Beneficiation method for recovering iron and titanium from low-grade vanadium titano-magnetite
By adopting a comprehensive process of crushing, tailings, grinding, magnetic separation and flotation in low-grade vanadium-titanium magnetite, the problem of low iron and titanium recovery rates in vanadium-titanium magnetite is solved and the concentrate grade is improved. and recycling rate, achieving efficient use of resources and environmental protection and energy saving.
Patent Information
- Application Number
- CN202410632215.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-21
- Publication Date
- 2024-10-15
AI Technical Summary
Existing technology is difficult to effectively recover iron and titanium in low-grade vanadium-titanium magnetite, resulting in low concentrate grade and low recovery rate, especially when the ore properties are complex.
The comprehensive process of crushing, tailing, grinding, weak magnetic separation, strong magnetic separation, classification, gravity separation and flotation is used to reduce the amount of low-grade ore fed into the grinding by pre-tailing and improve the grade of the concentrate. And improve the recovery rate of titanium through multi-layer magnetic separation and flotation.
It achieves efficient recovery of iron and titanium in low-grade vanadium-titanium magnetite, improves the concentrate grade and recovery rate, and reduces production costs. It is suitable for complex and difficult-to-select low-grade vanadium-titanium magnetite, and has the advantages of environmental protection and energy saving. .
Smart Images

Figure CN118768077A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of mineral processing, for example, to a mineral processing method for recovering iron and titanium from low-grade vanadium-titanium magnetite. Background Art
[0002] Vanadium-titanium magnetite is a composite mineral resource containing iron, vanadium and titanium. It is one of my country's strategic mineral resources and is widely used in national defense, military, metallurgy, aerospace, electronic technology and materials science. Vanadium-titanium magnetite is an important source of vanadium and titanium. Compared with other iron ore resources, vanadium-titanium magnetite contains a variety of valuable metals, so its comprehensive utilization value is higher. my country's mineral resources are very rich, but most of my country's mineral resources are poor ores, and there are fewer rich ores, especially high-grade iron ore resources suitable for blast furnace ironmaking, which have long relied on imports; at the same time, after decades of development and utilization, the reserves of rich ores are decreasing; at present, the prospective reserves of ultra-poor vanadium-titanium magnetite exceed 10 billion tons. Faced with increasingly tense international pressure and resource pressure, low-grade ores, complex and difficult-to-select ores and difficult-to-smelt ores have become important backup resources for my country's mineral resources. Therefore, the efficient development and utilization of low-grade vanadium-titanium magnetite is of great strategic significance to my country's economic construction and national defense construction.
[0003] For vanadium-titanium magnetite, there are many chemical elements in its ore, iron and titanium elements are closely coexisting, the mineral composition is complex, the intercalation relationship between minerals is also relatively complex, and the ore structure and mineral structure are diversified. Specifically, titanomagnetite generally has different degrees of titanolitization, chloritization and biotitization, which will affect the quality of iron concentrate; in addition, the occurrence state of ilmenite is mainly granular ilmenite and flaky ilmenite dissolved in titanomagnetite. The extremely fine ilmenite lamellae in titanomagnetite are difficult to be effectively recovered through mineral processing. The titanium in minerals such as titanomagnetite, titanophene and pyroxene is a dispersed titanium that is difficult to use, which restricts the recovery of titanium in titanium concentrate. In view of this, the utilization rate of iron and titanium in low-grade vanadium-titanium magnetite is currently low. Therefore, the sorting technology and comprehensive utilization of low-grade vanadium-titanium magnetite have always been a hot topic for research by scientific and technological workers at home and abroad.
[0004] At present, the main methods for the beneficiation and enrichment of vanadium-titanium magnetite include magnetic separation, gravity separation, electrostatic separation, flotation and a combination of multiple beneficiation methods. Generally speaking, vanadium-titanium magnetite ore needs to be crushed to a certain fineness, and vanadium-titanium magnetite concentrate is first obtained through strong magnetic separation. This part of the concentrate is mainly magnetite or titanium magnetite minerals, and then the ilmenite concentrate is obtained from the magnetic tailings by flotation, strong magnetic separation-flotation, gravity separation-electrostatic separation, strong magnetic separation-electrostatic separation and other methods. For example, Chinese patent document CN201410019663.8 discloses an efficient beneficiation method for comprehensive recovery of low-grade vanadium-titanium magnetite, which adopts a two-stage grinding-two-stage weak magnetic separation-gravity separation process. By using this process, iron concentrate with a TFe grade of 53.64% and TiO 2 The titanium concentrate with a grade of 42.63% is produced. However, although the process is simple, a large amount of low-grade vanadium-titanium magnetite gangue directly enters the grinding stage, resulting in a relatively low quality of the concentrate. In view of this, as more and more low-grade vanadium-titanium magnetite resources are put into development and utilization, if a large amount of lean ore resources containing surrounding rocks directly enter the grinding process, the quality of the concentrate will inevitably decline.
[0005] In summary, there is an urgent need for a mineral processing method that can effectively recover iron and titanium from complex and difficult-to-process low-grade vanadium-titanium magnetite, so that it can not only maximize the recovery and utilization of the valuable elements iron and titanium, but also improve the grade and recovery rate of the resulting concentrate. Summary of the invention
[0006] The purpose of the present invention is to overcome the deficiencies in the prior art and to provide a beneficiation method for recovering iron and titanium from low-grade vanadium-titanium magnetite, so that it is suitable for complex and difficult to select low-grade vanadium-titanium magnetite, and at least achieves the effect of not only maximizing the recovery and utilization of the valuable elements iron and titanium, but also improving the grade and recovery rate of the resulting concentrate.
[0007] The purpose of this disclosure is achieved through the following technical solutions:
[0008] On the one hand, a beneficiation method for recovering iron and titanium from low-grade vanadium-titanium magnetite is provided. The beneficiation method comprises: crushing the low-grade vanadium-titanium magnetite ore to obtain crushed ore; discarding the crushed ore to obtain rough discard concentrate and rough discard tailings; grinding and weak magnetic separation of the rough discard concentrate to obtain iron concentrate and iron-separated tailings; performing first strong magnetic separation on the iron-separated tailings to obtain first strong magnetic separation concentrate and first strong magnetic separation tailings; classifying the first strong magnetic separation concentrate to obtain coarse sand and fine mud; performing gravity separation on the coarse sand to obtain gravity separation concentrate and gravity separation tailings; performing second strong magnetic separation on the fine mud to obtain second strong magnetic separation concentrate and second strong magnetic separation tailings; and combining the gravity separation concentrate with the second strong magnetic separation concentrate for flotation to obtain sulfur concentrate, titanium concentrate and flotation tailings.
[0009] It should be noted that the first high-intensity magnetic separation tailings, the gravity separation tailings, the second high-intensity magnetic separation tailings and the flotation tailings are combined into the total tailings.
[0010] It should be understood that titanomagnetite generally has varying degrees of titanitization, chloritization and biotitization, which will affect the quality of iron ore concentrate; in addition, the occurrence state of ilmenite is mainly granular ilmenite and flaky ilmenite dissolved from titanomagnetite. The extremely fine ilmenite flakes in titanomagnetite are difficult to be effectively recovered through mineral processing. The titanium in minerals such as titanomagnetite, titanophene and pyroxene is dispersed titanium that is difficult to utilize, which restricts the recovery of titanium in titanium concentrate.
[0011] On this basis, in some embodiments, the TiO 2 The grade is 3.5% to 5.5%.
[0012] In some examples, the TFe grade in the low-grade vanadium-titanium magnetite ore is 12.5% to 16.0%.
[0013] It can be seen that in the above embodiment, the low-grade vanadium-titanium magnetite ore is a complex and difficult to select low-grade vanadium-titanium magnetite, for example, TFe and TiO 2 Low-grade gabbro-type vanadium-titanium magnetite.
[0014] In some embodiments, the crushing of low-grade vanadium-titanium magnetite ore to obtain crushed ore includes: performing secondary crushing and first screening on the low-grade vanadium-titanium magnetite ore to obtain secondary crushed ore and first intermediate ore, wherein the first intermediate ore is returned to the secondary crushing; and performing fine crushing and second screening on the secondary crushed ore to obtain the crushed ore and second intermediate ore, wherein the second intermediate ore is returned to the fine crushing.
[0015] In some examples, the particle size of the medium-crushed ore is -12.0 mm, and the particle size of the crushed ore is -3.0 mm.
[0016] In some examples, the secondary crushing is performed using a jaw crusher.
[0017] In some examples, the comminution is performed using a high pressure roller mill.
[0018] In some embodiments, the tailings discarding of the crushed ore to obtain rough discard concentrate and rough discard tailings includes: dry discarding of the crushed ore to obtain dry discard concentrate and dry discard tailings; and wet discarding of the dry discard tailings to obtain wet discard concentrate and the rough discard tailings, wherein the dry discard concentrate and the wet discard concentrate are combined into the rough discard concentrate.
[0019] In some examples, the magnetic field strength of the dry tail is 4000-7000 Oe.
[0020] In some examples, the magnetic field strength of the wet tailing is 4000-7000 Oe.
[0021] In the above embodiment, by performing the tailings discarding on the crushed ore, the ore processing volume of the grinding can be reduced, thereby reducing the ore dressing cost; wherein, by performing the dry tailings discarding on the crushed ore, magnetic iron can be recovered, and by performing the wet tailings discarding on the dry tailings, titanium recovery can be ensured.
[0022] In some embodiments, the grinding and weak magnetic separation of the roughing concentrate to obtain iron concentrate and iron-separated tailings includes: performing a first grinding on the roughing concentrate to obtain a first grinding product; performing a first stage of weak magnetic separation on the first grinding product to obtain a first stage of weak magnetic separation concentrate and a first stage of weak magnetic separation tailings; performing a second grinding on the first stage of weak magnetic separation concentrate to obtain a second grinding product; and performing a second stage of weak magnetic separation on the second grinding product to obtain the iron concentrate and a second stage of weak magnetic separation tailings, wherein the first stage of weak magnetic separation tailings and the second stage of weak magnetic separation tailings are combined into the iron-separated tailings.
[0023] In some examples, the mass percentage of minerals with a particle size of -0.074 mm in the first grinding product is 40% to 55%.
[0024] In some examples, the mass percentage of minerals with a particle size of -0.074 mm in the second grinding product is 60% to 95%.
[0025] In some examples, the grinding is performed using a rod mill.
[0026] Exemplarily, the first grinding and the second grinding are each performed using the rod mill.
[0027] In some examples, the low-intensity magnetic separation includes wet low-intensity magnetic separation.
[0028] Exemplarily, the first-stage weak magnetic separation and the second-stage weak magnetic separation each include the wet weak magnetic separation.
[0029] In some examples, the magnetic field strength of the one-stage weak magnetic separation is 2000-4000 Oe.
[0030] In some examples, the magnetic field strength of the second-stage weak magnetic separation is 1000-3000 Oe.
[0031] In some embodiments, the magnetic field strength of the first strong magnetic separation is 6000-9000 Oe.
[0032] In some embodiments, the particle size of the coarse sand is +0.074 mm, and the particle size of the fine mud is -0.074 mm.
[0033] In some examples, the classification is performed using a high frequency vibrating screen and a hydrocyclone.
[0034] In the above example, the classification can be accurately achieved at a finer particle size by using the combination of the high-frequency vibrating screen and the hydrocyclone to perform the classification.
[0035] In some embodiments, the re-selection of the coarse sand to obtain the re-selection concentrate and the re-selection tailings includes: performing a first-stage re-selection on the coarse sand to obtain a first-stage re-selection concentrate and a first-stage re-selection tailings; and performing a second-stage re-selection on the first-stage re-selection tailings to obtain a second-stage re-selection concentrate and the re-selection tailings, wherein the first-stage re-selection concentrate and the second-stage re-selection concentrate are combined into the re-selection concentrate.
[0036] In some examples, the gravity selection is performed using a spiral chute.
[0037] Exemplarily, the first-stage gravity selection and the second-stage gravity selection are each carried out using the spiral chute.
[0038] In the above example, by adopting the spiral chute to carry out the gravity separation, the recovery effect of coarse-grained heavy minerals can be improved compared with other equipment.
[0039] In some embodiments, the subjecting the fine mud to a second strong magnetic separation to obtain a second strong magnetic separation concentrate and a second strong magnetic separation tailings comprises: subjecting the fine mud to a first-stage strong magnetic separation to obtain a first-stage strong magnetic separation concentrate and a first-stage strong magnetic separation tailings; and subjecting the first-stage strong magnetic separation concentrate to a second-stage strong magnetic separation concentrate to obtain a second-stage strong magnetic separation concentrate and a second-stage strong magnetic separation tailings, wherein the first-stage strong magnetic separation tailings and the second-stage strong magnetic separation tailings are combined into the second strong magnetic separation tailings.
[0040] In some examples, the magnetic field strength of the one-stage high-intensity magnetic separation is 5000-7000 Oe.
[0041] In some examples, the magnetic field strength of the second-stage high-intensity magnetic separation is 3000-5000 Oe.
[0042] In some embodiments, the flotation includes flotation desulfurization and flotation titanium.
[0043] In some examples, the flotation desulfurization is performed once.
[0044] In some examples, the flotation of titanium includes rough flotation, scavenging flotation, and concentrating flotation.
[0045] Exemplarily, the number of flotation roughing selection is 1 time, the number of flotation sweeping selection is 1 to 2 times, and the number of flotation cleaning selection is 2 to 4 times.
[0046] In some embodiments, the flotation reagents include sulfuric acid, butyl xanthate, 2 # Oil, diesel, sodium fluorosilicate and fatty acid collectors.
[0047] In some examples, in the flotation, the total amount of sulfuric acid is 4000-5500 g / t·feed ore, the total amount of butyl xanthate is 100-300 g / t·feed ore, and the 2 # The total amount of oil is 20-120 g / t·feed ore, the total amount of diesel is 200-500 g / t·feed ore, the total amount of sodium fluorosilicate is 300-700 g / t·feed ore, and the total amount of fatty acid collector is 3000-4500 g / t·feed ore.
[0048] In some examples, the fatty acid collector includes MOH and styrenephosphonic acid.
[0049] Exemplarily, the mass ratio of the MOH to the styrenephosphonic acid is 4:1.
[0050] In the above example, by using the MOH and the styrenephosphonic acid as the fatty acid collector, the selective capture ability of the fatty acid collector can be improved; on this basis, by limiting the mass ratio of the MOH to the styrenephosphonic acid, the selective capture ability of the fatty acid collector can be further improved.
[0051] It should be noted that the principle of the mineral processing method provided in the present disclosure includes: first, the low-grade vanadium-titanium magnetite ore is crushed (for example, the medium crushing and the fine crushing) and the tailings are discarded (for example, the dry tailings and the wet tailings) to obtain the rough concentrate; secondly, the rough concentrate is subjected to the grinding (for example, the first grinding and the second grinding) and the weak magnetic separation (for example, the first weak magnetic separation and the second weak magnetic separation) to obtain the iron concentrate and titanium selection material (that is, the iron selection tailings); then, the above-mentioned titanium selection material is subjected to the first strong magnetic separation and the The classification is performed to obtain the coarse sand and the fine mud; then, the coarse sand is subjected to the gravity separation (for example, the first-stage gravity separation and the second-stage gravity separation) to obtain the gravity separation concentrate and the gravity separation tailings; then, the fine mud is subjected to the second high-intensity magnetic separation (for example, the first-stage high-intensity magnetic separation and the second-stage high-intensity magnetic separation) to obtain the second high-intensity magnetic separation concentrate and the second high-intensity magnetic separation tailings; finally, the pre-enriched concentrate (that is, the gravity separation concentrate and the second high-intensity magnetic separation concentrate) is subjected to the flotation (for example, the flotation desulfurization and the flotation titanium selection) to obtain the sulfur concentrate, the titanium concentrate and the flotation tailings.
[0052] In this regard, it is worth noting that the mineral processing method provided by the present disclosure can preferentially discard part of the low-grade vanadium-titanium magnetite gangue by pre-carrying out the tailings discarding before the grinding and the weak magnetic separation, which can not only improve the grade of the in-grinding material (i.e., the roughing concentrate) for the grinding, thereby improving the grade and recovery rate of the obtained concentrate (for example, the titanium concentrate and the iron concentrate), but also reduce the ore processing volume of the grinding, thereby reducing production energy consumption and reducing the cost of tailings processing, which is in line with the environmental protection and energy-saving concept of "more crushing, less grinding, and early discarding when possible" in the mineral processing industry, and can maximize the economic benefits of the enterprise; in addition, for the For low-grade vanadium-titanium magnetite, iron is mainly found in titanomagnetite, and titanium is mainly found in ilmenite. Since the magnetism of ilmenite is weaker than that of titanomagnetite, the first strong magnetic separation of the titanium material obtained by the weak magnetic separation can enrich the titanium-containing minerals to reduce the processing volume of subsequent operations, thereby reducing costs and simplifying the process. On this basis, by classifying the first strong magnetic concentrate and performing the gravity separation and the second strong magnetic separation on the coarse sand and the fine mud obtained by the classification, not only can the separation effects of the gravity separation and the second strong magnetic separation be improved, but also it is beneficial to the subsequent flotation.
[0053] The beneficial effects of the present disclosure are:
[0054] 1. The present invention provides a beneficiation method for recovering iron and titanium from low-grade vanadium-titanium magnetite, which can effectively recover valuable metals to obtain high-quality iron concentrate and titanium concentrate, providing a new way for the efficient development and utilization of low-grade vanadium-titanium magnetite, and can improve the utilization rate of my country's vanadium-titanium magnetite resources. It is of great significance to alleviate my country's dependence on imports of high-grade iron ore resources.
[0055] 2. The present invention provides a beneficiation method for recovering iron and titanium from low-grade vanadium-titanium magnetite, which is suitable for low-grade vanadium-titanium magnetite with complex ore properties and has the advantages of a wide range of applications and good comprehensive recovery effect.
[0056] 3. The present invention provides a beneficiation method for recovering iron and titanium from low-grade vanadium-titanium magnetite, which can reduce costs and thus improve production efficiency.
[0057] 4. The present invention provides a beneficiation method for recovering iron and titanium from low-grade vanadium-titanium magnetite. The process is mature, green and environmentally friendly, easy to control, and convenient for promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] In order to more clearly illustrate the technical solutions in the present disclosure, the following briefly introduces the drawings required to be used in some embodiments of the present disclosure. Obviously, the drawings described below are only drawings of some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can also be obtained based on these drawings. In addition, the drawings described below can be regarded as schematic diagrams, and are not limitations on the actual process of the method involved in the embodiments of the present disclosure.
[0059] Figure 1 A process flow chart of a beneficiation method for recovering iron and titanium from low-grade vanadium-titanium magnetite is provided in the present invention. DETAILED DESCRIPTION
[0060] The technical solutions in some embodiments of the present disclosure are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments provided by the present disclosure, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present disclosure.
[0061] In the following, the terms "first", "second", etc. are used for descriptive purposes only and are not to be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first", "second", etc. may explicitly or implicitly include one or more of the features.
[0062] When describing some embodiments, the expression "A and / or B" may be used. It is easy to understand that "A and / or B" includes the following three combinations: only A, only B, and a combination of A and B.
[0063] When describing some embodiments, the expressions "at least one of A, B and C" and "at least one of A, B or C" may be used, both of which have the same meaning and include the following combinations of A, B and C: A only, B only, C only, the combination of A and B, the combination of A and C, the combination of B and C, and the combination of A, B and C.
[0064] Example 1
[0065] This embodiment provides a beneficiation method for recovering iron and titanium from low-grade vanadium-titanium magnetite, so as to recover iron and titanium from a vanadium-titanium magnetite ore, wherein the grade of TFE in the vanadium-titanium magnetite is 12.98%, and the grade of TiO 2 The grade is 3.72%, and the quantitative results of its main minerals are shown in Table 1.
[0066] Table 1 Main mineral composition and content of raw ore comprehensive sample
[0067] Mineral Name Plagioclase Pyroxene Hornblende Titanomagnetite Ilmenite Epidote Chlorite content(%) 34.00 22.08 12.21 9.31 5.58 3.44 2.68 Mineral Name Biotite Peridot quartz Calcite Kaolinite Spinel apatite content(%) 2.57 2.29 1.35 1.10 0.97 0.75 0.59 Mineral Name Pyrrhotite Sphene Pyrite Rutile Other minerals content(%) 0.41 0.36 0.09 0.07 0.15
[0068] like Figure 1 As shown, the above-mentioned mineral processing method comprises:
[0069] S1. The vanadium-titanium magnetite ore (ie, the raw ore) is crushed by a jaw crusher and then sieved to obtain a medium-crushed ore with a particle size of -12.0 mm and a first medium ore with a particle size of +12.0 mm; wherein the first medium ore is returned to the medium crushing step;
[0070] S2. The medium ore is crushed by a high pressure roller mill and then sieved to obtain a crushed ore with a particle size of -3.0 mm and a second medium ore with a particle size of +3.0 mm; wherein the second medium ore is returned to the fine crushing step;
[0071] S3. The crushed ore is dry-thrown, and the magnetic field strength is 5000Oe to obtain dry-throw concentrate and dry-throw tailings;
[0072] S4. The dry tailings are wet-discarded, and the magnetic field strength is 5000Oe to obtain wet-discarded concentrate and rough-discarded tailings; wherein the dry-discarded concentrate and the wet-discarded concentrate are combined into a rough-discarded concentrate;
[0073] S5. The coarse concentrate is ground by a rod mill to obtain a first grinding product; wherein the mass percentage of the mineral having a particle size of -0.074 mm in the first grinding product is 50%;
[0074] S6. The first grinding product is subjected to a wet weak magnetic separation with a magnetic field strength of 3000Oe to obtain a weak magnetic separation concentrate and a weak magnetic separation tailings;
[0075] S7. A rod mill is used to grind a weak magnetic separation concentrate to obtain a second grinding product; wherein the mass percentage of the mineral having a particle size of -0.074 mm in the second grinding product is 95%;
[0076] S8. The second grinding product is subjected to a two-stage wet weak magnetic separation with a magnetic field strength of 2000Oe to obtain an iron concentrate and a two-stage weak magnetic separation tailing; wherein the first stage weak magnetic separation tailing and the second stage weak magnetic separation tailing are combined into an iron separation tailing;
[0077] S9. The iron ore tailings are subjected to a first strong magnetic separation, with a magnetic field strength of 8000 Oe, to obtain a first strong magnetic separation concentrate and a first strong magnetic separation tailings;
[0078] S10. The first high-frequency vibrating screen and hydrocyclone are used to classify the concentrate to obtain coarse sand with a particle size of +0.074 mm and fine mud with a particle size of -0.074 mm;
[0079] S11. A spiral chute is used to perform a first stage of gravity separation on the coarse sand to obtain a first stage of gravity separation concentrate and a first stage of gravity separation tailings;
[0080] S12. The first stage gravity separation tailings are subjected to second stage gravity separation using a spiral chute to obtain a second stage gravity separation concentrate and gravity separation tailings; wherein the first stage gravity separation concentrate and the second stage gravity separation concentrate are combined into a gravity separation concentrate;
[0081] S13. The fine mud is subjected to a strong magnetic separation with a magnetic field strength of 6000Oe to obtain a strong magnetic separation concentrate and a strong magnetic separation tailings;
[0082] S14. The first stage strong magnetic separation concentrate is subjected to a second stage strong magnetic separation, and the magnetic field strength is 4000Oe to obtain a second stage strong magnetic separation concentrate and a second stage strong magnetic separation tailings; wherein the gravity separation concentrate and the second stage strong magnetic separation concentrate are combined into a floating material; the first stage strong magnetic separation tailings and the second stage strong magnetic separation tailings are combined into the second stage strong magnetic separation tailings;
[0083] S15. The floating material is floated to obtain sulfur concentrate, titanium concentrate and flotation tailings; wherein the first strong magnetic separation tailings, gravity separation tailings, second strong magnetic separation tailings and flotation tailings are combined into total tailings; the reagents used in flotation include sulfuric acid 5400g / t·feed, butyl xanthate 200g / t·feed, 2 #Oil 116g / t·feed, diesel 460g / t·feed, sodium fluorosilicate 500g / t·feed and fatty acid collector (i.e., MOH and styrenephosphonic acid in a mass ratio of 4:1) 3950g / t·feed; flotation includes flotation desulfurization and flotation titanium, and flotation titanium includes flotation roughing, flotation scavenging and flotation concentration; the number of flotation desulfurization is 1 time; the number of flotation roughing is 1 time, the number of flotation scavenging is 1 time, and the number of flotation concentration is 4 times.
[0084] The results show that in the ore dressing method of this embodiment, the yield of iron concentrate is 9.16%, the grade of TFe is 61.44%, and the recovery rate of TFE is 43.36%; the yield of titanium concentrate is 3.50%, and the grade of TiO 2 The grade is 47.08%, TiO 2 The recovery rate is 44.28%. Therefore, the ore dressing method of this embodiment achieves effective recovery of iron and titanium in low-grade vanadium-titanium magnetite.
[0085] Example 2
[0086] This embodiment provides a beneficiation method for recovering iron and titanium from low-grade vanadium-titanium magnetite, so as to recover iron and titanium from a vanadium-titanium magnetite ore, wherein the grade of TFE in the vanadium-titanium magnetite ore is 14.06%, and the grade of TiO 2 The grade is 4.53%, and the quantitative results of its main minerals are shown in Table 2.
[0087] Table 2 Main mineral composition and content of raw ore comprehensive sample
[0088] Mineral Name Feldspar Pyroxene Titanomagnetite Ilmenite Peridot Amphibole Chlorite content(%) 38.50 29.10 11.25 5.35 5.00 2.80 2.50 Mineral Name apatite Biotite Pyrrhotite quartz Sphene Epidote Calcite content(%) 1.22 1.22 0.59 0.40 0.31 0.22 0.21 Mineral Name Chalcopyrite Other minerals content(%) 0.01 1.32
[0089] like Figure 1 As shown, the above-mentioned mineral processing method comprises:
[0090] S1. The vanadium-titanium magnetite ore (ie, the raw ore) is crushed by a jaw crusher and then sieved to obtain a medium-crushed ore with a particle size of -12.0 mm and a first medium ore with a particle size of +12.0 mm; wherein the first medium ore is returned to the medium crushing step;
[0091] S2. The medium ore is crushed by a high pressure roller mill and then sieved to obtain a crushed ore with a particle size of -3.0 mm and a second medium ore with a particle size of +3.0 mm; wherein the second medium ore is returned to the fine crushing step;
[0092] S3. The crushed ore is dry-discarded, and the magnetic field strength is 7000Oe to obtain dry-discarded concentrate and dry-discarded tailings;
[0093] S4. The dry tailings are wet-discarded, and the magnetic field strength is 7000Oe to obtain wet-discarded concentrate and rough-discarded tailings; wherein the dry-discarded concentrate and the wet-discarded concentrate are combined into a rough-discarded concentrate;
[0094] S5. Grinding the coarse concentrate with a rod mill to obtain a first grinding product; wherein the mass percentage of the mineral having a particle size of -0.074 mm in the first grinding product is 40%;
[0095] S6. The first grinding product is subjected to a wet weak magnetic separation with a magnetic field strength of 2000Oe to obtain a weak magnetic separation concentrate and a weak magnetic separation tailings;
[0096] S7. A rod mill is used to grind a weak magnetic separation concentrate to obtain a second grinding product; wherein the mass percentage of the mineral with a particle size of -0.074 mm in the second grinding product is 64.09%;
[0097] S8. The second grinding product is subjected to a two-stage wet weak magnetic separation with a magnetic field strength of 1500Oe to obtain an iron concentrate and a two-stage weak magnetic separation tailing; wherein the first stage weak magnetic separation tailing and the second stage weak magnetic separation tailing are combined into an iron separation tailing;
[0098] S9. The iron ore tailings are subjected to a first strong magnetic separation, with a magnetic field strength of 8000 Oe, to obtain a first strong magnetic separation concentrate and a first strong magnetic separation tailings;
[0099] S10. The first high-frequency vibrating screen and hydrocyclone are used to classify the concentrate to obtain coarse sand with a particle size of +0.074 mm and fine mud with a particle size of -0.074 mm;
[0100] S11. A spiral chute is used to perform a first stage of gravity separation on the coarse sand to obtain a first stage of gravity separation concentrate and a first stage of gravity separation tailings;
[0101] S12. The first stage gravity separation tailings are subjected to second stage gravity separation using a spiral chute to obtain a second stage gravity separation concentrate and gravity separation tailings; wherein the first stage gravity separation concentrate and the second stage gravity separation concentrate are combined into a gravity separation concentrate;
[0102] S13. The fine mud is subjected to a strong magnetic separation with a magnetic field strength of 6000Oe to obtain a strong magnetic separation concentrate and a strong magnetic separation tailings;
[0103] S14. The first stage strong magnetic separation concentrate is subjected to a second stage strong magnetic separation, and the magnetic field strength is 4000Oe to obtain a second stage strong magnetic separation concentrate and a second stage strong magnetic separation tailings; wherein the gravity separation concentrate and the second stage strong magnetic separation concentrate are combined into a floating material; the first stage strong magnetic separation tailings and the second stage strong magnetic separation tailings are combined into the second stage strong magnetic separation tailings;
[0104] S15. The floating material is floated to obtain sulfur concentrate, titanium concentrate and flotation tailings; wherein the first strong magnetic separation tailings, gravity separation tailings, second strong magnetic separation tailings and flotation tailings are combined into total tailings; the reagents used in flotation include sulfuric acid 4400g / t·feed, butyl xanthate 100g / t·feed, 2 # Oil 21g / t·feed, diesel 200g / t·feed, sodium fluorosilicate 350g / t·feed and fatty acid collector (i.e., MOH and styrenephosphonic acid in a mass ratio of 4:1) 4400g / t·feed; flotation includes flotation desulfurization and flotation titanium, and flotation titanium includes flotation roughing, flotation scavenging and flotation concentration; the number of flotation desulfurization is 1 time; the number of flotation roughing is 1 time, the number of flotation scavenging is 1 time, and the number of flotation concentration is 4 times.
[0105] The results show that in the ore dressing method of this embodiment, the yield of iron concentrate is 9.37%, the grade of TFe is 60.18%, and the recovery rate of TFE is 40.11%; the yield of titanium concentrate is 3.56%, and the grade of TiO 2 The grade is 47.13%, TiO 2 The recovery rate is 37.09%. Therefore, the ore dressing method of this embodiment achieves effective recovery of iron and titanium in low-grade vanadium-titanium magnetite.
[0106] Example 3
[0107] This embodiment provides a beneficiation method for recovering iron and titanium from low-grade vanadium-titanium magnetite, so as to recover iron and titanium from a vanadium-titanium magnetite ore, wherein the grade of TFE in the vanadium-titanium magnetite ore is 15.54%, and the grade of TiO 2 The grade is 5.05%, and the quantitative results of its main minerals are shown in Table 3.
[0108] Table 3 Main mineral composition and content of raw ore comprehensive sample
[0109] Mineral Name Pyroxene Titanomagnetite Biotite Sodium feldspar Chlorite Hornblende Ilmenite content(%) 57.69 13.44 8.86 5.08 4.20 3.56 2.23 Mineral Name Calcite Sphene Potassium feldspar apatite quartz Pyrite Illite content(%) 1.36 1.74 0.54 0.28 0.25 0.24 0.20 Mineral Name Epidote Chalcopyrite Peridot Pyrrhotite Nickel-cobalt minerals Zircon Other minerals content(%) 0.168 0.12 0.016 0.007 0.005 0.001 0.015
[0110] like Figure 1 As shown, the above-mentioned mineral processing method comprises:
[0111] S1. The vanadium-titanium magnetite ore (ie, the raw ore) is crushed by a jaw crusher and then sieved to obtain a medium-crushed ore with a particle size of -12.0 mm and a first medium ore with a particle size of +12.0 mm; wherein the first medium ore is returned to the medium crushing step;
[0112] S2. The medium ore is crushed by a high pressure roller mill and then sieved to obtain a crushed ore with a particle size of -3.0 mm and a second medium ore with a particle size of +3.0 mm; wherein the second medium ore is returned to the fine crushing step;
[0113] S3. The crushed ore is dry-discarded, and the magnetic field strength is 4500Oe to obtain dry-discarded concentrate and dry-discarded tailings;
[0114] S4. The dry tailings are wet-discarded, and the magnetic field strength is 4500Oe to obtain wet-discarded concentrate and rough-discarded tailings; wherein the dry-discarded concentrate and the wet-discarded concentrate are combined into a rough-discarded concentrate;
[0115] S5. The coarse concentrate is ground by a rod mill to obtain a first grinding product; wherein the mass percentage of the mineral having a particle size of -0.074 mm in the first grinding product is 48.8%;
[0116] S6. The first grinding product is subjected to a wet weak magnetic separation with a magnetic field strength of 2000Oe to obtain a weak magnetic separation concentrate and a weak magnetic separation tailings;
[0117] S7. A rod mill is used to grind a weak magnetic separation concentrate to obtain a second grinding product; wherein the mass percentage of the mineral having a particle size of -0.074 mm in the second grinding product is 84%;
[0118] S8. The second grinding product is subjected to a two-stage wet weak magnetic separation with a magnetic field strength of 2000Oe to obtain an iron concentrate and a two-stage weak magnetic separation tailing; wherein the first stage weak magnetic separation tailing and the second stage weak magnetic separation tailing are combined into an iron separation tailing;
[0119] S9. The iron ore tailings are subjected to a first strong magnetic separation, with a magnetic field strength of 6000 Oe, to obtain a first strong magnetic separation concentrate and a first strong magnetic separation tailings;
[0120] S10. The first high-frequency vibrating screen and hydrocyclone are used to classify the concentrate to obtain coarse sand with a particle size of +0.074 mm and fine mud with a particle size of -0.074 mm;
[0121] S11. A spiral chute is used to perform a first stage of gravity separation on the coarse sand to obtain a first stage of gravity separation concentrate and a first stage of gravity separation tailings;
[0122] S12. The first stage gravity separation tailings are subjected to second stage gravity separation using a spiral chute to obtain a second stage gravity separation concentrate and gravity separation tailings; wherein the first stage gravity separation concentrate and the second stage gravity separation concentrate are combined into a gravity separation concentrate;
[0123] S13. The fine mud is subjected to a strong magnetic separation with a magnetic field strength of 6000Oe to obtain a strong magnetic separation concentrate and a strong magnetic separation tailings;
[0124] S14. The first stage strong magnetic separation concentrate is subjected to a second stage strong magnetic separation, and the magnetic field strength is 4000Oe to obtain a second stage strong magnetic separation concentrate and a second stage strong magnetic separation tailings; wherein the gravity separation concentrate and the second stage strong magnetic separation concentrate are combined into a floating material; the first stage strong magnetic separation tailings and the second stage strong magnetic separation tailings are combined into the second stage strong magnetic separation tailings;
[0125] S15. The floating material is floated to obtain sulfur concentrate, titanium concentrate and flotation tailings; wherein the first strong magnetic separation tailings, gravity separation tailings, second strong magnetic separation tailings and flotation tailings are combined into total tailings; the reagents used in flotation include sulfuric acid 4800g / t·feed, butyl xanthate 100g / t·feed, 2 # Oil 60g / t·feed, diesel 300g / t·feed, sodium fluorosilicate 700g / t·feed and fatty acid collector (i.e., MOH and styrenephosphonic acid in a mass ratio of 4:1) 3400g / t·feed; flotation includes flotation desulfurization and flotation titanium, and flotation titanium includes flotation roughing, flotation scavenging and flotation concentration; the number of flotation desulfurization is 1 time; the number of flotation roughing is 1 time, the number of flotation scavenging is 1 time, and the number of flotation concentration is 4 times.
[0126] The results show that in the ore dressing method of this embodiment, the yield of iron concentrate is 14.03%, the grade of TFe is 55.46%, and the recovery rate of TFE is 50.05%; the yield of titanium concentrate is 3.31%, and the grade of TiO 2 The grade is 46.24%, TiO 2 The recovery rate is 30.31%. Therefore, the ore dressing method of this embodiment achieves effective recovery of iron and titanium in low-grade vanadium-titanium magnetite.
[0127] Comparative Example 1
[0128] Compare the control example 1 with the example 1; wherein, the control example 1 uses the same raw ore as the example 1, and the difference between the control example 1 and the example 2 is that the control example 1 uses the mineral processing method of the example 2 in the Chinese patent document CN201410019663.8.
[0129] The results show that the beneficiation method of comparative example 1 finally obtained an iron concentrate with a yield of 15.42%, a TFe grade of 47.50%, a TFe recovery rate of 56.43%, a yield of 0.42%, and a TiO 2 The grade is 41.23%, TiO 2 The recovery rate is 4.66% of titanium concentrate. It can be seen that compared with the beneficiation method of Example 1, the beneficiation method of Comparative Example 1 has a significantly worse recovery effect on titanium in the raw ore, and the product quality of the obtained iron concentrate and titanium concentrate is low. Therefore, for the recovery of iron and titanium from complex and difficult low-grade vanadium-titanium magnetite, compared with the beneficiation method of Comparative Example 1, the beneficiation method of Example 1 can recover TFe and TiO in the raw ore. 2 Better recovery effect can be achieved with lower grade.
[0130] Comparative Example 2
[0131] Comparison is made between Control Example 2 and Example 1; wherein, Control Example 2 uses the same raw ore as Example 1, and the difference between Control Example 2 and Example 1 is that Control Example 2 uses the mineral processing method of the embodiment in Chinese patent document CN201510605060.0.
[0132] The results show that the beneficiation method of comparative example 2 finally obtained an iron concentrate with a yield of 11.62%, a TFe grade of 55.58%, a TFe recovery rate of 49.76%, a yield of 3.33%, and a TiO 2 The grade is 46.27%, TiO 2 The recovery rate is 41.42% of titanium concentrate. It can be seen that compared with the beneficiation method of Example 1, the beneficiation method of Comparative Example 2 has a significantly worse recovery effect on titanium in the raw ore, and the product quality of the obtained iron concentrate and titanium concentrate is low. Therefore, for the recovery of iron and titanium from complex and difficult low-grade vanadium-titanium magnetite, compared with the beneficiation method of Comparative Example 2, the beneficiation method of Example 1 can recover TFe and TiO in the raw ore. 2 Better recovery effect can be achieved with lower grade.
[0133] Comparative Example 3
[0134] Compare Control Example 3 with Example 1; wherein, Control Example 3 uses the same raw ore as Example 1, and the difference between Control Example 3 and Example 1 is that Control Example 3 uses the mineral processing method of Example 1 in Chinese patent document CN201810619336.4.
[0135] The results show that the beneficiation method of comparative example 3 finally obtained an iron concentrate with a yield of 10.43%, a TFe grade of 53.58%, a TFe recovery rate of 43.05%, a yield of 9.74%, and a TiO 2 The grade is 20.27%, TiO 2 The recovery rate is 53.07% of titanium concentrate. It can be seen that compared with the beneficiation method of Example 1, the product quality of the iron concentrate and titanium concentrate obtained by the beneficiation method of Control Example 3 is significantly reduced, which shows that the beneficiation methods of other types of vanadium-titanium magnetite are not suitable for the complex and difficult to beneficiate low-grade vanadium-titanium magnetite involved in the present disclosure.
[0136] Comparative Example 4
[0137] Comparison is made between Control Example 4 and Example 2; wherein, Control Example 4 uses the same raw ore as Example 2, and the difference between Control Example 4 and Example 2 is that Control Example 4 uses the mineral processing method of the embodiment in Chinese patent document CN201010587892.1.
[0138] The results show that the beneficiation method of Comparative Example 4 finally obtained an iron concentrate with a yield of 11.13%, a TFe grade of 52.58%, and a TFe recovery rate of 45.09%. 2 The grade is 42.16%, TiO 2 The recovery rate is 51.34% of titanium concentrate. It can be seen that compared with the beneficiation method of Example 2, the product quality of the iron concentrate and titanium concentrate obtained by the beneficiation method of Control Example 4 is significantly reduced, which shows that the beneficiation methods of other types of vanadium-titanium magnetite are not suitable for the complex and difficult to beneficiate low-grade vanadium-titanium magnetite involved in the present disclosure.
[0139] Comparative Example 5
[0140] Comparison was made between the control example 5 and the embodiment 1; the difference between the control example 5 and the embodiment 1 is as follows:
[0141] 1) Delete S3~S4;
[0142] 2) S5 is replaced by: grinding the crushed ore with a rod mill to obtain a first grinding product; wherein the mass percentage of minerals with a particle size of -0.074 mm in the first grinding product is 50%;
[0143] Other conditions such as the selection of raw ore, the selection and dosage of reagents, and the remaining process flow and condition parameters are the same as those in Example 1 (compared with Example 1, this control example did not perform dry tailings and wet tailings, which is used to prove that the mineral processing method disclosed in the present invention is more effective).
[0144] The results show that the beneficiation method of comparative example 5 finally obtained an iron concentrate with a yield of 9.12%, a TFe grade of 61.26%, a TFe recovery rate of 43.04%, a yield of 3.48%, and a TiO 2 The grade is 46.97%, TiO 2 The recovery rate of titanium concentrate is 43.94%. In this regard, it should be understood that, under normal circumstances, the additional addition of tailings will lead to a decrease in recovery rate. However, compared with the beneficiation method of Example 1, the yield, grade and recovery rate of the iron concentrate and titanium concentrate obtained by the beneficiation method of Control Example 5 are not significantly different, which shows that the beneficiation method of Example 1 can reduce the amount of grinding while ensuring the beneficiation index, thereby reducing the beneficiation cost.
[0145] Comparative Example 6
[0146] Comparison was made between the control example 6 and the embodiment 1; the difference between the control example 6 and the embodiment 1 was as follows:
[0147] 1) Delete S4;
[0148] 2) Replace S3 with: dry tailings are discarded on the crushed ore, and the magnetic field strength is 5000Oe to obtain rough discard concentrate and rough discard tailings;
[0149] Other conditions such as the selection of raw ore, the selection and dosage of reagents, and the remaining process flow and condition parameters are the same as those in Example 1 (compared with Example 1, this control example did not perform wet tailings discarding to prove that the mineral processing method disclosed in the present invention is more effective).
[0150] The results show that the beneficiation method of comparative example 6 finally obtained an iron concentrate with a yield of 9.15%, a TFe grade of 61.33%, a TFe recovery rate of 43.23%, a yield of 3.19%, and a TiO 2 The grade is 46.67%, TiO 2 The recovery rate of titanium concentrate is 40.02%. It can be seen that compared with the beneficiation method of Example 1, the yield of iron concentrate obtained by the beneficiation method of Comparative Example 6, as well as the grade and recovery rate of TFe therein, have no significant difference, but the TiO in the obtained titanium concentrate is 2 The recovery rate of TiO in titanium concentrate decreased, which shows that wet tailing after dry tailing can increase the recovery of TiO in titanium concentrate. 2 recovery rate, thereby reducing the loss of titanium.
[0151] Comparative Example 7
[0152] Comparison was made between Reference Example 7 and Example 1; the difference between Reference Example 7 and Example 1 was as follows:
[0153] 1) Replace the coarse sand in S11 with fine mud;
[0154] 2) Replace the fine mud in S13 with coarse sand;
[0155] Other conditions such as the selection of raw ore, the selection and dosage of reagents, and the remaining process flow and condition parameters are the same as those in Example 1 (compared with Example 1, this control example replaces the gravity separation and strong magnetic separation of coarse sand and fine mud with strong magnetic separation and gravity separation of coarse sand and fine mud, respectively, to prove that the mineral processing method disclosed in the present invention is more effective).
[0156] The results show that the beneficiation method of comparative example 7 finally obtained an iron concentrate with a yield of 9.17%, a TFe grade of 61.27%, a TFe recovery rate of 43.29%, a yield of 3.71%, and a TiO 2 The grade is 39.84%, TiO 2 The recovery rate of titanium concentrate is 39.73%. It can be seen that compared with the ore dressing method of Example 1, the titanium concentrate obtained by the ore dressing method of Comparative Example 7 contains more TiO 2The grade and recovery rate of titanium ore decreased significantly, which shows that the strong magnetic separation and gravity separation of coarse sand and fine mud respectively will reduce the pre-enrichment effect of titanium, thus affecting the quality of titanium concentrate.
[0157] Therefore, the present invention provides a beneficiation method for recovering iron and titanium from low-grade vanadium-titanium magnetite, which is suitable for complex and difficult to select low-grade vanadium-titanium magnetite, and at least achieves the effect of not only maximizing the recovery and utilization of the valuable elements iron and titanium, but also improving the grade and recovery rate of the resulting concentrate.
[0158] The above is only a preferred embodiment of the present disclosure. It should be understood that the present disclosure is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not deviate from the spirit and scope of the present disclosure, and should be within the scope of protection of the claims attached to the present disclosure.
Claims
1. A beneficiation method for recovering iron and titanium from low-grade vanadium-titanium magnetite, characterized in that: include: Crushing low-grade vanadium-titanium magnetite ore to obtain crushed ore; The crushed ore is subjected to tailings discarding to obtain rough discarding concentrate and rough discarding tailings; Grinding and weak magnetic separation are performed on the rough cast concentrate to obtain iron concentrate and iron tailings; Performing a first high-intensity magnetic separation on the iron ore tailings to obtain a first high-intensity magnetic separation concentrate and a first high-intensity magnetic separation tailings; Classifying the first high-intensity magnetic separation concentrate to obtain coarse sand and fine mud; Gravity separation is performed on the coarse sand to obtain gravity separation concentrate and gravity separation tailings; Performing second high intensity magnetic separation on the fine mud to obtain second high intensity magnetic separation concentrate and second high intensity magnetic separation tailings; as well as The gravity separation concentrate and the second high-intensity magnetic separation concentrate are combined and flotation is performed to obtain sulfur concentrate, titanium concentrate and flotation tailings.
2. The ore dressing method according to claim 1, characterized in that: The grade of TiO2 in the low-grade vanadium-titanium magnetite ore is 3.5% to 5.5%.
3. The ore dressing method according to claim 1, characterized in that: The method of crushing the low-grade vanadium-titanium magnetite ore to obtain crushed ore comprises: The low-grade vanadium-titanium magnetite ore is subjected to secondary crushing and first screening to obtain secondary crushed ore and first intermediate ore; wherein the first intermediate ore is returned to the secondary crushing; and The medium-crushed ore is subjected to fine crushing and second screening to obtain the crushed ore and second medium ore; wherein the second medium ore is returned to the fine crushing.
4. The ore dressing method according to claim 1, characterized in that: The method of discarding the tailings of the crushed ore to obtain rough discard concentrate and rough discard tailings includes: Performing dry tailings dumping on the crushed ore to obtain dry tailings dumping concentrate and dry tailings dumping; and The dry-throw tailings are wet-thrown to obtain wet-throw concentrate and the rough-throw tailings; wherein the dry-throw concentrate and the wet-throw concentrate are combined into the rough-throw concentrate.
5. The ore dressing method according to claim 1, characterized in that: The method of grinding and weak magnetic separation the rough concentrate to obtain iron concentrate and iron tailings comprises: Performing a first grinding on the rough ore concentrate to obtain a first grinding product; The first grinding product is subjected to a first stage of weak magnetic separation to obtain a first stage of weak magnetic separation concentrate and a first stage of weak magnetic separation tailings; performing a second grinding on the first stage weak magnetic separation concentrate to obtain a second grinding product; and The second grinding product is subjected to two-stage weak magnetic separation to obtain the iron concentrate and two-stage weak magnetic separation tailings; wherein the one-stage weak magnetic separation tailings and the two-stage weak magnetic separation tailings are combined into the iron separation tailings.
6. The ore dressing method according to claim 1, characterized in that: The magnetic field strength of the first strong magnetic separation is 6000-9000 Oe; and / or the particle size of the coarse sand is +0.074 mm, and the particle size of the fine mud is -0.074 mm.
7. The ore dressing method according to claim 1, characterized in that: The method of re-selecting the coarse sand to obtain re-selected concentrate and re-selected tailings comprises: Performing a first stage of gravity separation on the coarse sand to obtain a first stage of gravity separation concentrate and a first stage of gravity separation tailings; and The first stage gravity separation tailings are subjected to second stage gravity separation to obtain second stage gravity separation concentrate and the gravity separation tailings; wherein the first stage gravity separation concentrate and the second stage gravity separation concentrate are combined into the gravity separation concentrate.
8. The ore dressing method according to claim 1, characterized in that: The second high-intensity magnetic separation is performed on the fine mud to obtain the second high-intensity magnetic separation concentrate and the second high-intensity magnetic separation tailings, comprising: Performing a stage of high intensity magnetic separation on the fine mud to obtain a stage of high intensity magnetic separation concentrate and a stage of high intensity magnetic separation tailings; and The first-stage high-intensity magnetic separation concentrate is subjected to a second-stage high-intensity magnetic separation to obtain the second-stage high-intensity magnetic separation concentrate and the second-stage high-intensity magnetic separation tailings; wherein the first-stage high-intensity magnetic separation tailings and the second-stage high-intensity magnetic separation tailings are combined into the second high-intensity magnetic separation tailings.
9. The ore dressing method according to claim 1, characterized in that: The flotation includes flotation desulfurization and flotation titanium.
10. The ore dressing method according to claim 1 or 9, characterized in that: The reagents used in the flotation process include sulfuric acid, butyl xanthate, 2 # Oil, diesel, sodium fluorosilicate and fatty acid collectors.
Citation Information
Patent Citations
Beneficiation method for comprehensively using vanadium-bearing titanomagnetite low-grade lean ore and ore below cut-off grade
CN102166542A
Pre-selection method of vanadium titano-magnetite
CN114700157A
Efficient tailing discarding and beneficiation method for surface ore and external ore
CN115970839A
Beneficiation method for recovering ilmenite from total tailings of vanadium titano-magnetite
CN116273446A
Combined inhibitor suitable for high-calcium-magnesium ilmenite as well as preparation method and application of combined inhibitor
CN117138969A
Cited By
Method for discarding tailings before separation of low-grade molybdenum ore
CN119657325A
Method for discarding tailings before low-grade molybdenum ore selection
CN119657325B
Method for efficiently recovering ilmenite from inland river lacustrine facies placer
CN122558633A