mL (10 vol%) of triethanolamine solution and magnet were added. After the reactor was connected to the hydrogen production device, the air in the reactor was removed by a vacuum pump, and a xenon lamp was used to irradiate from above the reactor. The generated hydrogen was pushed into the gas chromatograph with high-purity air, and analyzed by a TCD detector. Finally, the average hydrogen production rate was calculated based on the amount of hydrogen generated in the 2 h reaction.

[0088] Example 2: This embodiment differs from Example 1 in that the amount of m-aminophenylboronic acid used is 2.5 mg. Other aspects are the same as Example 1.

[0089] When the dosage of m-aminophenylboric acid is 2.5 mg, the microscopic morphology of boron-doped carbon nitride is flaky.

[0090] Example 3: This embodiment differs from Example 1 in that the amount of m-aminophenylboronic acid used is 5 mg. Other aspects are the same as Example 1.

[0091] like Figure 1 As shown in a, when the dosage of m-aminophenylboric acid is 5 mg, the microscopic morphology of boron-doped carbon nitride begins to transform from flake to tubular.

[0092] Example 4: This embodiment differs from Example 1 in that the amount of m-aminophenylboronic acid used is 10 mg. Other aspects are the same as Example 1.

[0093] like Figure 1 As shown in b, when the dosage of m-aminophenylboric acid is 10 mg, the microscopic morphology of boron-doped carbon nitride is a hollow tube.

[0094] Example 5: This embodiment differs from Example 1 in that the amount of m-aminophenylboronic acid used is 20-25 mg. Other aspects are the same as Example 1.

[0095] like Figure 1 As shown in Figures 1d and 1e, when the amount of m-aminophenylboronic acid exceeded 15 mg, the hollow tubular structure began to collapse and a large number of holes appeared on the surface.

[0096] Example 6: This embodiment differs from Example 1 in that the amount of NiSnO3 used is 5 to 15 mg. The rest is the same as Example 1.

[0097] The visible light photocatalytic decomposition of water to produce hydrogen is Figure 3 shown.

[0098] Comparative Example 1: Prepare flake carbon nitride using urea as raw material. First, weigh 10g of urea, grind it thoroughly and place it in a crucible. Place the crucible in an oven at 150°C and heat it until it melts. After melting, take it out and cool it naturally to room temperature. Put the obtained sample into a muffle furnace at a heating rate of 2°C / min until it reaches 500°C. Calcined at 500°C for 2h, take it out after cooling to room temperature, and mark the obtained light yellow powder as CNS. Its visible light photocatalytic decomposition of water to produce hydrogen rate is as follows: Figure 3 As shown in Figure 2, its photocatalytic activity is only 237.64 μmol·g -1 ·h -1 .

[0099] In Example 1, the optimal amount of NiSnO3 in the NiSnO3-modified B-doped porous g-C3N4 nanotube composite photocatalyst is 10% (corresponding to 10 mg), and its photocatalytic activity is 5632.57 μmol·g -1 ·h -1 , which is 2.7 times that of B-doped porous g-C3N4 nanotubes.

[0100] Although the present invention has been described above in conjunction with the accompanying drawings, the present invention is not limited to the above-mentioned specific embodiments, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can make many modifications without departing from the purpose of the present invention, all of which are within the protection of the present invention.

Claims

1. A method for preparing NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst, characterized in that It proceeds as follows:

1. Preparation of B-doped porous g-C3N4 nanotubes: Urea and m-aminophenylboronic acid are placed in a crucible, and then heated in an oven until they are melted. After melting, the crucible is taken out and naturally cooled to room temperature, and then placed in a muffle furnace for calcination. After the calcination is completed, the crucible is cooled to room temperature to obtain B-doped porous g-C3N4 nanotubes.

2. Preparation of NiSnO3 nanoparticles: NiCl3·6H2O and K2SnO3·3H2O were dissolved in distilled water respectively, then mixed and stirred for 30 minutes, and then transferred to a high-pressure reactor and subjected to hydrothermal reaction in an oven. The obtained solid was washed, centrifuged, dried, and then calcined in a muffle furnace to obtain NiSnO3 nanoparticles.

3. Preparation of NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst: The B-doped porous g-C3N4 nanotubes were ultrasonically dispersed in N,N-dimethylformamide to obtain solution A, and the NiSnO3 nanoparticles were ultrasonically dispersed in n-hexane to obtain solution B; The above solution A and solution B are mixed and 10 mL of anhydrous ethanol is added, and the product is collected by centrifugation after ultrasonic dispersion for 1 hour, and then dispersed in anhydrous ethanol after washing, and finally the target product is collected by centrifugation, washed and dried to obtain NiSnO3 modified B doped porous g-C3N4 nanotube composite photocatalyst, thus completing the preparation method; The amount of urea in step 1 is 10 g, and the amount of m-aminophenylboronic acid is 2.5 mg to 25 mg; In step 2, NiCl3·6H2O and K2SnO3·3H2O are dissolved in distilled water respectively: 1 mmol of NiCl3·6H2O and 1 mmol of K2SnO3·3H2O are dissolved in 10 mL of distilled water respectively.

2. The method for preparing a NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst according to claim 1, characterized in that The heating rate in step 1 is 1-5°C / min.

3. The method for preparing a NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst according to claim 1, characterized in that The calcination temperature in step 1 is 400-600° C., and the calcination time is 2-4 hours.

4. The method for preparing a NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst according to claim 1, characterized in that The hydrothermal reaction in step 2: hydrothermal reaction at 150-200° C. for 18-24 hours.

5. The method for preparing a NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst according to claim 1, characterized in that The cleaning, centrifugation and drying in step 2 are as follows: washing with distilled water and anhydrous ethanol for 3 times respectively, then centrifuging at 8000r / min for 5 minutes, and then vacuum drying at 60°C for 6 to 10 hours.

6. The method for preparing a NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst according to claim 1, characterized in that The calcination temperature in step 2 is 300-350° C., and the calcination time is 2-6 hours.

7. The method for preparing a NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst according to claim 1, characterized in that In step 3, 0.1 g of B-doped porous g-C3N4 nanotubes were ultrasonically dispersed in 15 mL of N,N-dimethylformamide to obtain solution A, and 5 mg to 15 mg of NiSnO3 nanoparticles were ultrasonically dispersed in 15 mL of n-hexane to obtain solution B.

8. The method for preparing a NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst according to claim 1, characterized in that The ultrasonic dispersion time in step 3 is 30 minutes.

9. The method for preparing a NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst according to claim 1, characterized in that The washing in step 3: washing with anhydrous ethanol for 2 to 3 times; the dispersion: magnetic stirring for 10 hours.

10. The method for preparing a NiSnO3 modified B-doped porous g-C3N4 nanotube composite photocatalyst according to claim 1, characterized in that Washing and drying in step 3: wash with anhydrous ethanol 2 to 3 times, and then dry at 60° C. for 12 to 16 hours.

Citation Information

Patent Citations

  • Similar tubular borax-doped graphite phase carbon nitride nanometer material and preparation method thereof

    CN106732736A

  • B,S-codoped carbon nitride nanotube photocatalyst and preparing method and applications thereof

    CN109772409A

  • Gas sensor for detecting sulfur hexafluoride decomposition products and preparation method thereof

    CN113155913A

  • Boron-doped graphite phase carbon nitride as well as preparation method and application thereof

    CN116571265A

  • The nose wheel device for aircraft that allows free rotation while towing the aircraft

    KR1020230139030A