Cation resin regeneration process of nuclear power plant secondary circuit condensate polishing system
By adopting conventional acid liquid regeneration, ammonia water saturation treatment and double acid liquid regeneration steps in the condensate polishing treatment system of the nuclear power plant, the regeneration degree of the cation resin is improved, and the problem of insufficient regeneration degree of the cation resin in the existing technology is solved. It achieves efficient sodium ion removal and meets the index requirements of the World Association of Nuclear Power Operators.
Patent Information
- Application Number
- CN202310341286.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-15
AI Technical Summary
The existing acid regeneration process cannot meet the requirement of 99.4% regeneration of the cation resin in the condensate polishing system of the nuclear power plant, resulting in the sodium ion concentration at the mixed bed outlet exceeding the standard and failing to meet the excellent index requirements organized by the World Association of Nuclear Power Operators.
A cation resin regeneration process of a nuclear power plant condensate polishing system is adopted, including conventional acid regeneration, ammonia water saturation treatment and double acid solution regeneration. Through these steps, the regeneration degree of the cation resin is improved to not less than 95%, sodium The resin concentration is less than 0.3%.
It achieves efficient regeneration of cation resin, meets the excellent index requirements of the World Association of Nuclear Power Operators for sodium ion content in steam generator discharge water, and reduces the sodium ion content at the outlet of the mixed bed to less than 0.008ppb.
Smart Images

Figure CN118767997A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resin regeneration in a secondary loop condensate polishing system of a nuclear power plant, in particular to a cation resin regeneration process in a secondary loop condensate polishing system of a nuclear power plant. Background Art
[0002] During the operation of a nuclear power plant, the water quality inside the steam generator is controlled by feed water purification and continuous sewage discharge to prevent corrosion and impurity deposition in the steam generator. The sewage flow rate is 1% of the feed water flow rate, which means that the concentration multiple of the water in the steam generator is 100.
[0003] The water quality control of the secondary circuit of a nuclear power plant is very important for maintaining the good condition of the steam generator. It is mainly controlled by adding ammonia and ammonia water to adjust the pH to control corrosion, and the impurity ions are removed through the condensate polishing system. At the same time, the steam generator adopts continuous blowdown to control the concentration multiple to ensure the good water quality in the steam generator.
[0004] At present, the condensate polishing system generally consists of a pre-cation bed, a mixed bed, a clean condensate pump and a regeneration system, which is used to remove Na in the water at the initial start-up of the unit and when the condenser titanium tube is broken. + , Cl - and SO4 2- The condensate polishing system will run continuously from the start-up to full power of the unit to ensure that the water quality in the steam generator meets the standard. After the unit is at full power and the water quality in the steam generator meets the standard, the condensate polishing system will be shut down and put into standby mode.
[0005] According to the requirements of the World Association of Nuclear Operators, the excellent indicator of sodium ion content in steam generator wastewater is 0.8ppb. Under the full flow condition of the condensate polishing system, the sodium ion content at the outlet of the mixed bed must be less than 0.008ppb to ensure that the sodium ion concentration of the steam generator wastewater does not exceed 0.8ppb. This requires the regeneration degree of the mixed bed cation resin to reach 99.4%, that is, the proportion of sodium type resin should not exceed 0.6%, which is much higher than the requirements of general industrial facilities.
[0006] In the condensate polishing system, the cation bed will leak sodium first when it is close to failure. Therefore, when the cation bed fails, the cation resin of the mixed bed will gradually turn into sodium type resin until it fails. When the mixed bed resin fails, the failed mixed bed resin is hydraulically transported to the separation tower, and the spare resin in the resin storage tower is transported to the mixed bed for standby. After the failed mixed bed resin is air scrubbed, backwashed, layered and left to stand in the separation tower, the anion resin is transferred to the anion resin regeneration tower for regeneration, and the cation resin is transferred to the cation resin regeneration tower for regeneration. The cation resin is regenerated with acid for standby, and the anion resin is regenerated with alkali for standby. Then the cation resin and anion resin are transferred to the resin storage tower for mixing and forward washing for standby.
[0007] However, the conventional acid regeneration process is difficult to meet the requirement of 99.4% regeneration of cationic resin, that is, the proportion of sodium type resin is no more than 0.6%. Therefore, a more effective regeneration method is needed to ensure that the sodium ion concentration at the outlet of the mixed bed is less than 0.008ppb, so as to meet the regeneration degree requirement of the desalting bed under the unit operation condition.
[0008] The existing thermal power plant condensate polishing system uses ammonia operation to extend the operation time of the condensate polishing system and reduce the number of regeneration times, but this method is not suitable for nuclear power plants. Since the selectivity of ammonium is stronger than that of sodium, the mixed bed is prone to sodium leakage during ammonia operation, losing the absorption function of sodium ions, resulting in excessive sodium content in the water of the steam generator, affecting the safe and reliable operation of the steam generator. Summary of the invention
[0009] Based on this, the present invention aims at the problem that after the failure of the cation resin in the cation bed and the mixed bed of the condensate polishing system of the nuclear power plant, the existing acid regeneration process is difficult to meet the requirement that the regeneration degree of the cation resin is not less than 99.4%, that is, the proportion of the sodium type resin shall not be greater than 0.6%, so that when the cation bed / mixed bed after regeneration is put into full flow operation, it is impossible to meet the excellent index requirements of the World Association of Nuclear Operators for the sodium ion content of the steam generator discharge water. A cation resin regeneration process for the condensate polishing system of a nuclear power plant is provided. The process makes the cation resin regeneration degree not less than 95%, and the proportion of the sodium type resin concentration in the cation resin is less than 0.3%, so that the cation resin can be put into operation after regeneration and meet the excellent index requirements of the World Association of Nuclear Operators for the sodium ion content of the steam generator discharge water.
[0010] In order to achieve the above object, the present invention provides the following technical solutions:
[0011] A process for regenerating cation resin in a secondary circuit condensate polishing system of a nuclear power plant comprises the following steps: when the cation resin in the secondary circuit condensate polishing system of the nuclear power plant fails, the failed cation resin is firstly regenerated with conventional acid solution, then saturated with ammonia water, and finally regenerated with double amount of acid solution; wherein, regenerating the failed cation resin with conventional acid solution is an optional step, and the amount of acid solution used for regenerating the cation resin with double amount of acid solution is twice the amount of acid solution used for regenerating the cation resin with conventional acid solution.
[0012] Working principle: The failed cation resin is first regenerated with acid solution, and the cation resin undergoes the following ion exchange reaction:
[0013] R-Na + +H + →RH + +Na + ;
[0014] The cation resin after sulfuric acid regeneration is saturated with ammonia water. The selectivity of the cation resin for ammonia ions is greater than that for sodium ions and hydrogen ions. The cation resin undergoes the following ion exchange reaction:
[0015]
[0016]
[0017] The cation resin treated with ammonia water is regenerated with double amount of acid solution, and the cation resin undergoes the following ion exchange reaction:
[0018]
[0019] R-Na + +H + →RH + +Na + .
[0020] In the formula, It is an ammonium type cationic resin, RH + It is a hydrogen type positive resin, R-Na + It is a sodium type cationic resin, Na + is the sodium ion eluted from the failed cation resin, H + It is the hydrogen ion in the acid.
[0021] In one of the embodiments, when the cation resin of the secondary loop condensate polishing system of a nuclear power plant fails, the failed cation resin is first regenerated with conventional acid solution to achieve a regeneration degree of 95%, and the concentration of sodium type cation resin in the cation resin is 5%; then it is saturated with ammonia water; finally, it is regenerated with double the amount of acid solution, and finally the regeneration degree of the cation resin is not less than 95%, and the concentration of sodium type resin in the cation resin is less than 0.3%.
[0022] In one of the embodiments, when the cation resin of the secondary condensate polishing system of a nuclear power plant fails, the failed cation resin is first regenerated with conventional acid solution, then saturated with ammonia water, and finally regenerated with double amount of acid solution; the failure of the cation resin of the secondary condensate polishing system of the nuclear power plant includes two situations: the complete failure of the cation resin of the secondary condensate polishing system of the nuclear power plant and the incomplete failure of the cation resin of the secondary condensate polishing system of the nuclear power plant.
[0023] In one embodiment, when the cation resin of the secondary loop condensate polishing system of a nuclear power plant fails, the failed cation resin is fed with a 5wt% sulfuric acid solution for 1 hour, replaced, and washed with positive wash water to complete the conventional sulfuric acid solution regeneration of the cation resin, so that its regeneration degree reaches 95%, and the concentration of the sodium type cation resin in the cation resin accounts for 5%;
[0024] The regenerated cation resin is circulated with water, and ammonia water of 1.2 times the working exchange capacity of the cation resin is added during the circulation until the concentration of the ammonium type cation resin in the cation resin reaches the peak value. After the ammonia water is added, the circulation is continued for 2 hours, and then washed in series until the conductivity of the effluent is less than 2μs / cm, completing the ammonia saturation treatment of the cation resin;
[0025] After the cation resin has been saturated with ammonia water, it is fed with a 5wt% sulfuric acid solution for 2 hours, replaced and washed with positive washing water until the effluent conductivity is less than 3μs / cm, and then the cation resin is regenerated with double sulfuric acid, so that its regeneration degree is not less than 95%, and the concentration of sodium type resin in the cation resin accounts for less than 0.3%;
[0026] The volume of sulfuric acid solution for conventional sulfuric acid regeneration of cation resin is 8 times the volume of cation resin, and the amount of sulfuric acid for double-volume sulfuric acid regeneration of cation resin is 16 times the volume of cation resin.
[0027] In one of the embodiments, when the cation resin of the secondary loop condensate polishing system of a nuclear power plant has not completely failed, the cation resin that has not completely failed is first saturated with ammonia water and then regenerated with a double amount of acid solution.
[0028] In one of the embodiments, when the cation resin of the secondary circuit condensate polishing system of a nuclear power plant has not completely failed, the cation resin that has not completely failed is first saturated with ammonia water and then regenerated with double the amount of acid solution, so that the regeneration degree of the cation resin is finally not less than 95%, and the concentration of the sodium type resin in the cation resin is less than 0.3%.
[0029] In one embodiment, when the cation resin of the secondary loop condensate polishing system of the nuclear power plant has not failed, the cation resin that has not failed is circulated with water, and ammonia water of 1.2 times the working exchange capacity of the cation resin is added during the circulation until the concentration ratio of the ammonium type cation resin in the cation resin reaches a peak value, and the circulation is continued for 2 hours after the ammonia water is added, and then the cation resin is washed in series until the conductivity of the outlet water is less than 2μs / cm, thereby completing the ammonia water saturation treatment of the cation resin;
[0030] After the cation resin has been saturated with ammonia water, it is fed with a 5wt% sulfuric acid solution for 2 hours, replaced and washed with positive washing water until the effluent conductivity is less than 3μs / cm, and then the cation resin is regenerated with double sulfuric acid, so that its regeneration degree is not less than 95%, and the concentration of sodium type resin in the cation resin accounts for less than 0.3%;
[0031] The amount of sulfuric acid used for regeneration of the cation resin is 16 times the volume of the cation resin.
[0032] Preferably, the acid solution is a 5 wt % sulfuric acid solution.
[0033] Furthermore, the cationic resin of the secondary circuit condensate polishing system of a nuclear power plant is a mixed bed cationic resin of the secondary circuit condensate polishing system of a nuclear power plant or a cationic bed resin of the secondary circuit condensate polishing system of a nuclear power plant.
[0034] The present invention also provides a mixed bed resin regeneration process for a secondary loop condensate polishing system of a nuclear power plant, comprising the following steps:
[0035] When the mixed bed resin fails, the failed mixed bed resin is scrubbed with air, backwashed, layered and left to stand, and then the anion resin is regenerated and the cation resin is regenerated;
[0036] After the anion resin is qualified after entering the alkali solution, replacement and positive washing, the regeneration of the anion resin is completed;
[0037] The cation resin is regenerated by the cation resin regeneration process of the secondary circuit condensate polishing system of the nuclear power plant;
[0038] The regenerated cation resin and anion resin are mixed by air stirring and positive washing and then put into use after passing the test.
[0039] In one of the embodiments, the mixed bed resin regeneration process of the secondary loop condensate polishing system of the nuclear power plant is carried out in the mixed bed regeneration system of the secondary loop condensate polishing system of the nuclear power plant.
[0040] The present invention also provides a cation bed resin regeneration process for a nuclear power plant secondary loop condensate polishing system, comprising the following steps: when the cation bed resin fails, the failed cation bed resin is regenerated by the cation bed resin regeneration process for a nuclear power plant secondary loop condensate polishing system.
[0041] In one embodiment, the cation bed resin regeneration process of the secondary loop condensate polishing system of the nuclear power plant is carried out in the mixed bed regeneration system of the secondary loop condensate polishing system of the nuclear power plant.
[0042] In one of the embodiments, the cation bed resin regeneration process of the secondary loop condensate polishing system of the nuclear power plant is carried out in the cation bed regeneration system of the secondary loop condensate polishing system of the nuclear power plant.
[0043] The present invention also provides a resin regeneration process for a secondary condensate polishing system of a nuclear power plant, including the mixed bed resin regeneration process for a secondary condensate polishing system of a nuclear power plant and the cation bed resin regeneration process for a secondary condensate polishing system of a nuclear power plant.
[0044] Beneficial technical effects of the present invention:
[0045] The cationic resin regeneration process and resin regeneration process of the nuclear power plant secondary loop condensate polishing system of the present invention regenerate the failed cationic bed resin / mixed bed cation resin after the failed cationic bed resin / mixed bed cation resin is replaced, thereby improving the conversion rate of the nano-type cation resin in the cationic bed resin / mixed bed cation resin; after the failed cationic bed resin is regenerated and put into operation, the sodium content at the outlet of the cationic bed reaches a relatively low level, reducing the impact on the mixed bed, and finally achieving a sodium ion content of less than 0.008 ppb at the outlet of the mixed bed; after the failed mixed bed resin is regenerated and put into operation, the sodium ion content at the outlet of the mixed bed is less than 0.008 ppb. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is a schematic diagram of the structure of the mixed bed regeneration system of the secondary loop condensate polishing system of a nuclear power plant;
[0047] Figure 2 This is a schematic diagram of the structure of the cation bed regeneration system of the secondary circuit condensate polishing system of a nuclear power plant;
[0048] Figure 3 This is a relationship diagram between the regeneration degree of the cation resin and the amount of sulfuric acid solution used. The horizontal axis is the amount of sulfuric acid used, the value is the volume multiple of the cation resin, and the vertical axis is the regeneration degree of the cation resin. DETAILED DESCRIPTION
[0049] The technical solution of the present invention is described clearly and completely below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0050] In the secondary condensate polishing system of a nuclear power plant, the cation resin in the mixed bed is a hydrogen-type cation resin, and the following ion exchange reactions occur:
[0051]
[0052] In the formula, RH + Indicates hydrogen-type positive resin; Na + Represents sodium ion, R-Na + Indicates sodium type cationic resin, H + Represents hydrogen ion.
[0053] When the mixed bed of the secondary loop condensate polishing system of a nuclear power plant is in operation, the cation resin in the mixed bed undergoes a forward ion exchange reaction, and the hydrogen ions in the cation resin undergo an ion exchange reaction with the sodium ions in the steam generator feed water to generate sodium-type cation resin and hydrogen ions, thereby removing the sodium ions in the steam generator feed water.
[0054] When the hydrogen ions in the cation resin are completely exchanged with the sodium ions in the feed water, they can no longer undergo ion exchange reaction with the sodium ions in the feed water. This phenomenon of the cation resin is called "failure."
[0055] When the cation resin in the mixed bed of the secondary condensate polishing system of a nuclear power plant fails, sulfuric acid is added to the mixed bed, and the cation resin in the mixed bed undergoes a reverse ion exchange reaction. The sodium ions in the cation resin undergo an ion exchange reaction with the hydrogen ions in the sulfuric acid to generate hydrogen-type cation resin and sodium ions. This phenomenon of the cation resin is called "regeneration."
[0056] The regeneration degree of the cation resin refers to the concentration ratio of the hydrogen type cation resin in the cation resin after the cation resin is regenerated. The calculation formula is as follows:
[0057]
[0058] In the formula, [RH + ] is the concentration of hydrogen-type cation resin after cation resin regeneration, in mol / L; [R-Na + ] is the concentration of sodium type cation resin after cation resin regeneration, the unit is mol / L.
[0059] The ion exchange reaction of the cationic resin in the mixed bed of the secondary loop condensate polishing system of a nuclear power plant is a reversible reaction. The reaction equilibrium constant K of the reversible reaction is calculated by the following formula:
[0060]
[0061] In the formula, [R-Na + ] is the concentration of sodium cation resin when the reversible reaction is in equilibrium, the unit is mol / L. The concentration of the sodium cation resin can be replaced by the concentration ratio of the sodium cation resin in the cation resin; [RH + ] is the concentration of hydrogen-type cation resin when the reversible reaction is in equilibrium, the unit is mol / L. The concentration of hydrogen-type cation resin can be replaced by the concentration ratio of hydrogen-type cation resin in cation resin; [Na + ] is the concentration of sodium ions when the reversible reaction is in equilibrium, in mol / L; [H + ] is the concentration of hydrogen ions when the reversible reaction is in equilibrium, and the unit is mol / L.
[0062] The reaction equilibrium constant K of this reversible reaction is also called the selectivity constant of the cation resin to sodium ions and hydrogen ions. The cation resin in the mixed bed of the secondary loop condensate polishing system of the nuclear power plant has a greater selectivity to sodium ions than to hydrogen ions.
[0063] When the mixed bed of the secondary condensate polishing system of a nuclear power plant is in operation, the sodium ion concentration at the steam generator outlet is:
[0064]
[0065] In the formula, [R-Na + ] is the concentration of sodium type cation resin, the unit is mol / L, the concentration of sodium type cation resin can be replaced by the concentration ratio of sodium type cation resin in cation resin; [RH + ] is the concentration of hydrogen-type cation resin, in mol / L. The concentration of hydrogen-type cation resin can be replaced by the concentration ratio of hydrogen-type cation resin in cation resin; [Na + ] is the sodium ion concentration at the steam generator outlet, in mol / L; [H + ] is the hydrogen ion concentration, the unit is mol / L; K is the selectivity constant of the cationic resin for sodium ions and hydrogen ions.
[0066] When the mixed bed of the secondary condensate polishing system of a nuclear power plant is in operation, the effluent from the mixed bed is neutral and the concentration of hydrogen ions is a constant value, equal to 10 -7 mol / L; the sodium ion concentration at the steam generator outlet is directly proportional to the proportion of the sodium type cation resin in the cation resin, and inversely proportional to the proportion of the hydrogen type cation resin in the cation resin; when the cation resin in the mixed bed of the secondary loop condensate polishing system of the nuclear power plant fails, the cation resin in the mixed bed is regenerated with sulfuric acid. As the regeneration degree of the cation resin increases, the concentration of the sodium type cation resin continues to decrease, and the concentration of the hydrogen type cation resin continues to increase. The concentration of sodium ions that can be regenerated and replaced in the cation resin is getting smaller and smaller, which is manifested as the regeneration degree of the cation resin increases more and more slowly with the increase in the amount of sulfuric acid used; when the regeneration degree of the cation resin reaches 95%, the effect of increasing the amount of sulfuric acid to increase the regeneration degree of the cation resin is very poor.
[0067] Example 1
[0068] The present embodiment provides a cation resin regeneration process for a secondary loop condensate polishing system of a nuclear power plant, comprising the following steps: when the cation resin of the secondary loop condensate polishing system of a nuclear power plant fails, the failed cation resin is first regenerated with conventional acid solution, then saturated with ammonia water, and finally regenerated with double-volume acid solution; wherein the amount of acid solution used for regenerating the cation resin with double-volume acid solution is twice the amount of acid solution used for regenerating the cation resin with conventional acid solution.
[0069] Working principle: The failed cation resin is regenerated with acid solution, and the failed cation resin undergoes the following ion exchange reaction:
[0070] R-Na + +H + →RH + +Na + ;
[0071] The cation resin after sulfuric acid regeneration is saturated with ammonia water. The selectivity of the cation resin for ammonia ions is greater than that for sodium ions and hydrogen ions. The cation resin undergoes the following ion exchange reaction:
[0072]
[0073]
[0074] The cation resin treated with ammonia water is regenerated with double amount of acid solution, and the cation resin undergoes the following ion exchange reaction:
[0075]
[0076] R-Na + +H + →RH + +Na + .
[0077] In the formula, It is an ammonium type cationic resin, RH + It is a hydrogen type positive resin, R-Na + It is a sodium type cationic resin, Na + is the sodium ion eluted from the failed cation resin, H + It is the hydrogen ion in the acid.
[0078] Further, in this embodiment, the failure of the cation resin in the secondary condensate polishing system of the nuclear power plant is the complete failure of the cation resin in the secondary condensate polishing system of the nuclear power plant or the incomplete failure of the cation resin in the secondary condensate polishing system of the nuclear power plant.
[0079] Furthermore, in this embodiment, when the cation resin of the secondary loop condensate polishing system of the nuclear power plant fails, the failed cation resin is first regenerated with conventional acid solution to achieve a regeneration degree of 95%, and the concentration of sodium type cation resin in the cation resin is 5%; then it is saturated with ammonia water; finally, it is regenerated with double the amount of acid solution, and finally the regeneration degree of the cation resin is not less than 95%, and the concentration of sodium type resin in the cation resin is less than 0.3%.
[0080] Furthermore, in this embodiment, the acid solution is a 5 wt % sulfuric acid solution.
[0081] Further, in this embodiment, when the cation resin of the secondary loop condensate polishing system of the nuclear power plant fails, the failed cation resin is fed with a 5wt% sulfuric acid solution for 1 hour, replaced and washed with positive wash water to complete the conventional sulfuric acid solution regeneration of the cation resin, so that its regeneration degree reaches 95%, and the concentration of the sodium type cation resin in the cation resin accounts for 5%;
[0082] The regenerated cation resin is circulated with water, and ammonia water of 1.2 times the working exchange capacity of the cation resin is added during the circulation until the concentration of the ammonium type cation resin in the cation resin reaches the peak value. After the ammonia water is added, the circulation is continued for 2 hours, and then washed in series until the conductivity of the effluent is less than 2μs / cm, completing the ammonia saturation treatment of the cation resin;
[0083] After the cation resin has been saturated with ammonia water, it is fed with a 5wt% sulfuric acid solution for 2 hours, replaced and washed with positive washing water until the effluent conductivity is less than 3μs / cm, and then the cation resin is regenerated with double sulfuric acid, so that its regeneration degree is not less than 95%, and the concentration of sodium type resin in the cation resin accounts for less than 0.3%;
[0084] The volume of sulfuric acid solution for conventional sulfuric acid regeneration of cation resin is 8 times the volume of cation resin, and the amount of sulfuric acid for double-volume sulfuric acid regeneration of cation resin is 16 times the volume of cation resin.
[0085] Furthermore, in this embodiment, the cation resin of the secondary circuit condensate polishing system of the nuclear power plant is a mixed bed cation resin of the secondary circuit condensate polishing system of the nuclear power plant.
[0086] After the mixed bed resin fails and is replaced, the failed mixed bed cation resin is first regenerated with conventional acid solution to achieve a regeneration degree of 95%, and the concentration of sodium type cation resin in the cation resin is 5%; the cation resin after conventional acid regeneration is saturated with ammonia water. Since the selectivity of cation resin for ammonium ions is greater than that for sodium ions and hydrogen ions, most of the hydrogen type cation resin and sodium type cation resin are converted to ammonium type cation resin; the cation resin after ammonia saturation treatment is regenerated with double acid solution, and most of the sodium type cation resin and ammonium type cation resin are converted to hydrogen type cation resin, and finally the regeneration degree of cation resin is not less than 95%, and the concentration of sodium type resin in the cation resin is less than 0.3%. The ammonia leakage of the ammonium type cation resin with a concentration of less than 5% in the mixed bed cation resin has no adverse effect on the secondary circuit water quality of the nuclear power plant. In actual operation, the conductivity of the mixed bed outlet reaches below 0.06us / cm, indicating that there is no ammonia leakage. The regenerated mixed bed cation resin greatly reduces the concentration of sodium type cation resin in the cation resin.
[0087] Example 2
[0088] The present embodiment provides a process for regenerating the cation resin of the secondary loop condensate polishing system of a nuclear power plant, comprising the following steps: when the cation resin of the secondary loop condensate polishing system of the nuclear power plant has not failed, firstly subjecting the cation resin that has not failed to failure to saturation treatment with ammonia water, and then subjecting it to double-volume acid liquid regeneration; wherein the amount of acid liquid used for regenerating the cation resin with double-volume acid liquid is twice the amount of acid liquid used for regenerating the cation resin with conventional acid liquid.
[0089] Working principle: The cation resin that has not completely failed is saturated with ammonia water. The selectivity of the cation resin for ammonia ions is greater than that for sodium ions and hydrogen ions. The cation resin that has not completely failed undergoes the following ion exchange reaction:
[0090]
[0091]
[0092] The cation resin treated with ammonia water is regenerated with double amount of acid solution, and the cation resin undergoes the following ion exchange reaction:
[0093]
[0094] R-Na + +H + →RH + +Na + .
[0095] In the formula, It is an ammonium type cationic resin, RH + It is a hydrogen type positive resin, R-Na + It is a sodium type cationic resin, Na + is the sodium ion eluted from the failed cation resin, H + It is the hydrogen ion in the acid.
[0096] Furthermore, in this embodiment, when the cation resin of the secondary circuit condensate polishing system of the nuclear power plant has not completely failed, the cation resin that has not completely failed is first subjected to conventional acid regeneration to achieve a regeneration degree of 95%, and the concentration of sodium type cation resin in the cation resin accounts for 5%; then it is subjected to ammonia saturation treatment; finally, it is subjected to double acid regeneration, and finally the regeneration degree of the cation resin is not less than 95%, and the concentration of sodium type resin in the cation resin accounts for less than 0.3%.
[0097] Furthermore, in this embodiment, the acid solution is a 5 wt % sulfuric acid solution.
[0098] Furthermore, in the present embodiment, when the cation resin of the secondary loop condensate polishing system of the nuclear power plant has not completely failed, the cation resin that has not completely failed is subjected to water circulation, and ammonia water of 1.2 times the working exchange capacity of the cation resin is added during the circulation until the concentration ratio of the ammonium type cation resin in the cation resin reaches a peak value. After the ammonia water is added, the circulation is continued for 2 hours, and then the cation resin is washed in series until the effluent conductivity is less than 2μs / cm, thereby completing the ammonia water saturation treatment of the cation resin; the cation resin after the ammonia water saturation treatment is subjected to a 5wt% sulfuric acid solution for 2 hours, displacement and forward washing with forward washing water until the effluent conductivity is less than 3μs / cm, and then the cation resin is regenerated with double sulfuric acid, so that its regeneration degree is not less than 95%, and the concentration ratio of the sodium type resin in the cation resin is less than 0.3%; the amount of sulfuric acid used for the double sulfuric acid regeneration of the cation resin is 16 times the volume of the cation resin.
[0099] Furthermore, in this embodiment, the cation resin of the secondary circuit condensate polishing system of the nuclear power plant is a mixed bed cation resin of the secondary circuit condensate polishing system of the nuclear power plant.
[0100] After the mixed bed resin fails and is replaced, the failed mixed bed cation resin is first regenerated with conventional acid solution to achieve a regeneration degree of 95%, and the concentration of sodium type cation resin in the cation resin is 5%; the cation resin after conventional acid regeneration is saturated with ammonia water. Since the selectivity of cation resin for ammonium ions is greater than that for sodium ions and hydrogen ions, most of the hydrogen type cation resin and sodium type cation resin are converted to ammonium type cation resin; the cation resin after ammonia saturation treatment is regenerated with double acid solution, and most of the sodium type cation resin and ammonium type cation resin are converted to hydrogen type cation resin, and finally the regeneration degree of cation resin is not less than 95%, and the concentration of sodium type resin in the cation resin is less than 0.3%. The ammonia leakage of the ammonium type cation resin with a concentration of less than 5% in the mixed bed cation resin has no adverse effect on the secondary circuit water quality of the nuclear power plant. In actual operation, the conductivity of the mixed bed outlet reaches below 0.06us / cm, indicating that there is no ammonia leakage. The regenerated mixed bed cation resin greatly reduces the concentration of sodium type cation resin in the cation resin.
[0101] Example 3
[0102] The rest is the same as Example 1, except that the cationic resin of the secondary circuit condensate polishing system of the nuclear power plant in this example is the cationic bed resin of the secondary circuit condensate polishing system of the nuclear power plant.
[0103] After the cation bed resin fails and is replaced, the failed cation bed resin is first regenerated with conventional acid solution to reach a regeneration degree of 95%, and the concentration of sodium type cation resin in the cation resin is 5%; the cation resin after conventional acid solution regeneration is saturated with ammonia water. Since the selectivity of cation resin for ammonium ions is greater than that for sodium ions and hydrogen ions, most of the hydrogen type cation resin and sodium type cation resin are converted to ammonium type cation resin; the cation resin after ammonia solution saturation treatment is regenerated with double amount of acid solution, and most of the sodium type cation resin and ammonium type cation resin are converted to hydrogen type cation resin, and finally the regeneration degree of cation resin is not less than 95%, and the concentration of sodium type resin in the cation resin is less than 0.3%. The ammonia leakage of the ammonium type cation resin with a concentration of less than 5% in the cation bed resin has no adverse effect on the secondary circuit water quality of the nuclear power plant. In actual operation, the conductivity at the outlet of the mixed bed reaches below 0.06us / cm, indicating that there is no ammonia leakage. The regenerated cation bed resin greatly reduces the concentration of sodium-type cation resin in the cation resin, so that the sodium content at the cation bed outlet reaches a relatively low level after the cation bed is put into operation, reducing the impact on the mixed bed.
[0104] Example 4
[0105] The rest is the same as Example 2, except that the cationic resin of the secondary loop condensate polishing system of the nuclear power plant in this example is the cationic bed resin of the secondary loop condensate polishing system of the nuclear power plant.
[0106] After the cation bed resin fails and is replaced, the failed cation bed resin is first regenerated with conventional acid solution to reach a regeneration degree of 95%, and the concentration of sodium type cation resin in the cation resin is 5%; the cation resin after conventional acid solution regeneration is saturated with ammonia water. Since the selectivity of cation resin for ammonium ions is greater than that for sodium ions and hydrogen ions, most of the hydrogen type cation resin and sodium type cation resin are converted to ammonium type cation resin; the cation resin after ammonia solution saturation treatment is regenerated with double amount of acid solution, and most of the sodium type cation resin and ammonium type cation resin are converted to hydrogen type cation resin, and finally the regeneration degree of cation resin is not less than 95%, and the concentration of sodium type resin in the cation resin is less than 0.3%. The ammonia leakage of the ammonium type cation resin with a concentration of less than 5% in the cation bed resin has no adverse effect on the secondary circuit water quality of the nuclear power plant. In actual operation, the conductivity at the outlet of the mixed bed reaches below 0.06us / cm, indicating that there is no ammonia leakage. The regenerated cation bed resin greatly reduces the concentration of sodium-type cation resin in the cation resin, so that the sodium content at the cation bed outlet reaches a relatively low level after the cation bed is put into operation, reducing the impact on the mixed bed.
[0107] Example 5
[0108] This embodiment provides a mixed bed resin regeneration process for a secondary loop condensate polishing system of a nuclear power plant, comprising the following steps:
[0109] When the mixed bed resin fails, the failed mixed bed resin is scrubbed with air, backwashed, layered and left to stand, and then the anion resin is regenerated and the cation resin is regenerated;
[0110] After the anion resin is qualified after entering the alkali solution, replacement and positive washing, the regeneration of the anion resin is completed;
[0111] The cation resin is regenerated by the cation resin regeneration process of the nuclear power plant secondary loop condensate polishing system of Example 1;
[0112] The regenerated cation resin and anion resin are mixed by air stirring and positive washing and then put into use after passing the test.
[0113] Further, in this embodiment, the mixed bed resin regeneration process of the secondary loop condensate polishing system of the nuclear power plant is carried out in the mixed bed regeneration system of the secondary loop condensate polishing system of the nuclear power plant, and comprises the following steps:
[0114] When the mixed bed resin fails, the failed mixed bed resin is sent to the separation tower through the resin inlet, and the spare mixed bed resin in the resin storage tower is sent to the mixed bed through the resin outlet for operation;
[0115] The failed mixed bed resin is scrubbed with air at the forward wash water inlet, backwashed and layered with backwash water at the backwash water inlet, and left to stand in the separation tower. The anion resin is transferred to the anion resin regeneration tower for regeneration, and the cation resin is transferred to the cation resin regeneration tower for regeneration.
[0116] The anion resin is regenerated in the anion resin regeneration tower after the anion resin is replaced by alkali solution at the alkali solution inlet and washed by positive washing water at the positive washing water inlet. The regenerated anion resin is transferred to the resin storage tower, and the generated wastewater is discharged through the wastewater outlet.
[0117] The cation resin is fed with a 5wt% sulfuric acid solution for 1 hour at the acid inlet in the cation resin regeneration tower, and then replaced and washed with positive washing water at the positive washing water inlet, and then the conventional sulfuric acid solution regeneration of the cation resin is completed, so that the regeneration degree reaches 95%, and the concentration of the sodium type cation resin in the cation resin accounts for 5%; the regenerated cation resin is left in the cation resin regeneration tower for ammonia saturation treatment, and the generated wastewater is discharged through the wastewater outlet;
[0118] The cation resin is circulated with water in the cation resin regeneration tower and the resin storage tower. During the circulation, ammonia water of 1.2 times the working exchange capacity of the cation resin is added to the cation resin regeneration tower until the concentration of the ammonium type cation resin in the cation resin reaches a peak value. After the ammonia water is added, the circulation is continued for 2 hours, and then the resin storage tower and the cation regeneration tower are washed in series to complete the ammonia saturation treatment of the cation resin.
[0119] When the conductivity of the water out of the resin storage tower is less than 2μs / cm, the cation resin washing is completed; after the cation resin washing is completed, the cation resin in the cation resin regeneration tower is regenerated by double sulfuric acid solution; the cation resin in the cation resin regeneration tower is fed with 5wt% sulfuric acid solution for 2 hours through the acid inlet, and the positive washing water inlet is replaced and washed with positive washing water until the conductivity of the water out of the cation resin regeneration tower is less than 3μs / cm, and then the double sulfuric acid solution regeneration of the cation resin is completed; the cation resin regenerated with double sulfuric acid solution is transferred to the resin storage tower, and the generated wastewater is discharged through the wastewater outlet;
[0120] The cation resin and anion resin in the resin storage tower are mixed by air stirring and forwardly washed with forward washing water at the forward washing water inlet until the conductivity of the water out of the resin storage tower is less than 1μs / cm and then put into use;
[0121] The volume of sulfuric acid solution for conventional sulfuric acid regeneration of cation resin is 8 times the volume of cation resin, and the amount of sulfuric acid for double-volume sulfuric acid regeneration of cation resin is 16 times the volume of cation resin.
[0122] Furthermore, in the present embodiment, the mixed bed resin regeneration system of the secondary circuit condensate polishing system of the nuclear power plant comprises a separation tower, a cation resin regeneration tower, an anion resin regeneration tower and a resin storage tower, wherein spare resin is stored in the resin storage tower; the separation tower is provided with a forward wash water inlet, a resin inlet and a backwash water inlet, a cation resin outlet and an anion resin outlet; the cation resin regeneration tower is provided with a cation resin inlet, a forward wash water inlet, an acid inlet, a cation resin outlet and a wastewater outlet; the anion resin regeneration tower is provided with an anion resin inlet, a forward wash water inlet, an alkali inlet, an anion resin outlet and a wastewater outlet; the resin storage tower is provided with a forward wash water inlet, a resin outlet and a wastewater outlet; the cation resin outlet of the separation tower is connected with the cation resin inlet pipeline of the cation resin regeneration tower, and the anion resin outlet of the separation tower is connected with the anion resin inlet pipeline of the anion resin regeneration tower; the resin outlet of the resin storage tower is respectively connected with the mixed bed and cation bed pipelines.
[0123] The regenerated mixed bed resin was put into full flow operation. During the operation of the mixed bed, the sodium ion content in the steam generator wastewater no longer increased and was slightly reduced. After the mixed bed was put into operation, the sodium ion content at the mixed bed outlet was less than 0.008ppb, and the sodium ion concentration of the steam generator wastewater was maintained at 0.45ppb, achieving the expected target.
[0124] Example 6
[0125] This embodiment provides a mixed bed resin regeneration process for a secondary loop condensate polishing system of a nuclear power plant, comprising the following steps:
[0126] When the mixed bed resin fails, the failed mixed bed resin is scrubbed with air, backwashed, layered and left to stand, and then the anion resin is regenerated and the cation resin is regenerated;
[0127] After the anion resin is qualified after entering the alkali solution, replacement and positive washing, the regeneration of the anion resin is completed;
[0128] The cation resin is regenerated by the cation resin regeneration process of the nuclear power plant secondary loop condensate polishing system of Example 2;
[0129] The regenerated cation resin and anion resin are mixed by air stirring and positive washing and then put into use after passing the test.
[0130] Further, in this embodiment, the mixed bed resin regeneration process of the secondary loop condensate polishing system of the nuclear power plant is carried out in the mixed bed regeneration system of the secondary loop condensate polishing system of the nuclear power plant, and comprises the following steps:
[0131] When the mixed bed resin fails, the failed mixed bed resin is sent to the separation tower through the resin inlet, and the spare mixed bed resin in the resin storage tower is sent to the mixed bed through the resin outlet for operation;
[0132] The failed mixed bed resin is scrubbed with air at the forward wash water inlet, backwashed and layered with backwash water at the backwash water inlet, and left to stand in the separation tower. The anion resin is transferred to the anion resin regeneration tower for regeneration, and the cation resin is transferred to the cation resin regeneration tower for regeneration.
[0133] The anion resin is regenerated in the anion resin regeneration tower after the anion resin is replaced by alkali solution at the alkali solution inlet and washed by positive washing water at the positive washing water inlet. The regenerated anion resin is transferred to the resin storage tower, and the generated wastewater is discharged through the wastewater outlet.
[0134] The cation resin is saturated with ammonia water in the cation resin regeneration tower, and the generated wastewater is discharged through the wastewater outlet;
[0135] The cation resin is circulated with water in the cation resin regeneration tower and the resin storage tower. During the circulation, ammonia water of 1.2 times the working exchange capacity of the cation resin is added to the cation resin regeneration tower until the concentration of the ammonium type cation resin in the cation resin reaches a peak value. After the ammonia water is added, the circulation is continued for 2 hours, and then the resin storage tower and the cation regeneration tower are washed in series to complete the ammonia saturation treatment of the cation resin.
[0136] When the conductivity of the water out of the resin storage tower is less than 2μs / cm, the cation resin washing is completed; after the cation resin washing is completed, the cation resin in the cation resin regeneration tower is regenerated by double sulfuric acid solution; the cation resin in the cation resin regeneration tower is fed with 5wt% sulfuric acid solution for 2 hours through the acid inlet, and the positive washing water inlet is replaced and washed with positive washing water until the conductivity of the water out of the cation resin regeneration tower is less than 3μs / cm, and then the double sulfuric acid solution regeneration of the cation resin is completed; the cation resin regenerated with double sulfuric acid solution is transferred to the resin storage tower, and the generated wastewater is discharged through the wastewater outlet;
[0137] The cation resin and anion resin in the resin storage tower are mixed by air stirring and forwardly washed with forward washing water at the forward washing water inlet until the conductivity of the water out of the resin storage tower is less than 1μs / cm and then put into use;
[0138] The amount of sulfuric acid used for regeneration of the cation resin is 16 times the volume of the cation resin.
[0139] The regenerated mixed bed resin was put into full flow operation. During the operation of the mixed bed, the sodium ion content in the steam generator wastewater no longer increased and was slightly reduced. After the mixed bed was put into operation, the sodium ion content at the mixed bed outlet was less than 0.008ppb, and the sodium ion concentration of the steam generator wastewater was maintained at 0.45ppb, achieving the expected target.
[0140] Example 7
[0141] This embodiment provides a cation bed resin regeneration process for a secondary loop condensate polishing system of a nuclear power plant, comprising the following steps:
[0142] When the cation bed resin fails, the failed cation bed resin is regenerated by the cation resin regeneration process of the nuclear power plant secondary loop condensate polishing system of Example 3.
[0143] Further, in this embodiment, the cation bed resin regeneration process of the secondary circuit condensate polishing system of the nuclear power plant is carried out in the mixed bed regeneration system of the secondary circuit condensate polishing system of the nuclear power plant, and comprises the following steps:
[0144] When the cation bed resin fails, the failed cation bed resin is sent to the separation tower through the resin inlet, and the spare cation bed resin in the resin storage tower is sent to the cation bed through the resin outlet for operation;
[0145] The failed cation bed resin is transferred to the cation resin regeneration tower through the separation tower for regeneration;
[0146] The cation bed resin in the cation resin regeneration tower is fed with a 5wt% sulfuric acid solution for 1 hour, and then replaced and washed with positive washing water at the positive washing water inlet, and then the conventional sulfuric acid solution regeneration of the cation bed resin is completed, so that its regeneration degree reaches 95%, and the concentration of sodium type cation resin in the cation bed resin accounts for 5%; the regenerated cation bed resin is left in the cation resin regeneration tower for ammonia saturation treatment, and the generated wastewater is discharged through the wastewater outlet;
[0147] The cation bed resin is circulated with water in the cation resin regeneration tower and the resin storage tower. During the circulation, ammonia water of 1.2 times the working exchange capacity of the cation bed resin is added to the cation resin regeneration tower until the concentration of the ammonium type cation resin in the cation bed resin reaches a peak value. After the ammonia water is added, the circulation is continued for 2 hours, and then the resin storage tower and the cation regeneration tower are washed in series to complete the ammonia saturation treatment of the cation bed resin.
[0148] When the conductivity of the water out of the resin storage tower is less than 2μs / cm, the cation bed resin serial washing is completed; after the cation bed resin serial washing is completed, the cation bed resin in the cation resin regeneration tower is regenerated by double sulfuric acid solution; the cation bed resin in the cation resin regeneration tower is fed with 5wt% sulfuric acid solution for 2 hours through the acid inlet, and the positive washing water inlet is replaced and forward washed until the conductivity of the water out of the cation resin regeneration tower is less than 3μs / cm, and then the regeneration of the cation bed resin with double sulfuric acid solution is completed; the cation bed resin regenerated with double sulfuric acid solution is transferred to the resin storage tower, and the generated wastewater is discharged through the wastewater outlet;
[0149] The cation bed resin in the resin storage tower is forwardly washed with forward washing water through the forward washing water inlet until the conductivity of the water out of the resin storage tower is less than 1μs / cm and then it is ready for use;
[0150] The volume of sulfuric acid solution for conventional sulfuric acid regeneration of cation bed resin is 8 times the volume of cation bed resin, and the amount of sulfuric acid for double sulfuric acid regeneration of cation bed resin is 16 times the volume of cation bed resin.
[0151] The regenerated cation bed resin was put into full flow operation. During the operation of the cation bed, the sodium ion content in the steam generator wastewater no longer increased in the mixed bed, and it was slightly reduced. After the cation bed was put into operation, the sodium ion content at the mixed bed outlet was less than 0.008ppb, and the sodium ion concentration of the steam generator wastewater was maintained at 0.45ppb, achieving the expected target.
[0152] Example 8
[0153] This embodiment provides a cation bed resin regeneration process for a secondary loop condensate polishing system of a nuclear power plant, comprising the following steps:
[0154] When the cation bed resin fails, the failed cation bed resin is regenerated by the cation resin regeneration process of the nuclear power plant secondary loop condensate polishing system of Example 3.
[0155] Further, in this embodiment, the cation bed resin regeneration process of the secondary circuit condensate polishing system of the nuclear power plant is carried out in the cation bed regeneration system of the secondary circuit condensate polishing system of the nuclear power plant, and comprises the following steps:
[0156] When the cation bed resin fails, the failed cation bed resin is sent to the cation resin regeneration tower through the cation resin inlet for regeneration, and the spare cation bed resin in the resin storage tower is sent to the cation bed through the resin outlet for operation;
[0157] The cation bed resin in the cation resin regeneration tower is fed with a 5wt% sulfuric acid solution for 1 hour, and then replaced and washed with positive washing water at the positive washing water inlet, and then the conventional sulfuric acid solution regeneration of the cation bed resin is completed, so that its regeneration degree reaches 95%, and the concentration of sodium type cation resin in the cation bed resin accounts for 5%; the regenerated cation bed resin is left in the cation resin regeneration tower for ammonia saturation treatment, and the generated wastewater is discharged through the wastewater outlet;
[0158] The cation bed resin is circulated with water in the cation resin regeneration tower and the resin storage tower. During the circulation, ammonia water of 1.2 times the working exchange capacity of the cation bed resin is added to the cation resin regeneration tower until the concentration of the ammonium type cation resin in the cation bed resin reaches a peak value. After the ammonia water is added, the circulation is continued for 2 hours, and then the resin storage tower and the cation regeneration tower are washed in series to complete the ammonia saturation treatment of the cation bed resin.
[0159] When the conductivity of the water out of the resin storage tower is less than 2μs / cm, the cation bed resin serial washing is completed; after the cation bed resin serial washing is completed, the cation bed resin in the cation resin regeneration tower is regenerated by double sulfuric acid solution; the cation bed resin in the cation resin regeneration tower is fed with 5wt% sulfuric acid solution for 2 hours through the acid inlet, and the positive washing water inlet is replaced and forward washed until the conductivity of the water out of the cation resin regeneration tower is less than 3μs / cm, and then the regeneration of the cation bed resin with double sulfuric acid solution is completed; the cation bed resin regenerated with double sulfuric acid solution is transferred to the resin storage tower, and the generated wastewater is discharged through the wastewater outlet;
[0160] The cation bed resin in the resin storage tower is forwardly washed with forward washing water through the forward washing water inlet until the conductivity of the water out of the resin storage tower is less than 1μs / cm and then it is ready for use;
[0161] The volume of sulfuric acid solution for conventional sulfuric acid regeneration of cation bed resin is 8 times the volume of cation bed resin, and the amount of sulfuric acid for double sulfuric acid regeneration of cation bed resin is 16 times the volume of cation bed resin.
[0162] The regenerated cation bed resin was put into full flow operation. During the operation of the cation bed, the sodium ion content in the steam generator wastewater no longer increased in the mixed bed, and it was slightly reduced. After the cation bed was put into operation, the sodium ion content at the mixed bed outlet was less than 0.008ppb, and the sodium ion concentration of the steam generator wastewater was maintained at 0.45ppb, achieving the expected target.
[0163] Example 9
[0164] This embodiment provides a cation bed resin regeneration process for a secondary loop condensate polishing system of a nuclear power plant, comprising the following steps:
[0165] When the cation bed resin is not completely ineffective, the cation bed resin that is not completely ineffective is regenerated by the cation resin regeneration process of the nuclear power plant secondary loop condensate polishing system of Example 4.
[0166] Further, in this embodiment, the cation bed resin regeneration process of the secondary circuit condensate polishing system of the nuclear power plant is carried out in the mixed bed regeneration system of the secondary circuit condensate polishing system of the nuclear power plant, and comprises the following steps:
[0167] When the cation bed resin is not completely ineffective, the cation bed resin that is not completely ineffective is sent to the separation tower through the resin inlet, and the spare cation bed resin in the resin storage tower is sent to the cation bed through the resin outlet for operation;
[0168] The cation bed resin that has not been completely ineffective is transferred to the cation resin regeneration tower through the separation tower for regeneration; the cation bed resin that has not been completely ineffective is saturated with ammonia water in the cation resin regeneration tower, and the generated wastewater is discharged through the wastewater outlet;
[0169] The cation bed resin that has not been completely ineffective is circulated with water in the cation resin regeneration tower and the resin storage tower. During the circulation, ammonia water of 1.2 times the working exchange capacity of the cation bed resin is added to the cation resin regeneration tower until the concentration of the ammonium type cation resin in the cation bed resin reaches a peak value. After the ammonia water is added, the circulation is continued for 2 hours, and then the resin storage tower and the cation regeneration tower are washed in series to complete the ammonia saturation treatment of the cation bed resin.
[0170] When the conductivity of the water out of the resin storage tower is less than 2μs / cm, the cation bed resin serial washing is completed; after the cation bed resin serial washing is completed, the cation bed resin in the cation resin regeneration tower is regenerated by double sulfuric acid solution; the cation bed resin in the cation resin regeneration tower is fed with 5wt% sulfuric acid solution for 2 hours through the acid inlet, and the positive washing water inlet is replaced and forward washed until the conductivity of the water out of the cation resin regeneration tower is less than 3μs / cm, and then the regeneration of the cation bed resin with double sulfuric acid solution is completed; the cation bed resin regenerated with double sulfuric acid solution is transferred to the resin storage tower, and the generated wastewater is discharged through the wastewater outlet;
[0171] The cation bed resin in the resin storage tower is washed with positive washing water through the positive washing water inlet until the conductivity of the water out of the resin storage tower is less than 1μs / cm and then put into use; the amount of sulfuric acid used for regeneration of the cation bed resin with double sulfuric acid is 16 times the volume of the cation bed resin.
[0172] The regenerated cation bed resin was put into full flow operation. During the operation of the cation bed, the sodium ion content in the steam generator wastewater no longer increased in the mixed bed, and it was slightly reduced. After the cation bed was put into operation, the sodium ion content at the mixed bed outlet was less than 0.008ppb, and the sodium ion concentration of the steam generator wastewater was maintained at 0.45ppb, achieving the expected target.
[0173] Example 10
[0174] This embodiment provides a cation bed resin regeneration process for a secondary loop condensate polishing system of a nuclear power plant, comprising the following steps:
[0175] When the cation bed resin fails, the failed cation bed resin is regenerated by the cation resin regeneration process of the nuclear power plant secondary loop condensate polishing system of Example 4.
[0176] Further, in this embodiment, the cation bed resin regeneration process of the secondary circuit condensate polishing system of the nuclear power plant is carried out in the cation bed regeneration system of the secondary circuit condensate polishing system of the nuclear power plant, and comprises the following steps:
[0177] When the cation bed resin fails, the failed cation bed resin is sent to the cation resin regeneration tower through the cation resin inlet for regeneration, and the spare cation bed resin in the resin storage tower is sent to the cation bed through the resin outlet for operation;
[0178] The cation bed resin is saturated with ammonia water in the cation resin regeneration tower, and the generated wastewater is discharged through the wastewater outlet; the cation bed resin is circulated with water in the cation resin regeneration tower and the resin storage tower, and ammonia water 1.2 times the working exchange capacity of the cation bed resin is added to the cation resin regeneration tower during the circulation until the concentration of the ammonium type cation resin in the cation bed resin reaches a peak value, and the circulation is continued for 2 hours after the ammonia water is added, and then the resin storage tower and the cation regeneration tower are washed in series to complete the ammonia water saturation treatment of the cation bed resin;
[0179] When the conductivity of the water out of the resin storage tower is less than 2μs / cm, the cation bed resin serial washing is completed; after the cation bed resin serial washing is completed, the cation bed resin in the cation resin regeneration tower is regenerated by double sulfuric acid solution; the cation bed resin in the cation resin regeneration tower is fed with 5wt% sulfuric acid solution for 2 hours through the acid inlet, and the positive washing water inlet is replaced and forward washed until the conductivity of the water out of the cation resin regeneration tower is less than 3μs / cm, and then the regeneration of the cation bed resin with double sulfuric acid solution is completed; the cation bed resin regenerated with double sulfuric acid solution is transferred to the resin storage tower, and the generated wastewater is discharged through the wastewater outlet;
[0180] The cation bed resin in the resin storage tower is washed with positive washing water through the positive washing water inlet until the conductivity of the water out of the resin storage tower is less than 1μs / cm and then put into use; the amount of sulfuric acid used for regeneration of the cation bed resin with double sulfuric acid is 16 times the volume of the cation bed resin.
[0181] The regenerated cation bed resin was put into full flow operation. During the operation of the cation bed, the sodium ion content in the steam generator wastewater no longer increased in the mixed bed, and it was slightly reduced. After the cation bed was put into operation, the sodium ion content at the mixed bed outlet was less than 0.008ppb, and the sodium ion concentration of the steam generator wastewater was maintained at 0.45ppb, achieving the expected target.
[0182] In the above-mentioned present embodiment, the mixed bed resin regeneration system of the secondary circuit condensate polishing system of the nuclear power plant comprises a separation tower, a cation resin regeneration tower, an anion resin regeneration tower and a resin storage tower, wherein spare resin is stored in the resin storage tower; the separation tower is provided with a forward wash water inlet, a resin inlet and a backwash water inlet, a cation resin outlet and an anion resin outlet; the cation resin regeneration tower is provided with a cation resin inlet, a forward wash water inlet, an acid inlet, a cation resin outlet and a wastewater outlet; the anion resin regeneration tower is provided with an anion resin inlet, a forward wash water inlet, an alkali inlet, an anion resin outlet and a wastewater outlet; the resin storage tower is provided with a forward wash water inlet, a resin outlet and a wastewater outlet; the cation resin outlet of the separation tower is connected with the cation resin inlet pipeline of the cation resin regeneration tower, and the anion resin outlet of the separation tower is connected with the anion resin inlet pipeline of the anion resin regeneration tower; the resin outlet of the resin storage tower is connected with the mixed bed and cation bed pipelines respectively.
[0183] In the above-mentioned present embodiment, the cationic bed resin regeneration system of the secondary circuit condensate polishing system of the nuclear power plant comprises a cationic resin regeneration tower and a resin storage tower, in which spare resin is stored; the cationic resin regeneration tower is provided with a cationic resin inlet, a positive wash water inlet, an acid liquid inlet, a cationic resin outlet and a waste water outlet; the resin storage tower is provided with a positive wash water inlet, a resin outlet and a waste water outlet; the resin outlet of the resin storage tower is connected with the cationic bed pipeline.
[0184] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A cation resin regeneration process for a secondary loop condensate polishing system of a nuclear power plant, characterized in that: The method comprises the following steps: when the cation resin of the secondary circuit condensate polishing system of a nuclear power plant fails, the failed cation resin is firstly regenerated with conventional acid solution, then saturated with ammonia water, and finally regenerated with double amount of acid solution; wherein, the conventional acid solution regeneration of the failed cation resin is an optional step, and the amount of acid solution used for the double amount of acid solution regeneration of the cation resin is twice the amount of acid solution used for the conventional acid solution regeneration of the cation resin.
2. The process for regenerating cationic resin in the secondary circuit condensate polishing system of a nuclear power plant according to claim 1, characterized in that: When the cation resin of the secondary condensate polishing system of a nuclear power plant fails, the failed cation resin is first regenerated with conventional acid solution, then saturated with ammonia water, and finally regenerated with double amount of acid solution; the failure of the cation resin of the secondary condensate polishing system of the nuclear power plant refers to the complete failure of the cation resin of the secondary condensate polishing system of the nuclear power plant or the incomplete failure of the cation resin of the secondary condensate polishing system of the nuclear power plant.
3. The process for regenerating cationic resin in the secondary circuit condensate polishing system of a nuclear power plant according to claim 2, characterized in that: When the cation resin of the secondary circuit condensate polishing system of a nuclear power plant fails, the failed cation resin is first regenerated with conventional acid solution to achieve a regeneration degree of 95%, with the concentration of sodium type cation resin in the cation resin accounting for 5%; then it is saturated with ammonia water; finally, it is regenerated with double the amount of acid solution, ultimately making the regeneration degree of the cation resin not less than 95%, with the concentration of sodium type resin in the cation resin accounting for less than 0.3%.
4. The process for regenerating cation resin in the secondary circuit condensate polishing system of a nuclear power plant according to claim 3, characterized in that: When the cation resin of the secondary circuit condensate polishing system of a nuclear power plant fails, the failed cation resin is fed with a 5wt% sulfuric acid solution for 1 hour, replaced and washed with positive wash water to complete the conventional sulfuric acid solution regeneration of the cation resin, so that its regeneration degree reaches 95%, and the concentration of sodium type cation resin in the cation resin accounts for 5%; the regenerated cation resin is circulated with water, and ammonia water with a working exchange capacity of 1.2 times of the cation resin is added while circulating until the concentration of ammonium type cation resin in the cation resin reaches a peak value, and the circulation continues for 2 hours after the ammonia water is added, and then washed in series until the output The water conductivity is less than 2μs / cm, and the ammonia saturation treatment of the cation resin is completed; the cation resin after the ammonia saturation treatment is fed with a 5wt% sulfuric acid solution for 2 hours, replaced and washed with positive washing water until the outlet water conductivity is less than 3μs / cm, and then the cation resin is regenerated with double sulfuric acid, so that its regeneration degree is not less than 95%, and the concentration of sodium type resin in the cation resin is less than 0.3%; the volume of sulfuric acid solution for conventional sulfuric acid regeneration of the cation resin is 8 times the volume of the cation resin, and the amount of sulfuric acid used for double sulfuric acid regeneration of the cation resin is 16 times the volume of the cation resin.
5. The process for regenerating cation resin in the secondary circuit condensate polishing system of a nuclear power plant according to claim 1, characterized in that: When the cation resin of the secondary circuit condensate polishing system of a nuclear power plant has not completely failed, the cation resin that has not completely failed is first saturated with ammonia water and then regenerated with double the amount of acid solution.
6. The process for regenerating cation resin in the secondary circuit condensate polishing system of a nuclear power plant according to claim 5, characterized in that: When the cation resin of the secondary circuit condensate polishing system of a nuclear power plant has not completely failed, the cation resin that has not completely failed is first saturated with ammonia water and then regenerated with double the amount of acid solution, so that the regeneration degree of the cation resin is finally not less than 95%, and the concentration of sodium type resin in the cation resin is less than 0.3%.
7. The process for regenerating cation resin in the secondary circuit condensate polishing system of a nuclear power plant according to claim 6, characterized in that: When the cation resin of the secondary loop condensate polishing system of the nuclear power plant has not failed, the cation resin that has not failed is circulated with water, and ammonia water of 1.2 times the working exchange capacity of the cation resin is added during the circulation until the concentration ratio of ammonium type cation resin in the cation resin reaches a peak value. After the ammonia water is added, the circulation continues for 2 hours, and then the cation resin is washed in series until the effluent conductivity is less than 2μs / cm, thereby completing the ammonia saturation treatment of the cation resin; the cation resin after the ammonia saturation treatment is fed with 5wt% sulfuric acid solution for 2 hours, replaced and washed with positive washing water until the effluent conductivity is less than 3μs / cm, and then the cation resin is regenerated with double sulfuric acid, so that its regeneration degree is not less than 95%, and the concentration ratio of sodium type resin in the cation resin is less than 0.3%; the amount of sulfuric acid used for the double sulfuric acid regeneration of the cation resin is 16 times the volume of the cation resin.
8. The process for regenerating cation resin in a secondary circuit condensate polishing system of a nuclear power plant according to claim 1, characterized in that: The cationic resin of the secondary circuit condensate polishing system of a nuclear power plant is a mixed bed cationic resin of the secondary circuit condensate polishing system of a nuclear power plant or a cationic bed resin of the secondary circuit condensate polishing system of a nuclear power plant.
9. The process for regenerating cation resin in a secondary circuit condensate polishing system of a nuclear power plant according to claim 1, characterized in that: The acid solution is a 5wt% sulfuric acid solution.
10. A mixed bed resin regeneration process for a secondary circuit condensate polishing system of a nuclear power plant, when the mixed bed resin fails, the failed mixed bed resin is scrubbed with air, backwashed, layered and left to stand, the anion resin is regenerated, and the cation resin is regenerated; the anion resin is regenerated after being fed with alkali solution, replaced and forwardly washed to be qualified; the regenerated cation resin and anion resin are mixed with air and forwardly washed to be ready for use, characterized in that: The cation resin is regenerated by the cation resin regeneration process of the nuclear power plant secondary loop condensate polishing system as described in any one of claims 1-9.
11. The mixed bed resin regeneration process for the secondary circuit condensate polishing system of a nuclear power plant according to claim 10, characterized in that: The mixed bed resin regeneration process of the secondary loop condensate polishing system of the nuclear power plant is carried out in the mixed bed regeneration system of the secondary loop condensate polishing system of the nuclear power plant.
12. A cation bed resin regeneration process for a secondary loop condensate polishing system of a nuclear power plant, characterized in that: When the cation bed resin fails, the failed cation bed resin is regenerated by the cation resin regeneration process of the nuclear power plant secondary loop condensate polishing system as described in any one of claims 1-9.
13. The mixed bed resin regeneration process for the secondary circuit condensate polishing system of a nuclear power plant according to claim 12, characterized in that: The cation bed resin regeneration process of the secondary circuit condensate polishing system of a nuclear power plant is carried out in the mixed bed regeneration system of the secondary circuit condensate polishing system of a nuclear power plant.
14. The mixed bed resin regeneration process for the secondary circuit condensate polishing system of a nuclear power plant according to claim 12, characterized in that: The cation bed resin regeneration process of the secondary circuit condensate polishing system of a nuclear power plant is carried out in the cation bed regeneration system of the secondary circuit condensate polishing system of a nuclear power plant.
15. A resin regeneration process for a secondary circuit condensate polishing system of a nuclear power plant, characterized in that: It includes the mixed bed resin regeneration process of the secondary circuit condensate polishing system of the nuclear power plant and the cation bed resin regeneration process of the secondary circuit condensate polishing system of the nuclear power plant.
Citation Information
Patent Citations
Separation and purification method for lysine
CN102206168A
Ion exchange resin regeneration process and device
CN113042114A
Duel compartment coagulation mixed beds external regeneration knockout tower and regeneration art work
CN1919460A
Ion exchange resin regeneration device
CN214765522U
Regenerating method of condensed water desalting equipment using ammonia
JP1980094649A
Cited By
Method for reducing amount of regenerated tritium-containing wastewater of high-temperature gas cooled reactor condensate polishing system