Method for avoiding generation of hydrogen sulfide in sulfur flotation process of iron separation tailings and application of method
By using collectors and defoaming agents instead of sulfuric acid in the flotation process of iron dressing tailings, flotation under acid-free conditions is achieved, the problem of hydrogen sulfide gas generation is solved, and the grade and yield of sulfur concentrate are improved. , improving environmental and safety conditions.
Patent Information
- Application Number
- CN202411141007.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-10-15
AI Technical Summary
During the flotation process of iron beneficiation tailings, existing technologies cannot effectively avoid the generation of hydrogen sulfide gas, leading to environmental pollution and safety hazards. Moreover, existing treatment methods mainly focus on terminal treatment rather than solving the problem from the source.
By adding collectors and defoaming agents during the titanium flotation desulfurization process of iron ore dressing tailings, the sulfuric acid is replaced for coarse flotation, selection and sweeping of flotation sulfur, and diesel is used as a collector and defoamer to adjust the pH value of the slurry. , realize flotation under acid-free conditions and avoid the generation of hydrogen sulfide gas.
It realizes that no hydrogen sulfide gas is generated during the flotation process of iron beneficiation tailings, improves the environmental safety of the flotation workshop, improves the grade and yield of sulfur concentrate, and reduces processing costs and complexity.
Smart Images

Figure CN118768081A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mineral processing, and in particular to a method for preventing the generation of hydrogen sulfide in a sulfur flotation process of iron ore tailings and an application thereof. Background Art
[0002] In the flotation process of recovering titanium concentrate from iron ore tailings, flotation desulfurization treatment is generally carried out before titanium flotation to ensure that the sulfur content in the titanium concentrate meets the standard. The desulfurized concentrate will be further sorted to obtain a sulfur concentrate with a sulfur grade of more than 30%, which will be sold as a processing by-product. However, the existing process will produce a large amount of hydrogen sulfide (H2S) gas during the flotation process. Hydrogen sulfide is a toxic and harmful gas with acute toxicity. Inhaling a small amount of high-concentration hydrogen sulfide can be fatal in a short period of time, while low-concentration hydrogen sulfide has effects on the eyes, respiratory system and central nervous system. Therefore, it is necessary to control the hydrogen sulfide gas generated in the industrial flotation section.
[0003] At present, there are many methods for the treatment of hydrogen sulfide industrial gas at home and abroad. These methods are mainly divided into two categories: wet method and dry method. Among them, wet treatment includes wet absorption method and wet oxidation method. The wet absorption method uses an absorbent (such as alkali solution) to absorb hydrogen sulfide gas and then treats the absorption liquid. The wet oxidation method uses an oxidant to oxidize hydrogen sulfide into sulfuric acid, which is then degraded or discharged. The dry treatment methods include iron oxide method, activated carbon method, molecular sieve method, ion exchange method, electron beam irradiation method, membrane separation method, biochemical desulfurization, etc. The iron oxide method oxidizes hydrogen sulfide gas into sulfur by contacting it with iron oxide, thereby achieving the purpose of removing hydrogen sulfide. The activated carbon method uses activated carbon to adsorb hydrogen sulfide gas. The molecular sieve method and ion exchange method use the adsorption properties of specific materials to remove hydrogen sulfide gas. The electron beam irradiation method decomposes hydrogen sulfide into sulfur and hydrogen through the action of electron beams. The membrane separation method uses specific membrane materials to separate hydrogen sulfide gas. Biochemical desulfurization degrades hydrogen sulfide by using specific microorganisms. The above methods for controlling hydrogen sulfide all have certain effects, but these methods all treat or comprehensively utilize hydrogen sulfide gas from the end, and do not solve the problem of hydrogen sulfide gas generation from the source.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The object of the present invention is to provide a method for preventing the generation of hydrogen sulfide in the sulfur flotation process of iron ore tailings and its application.
[0006] The object of the present invention is achieved through the following aspects:
[0007] In the first aspect, the present invention provides a method for avoiding the generation of hydrogen sulfide in the flotation sulfur process of iron ore tailings, comprising flotation titanium desulfurization of iron ore tailings of vanadium-titanium magnetite to obtain a desulfurized concentrate, adding a collector and a defoaming agent to the slurry of the desulfurized concentrate to carry out flotation sulfur roughing to obtain a roughing concentrate and a roughing tailings, adding a collector and a defoaming agent to the roughing concentrate to carry out multiple flotation sulfur selections, and adding a collector to the roughing tailings to carry out scavenging.
[0008] The defoaming agent includes any one of an organosilicon defoaming agent, a polyether defoaming agent, a mineral oil defoaming agent and a silicone oil defoaming agent, the collector is diesel, and the pH value of the slurry of the desulfurized concentrate is 3-6.
[0009] In a second aspect, the present invention provides an application of a method as described in any one of the aforementioned embodiments in preventing the generation of hydrogen sulfide gas during mineral processing.
[0010] The present invention has the following beneficial effects:
[0011] The invention provides a method for avoiding the generation of hydrogen sulfide in the flotation sulfur process of iron ore tailings and its application. The method adopts a collector and a defoamer to replace sulfuric acid as an auxiliary agent in the flotation sulfur roughing, flotation sulfur cleaning and scavenging processes. The defoamer can improve the thickness of the foam in the pulp and adjust the selectivity of the collector, so as to realize the flotation sulfur under acid-free conditions. At the same time, the defoamer selected by the invention is also helpful to improve the pH value of the pulp in the flotation sulfur process, so as to avoid the generation of hydrogen sulfide gas due to too low pH value while improving the sulfur grade, thereby improving the environmental safety of the flotation workshop operation. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0013] Figure 1 This is a flow chart of a method for avoiding the generation of hydrogen sulfide in the sulfur flotation process of iron ore tailings provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0014] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0015] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0016] In the flotation process of recovering ilmenite from iron ore tailings, flotation desulfurization is generally carried out before titanium flotation to ensure that the sulfur content in the titanium concentrate does not exceed the standard. The desulfurized concentrate obtained by flotation desulfurization will be further subjected to flotation sulfur concentration to make the sulfur grade reach more than 30%, so as to be sold as a processing by-product. However, a large amount of hydrogen sulfide (H2S) gas is currently produced during the flotation sulfur process.
[0017] Hydrogen sulfide (H2S) industrial gas is a harmful gas. The presence of hydrogen sulfide not only causes corrosion of equipment and pipelines and catalyst poisoning, but is also a strong neurotoxin that has a strong irritating effect on human mucous membranes, seriously threatening personal safety. It is one of the environmental pollutants that must be eliminated or controlled.
[0018] Hydrogen sulfide is soluble in water. At 0℃, 1 mol of water can dissolve about 2.6 mol of hydrogen sulfide. The aqueous solution of hydrogen sulfide is called hydrosulfuric acid, which is a weak acid. When it is heated, hydrogen sulfide escapes from the water. Hydrogen sulfide is an acute and highly toxic substance. Inhaling a small amount of high-concentration hydrogen sulfide can be fatal in a short period of time; while low-concentration hydrogen sulfide has effects on the eyes, respiratory system and central nervous system.
[0019] According to the hazardous gas control standards for production workshops in my country, the maximum allowable concentration of hydrogen sulfide in the air in the workshop is 10 mg / m 3 The maximum permissible concentration of hydrogen sulfide in the air in a residential environment is 0.0111 mg / m 3 .
[0020] At present, the treatment methods for hydrogen sulfide are to treat or comprehensively utilize hydrogen sulfide gas from the end, and the problem of hydrogen sulfide gas generation is not solved from the source. In the process of sulfur flotation, a large amount of hydrogen sulfide gas will still be produced, and the overall production cost and difficulty of the sulfur flotation process will increase. In addition, after the hydrogen sulfide is treated, the discharge of waste obtained by the treatment will also cause certain environmental pollution. Therefore, how to reduce or avoid the generation of hydrogen sulfide gas during flotation from the source, improve the working environment of the flotation workshop, and at the same time achieve or even exceed the sulfur grade in the existing mineral processing method, is a goal that this field has long wanted to achieve.
[0021] In a first aspect, the present invention provides a method for avoiding the generation of hydrogen sulfide in the flotation sulfur process of iron ore tailings, comprising flotation titanium desulfurization of iron ore tailings of vanadium-titanium magnetite to obtain a desulfurized concentrate, adding a collector and a defoaming agent to the slurry of the desulfurized concentrate instead of sulfuric acid to carry out flotation sulfur roughing to obtain a roughing concentrate and a roughing tailings, further adding a collector and a defoaming agent to the roughing concentrate instead of sulfuric acid to carry out multiple flotation sulfur selections, and adding a collector to the roughing tailings for scavenging.
[0022] The defoaming agent includes any one of an organosilicon defoaming agent, a polyether defoaming agent, a mineral oil defoaming agent and a silicone oil defoaming agent, the collector is diesel, and the pH value of the slurry of the desulfurized concentrate is 3-6.
[0023] Collectors and defoamers are used to replace sulfuric acid as auxiliary agents in the flotation sulfur roughing, flotation sulfur cleaning and scavenging processes, wherein the defoamer can improve the thickness of the foam in the slurry and adjust the selectivity of the collector, thereby achieving flotation sulfur under acid-free conditions and improving the sulfur grade; at the same time, the defoamer selected in the present invention is also helpful to improve the pH value of the slurry during the flotation sulfur process, prevent the generation of hydrogen sulfide gas, and is beneficial to improving the safety of the working environment of the flotation workshop.
[0024] In an optional embodiment, during the flotation sulfur concentration and scavenging concentration, the pH value of the slurry is 3-6.
[0025] Preferably, the concentration of the defoaming agent is 0.5-6%. The concentration of the defoaming agent is the dilution concentration during use.
[0026] Preferably, the collector used is diesel.
[0027] In some embodiments, the present invention provides a method for avoiding the generation of hydrogen sulfide in a sulfur flotation process of iron ore tailings, which comprises the following steps:
[0028] S01. Source of desulfurized concentrate
[0029] In some embodiments, the desulfurized concentrate provided by the present invention is derived from iron ore tailings. The iron ore tailings are subjected to titanium flotation desulfurization to obtain desulfurized concentrate and desulfurized tailings. The desulfurized concentrate is applied to the subsequent flotation sulfur recovery process of the present invention, and the desulfurized tailings directly enter the titanium flotation process.
[0030] S02, floating sulfur roughing
[0031] Collectors and defoamers are added to the slurry of desulfurized concentrate for flotation sulfur roughing to obtain roughing concentrate and roughing tailings. The roughing concentrate is used for flotation sulfur selection, and the roughing tailings are scavenged again. The purpose of scavenging the roughing tailings again is to improve the utilization rate of raw materials and the recovery rate of S element.
[0032] In an optional embodiment, the concentration of the desulfurized concentrate slurry is 20-55%, and the pH value is 3-6.
[0033] In an optional embodiment, during the flotation sulfur roughing process, the mass ratio of the added collector to the dry basis of the desulfurized concentrate is 5-10 g / t, and the mass ratio of the defoaming agent to the dry basis of the desulfurized concentrate is 2-25 g / t.
[0034] Among them, since the raw ore pulp is a desulfurized concentrate obtained by flotation using butyl ammonium black powder as a collector, in an optional embodiment, the ore pulp of the desulfurized concentrate also includes butyl ammonium black powder, and the concentration of butyl ammonium black powder is related to the concentration of sulfur in the raw ore pulp.
[0035] Preferably, the process of re-scavenging the rougher tailings includes: adding a collector to the rougher tailings for scavenging, separating to obtain scavenged concentrate and scavenged tailings, returning the scavenged concentrate to the rougher sulfur floating, and returning the scavenged tailings to the titanium floating desulfurization for titanium floating.
[0036] Therefore, it can be understood that when the scavenged concentrate is returned for flotation sulfur roughing, the raw materials for the subsequent flotation sulfur roughing include the slurry of the desulfurized concentrate and the scavenged concentrate as well as the collector and defoamer.
[0037] When the scavenging tailings are returned for titanium flotation, the raw materials for the titanium flotation desulfurization process in step S01 are iron ore tailings, scavenging tailings and additives for titanium flotation desulfurization.
[0038] Preferably, the pulp concentration of the rougher tailings in the scavenging process is 15-45%, and the mass ratio of the added collector to the dry basis of the desulfurized concentrate is 1-4 g / t.
[0039] S03, Floating Sulfur Selection
[0040] In an optional embodiment, the roughing concentrate is subjected to floating sulfur concentration 2 to 6 times, for example, 2 times, 3 times, 4 times, 5 times or 6 times, and the number of floating sulfur concentration can be determined according to the sulfur grade in the concentrate obtained by floating sulfur concentration.
[0041] Preferably, in order to save costs and ensure that the sulfur grade in the concentrate obtained after floating sulfur concentration, which can be used as a processing by-product, is high, the number of floating sulfur concentration is 3 times. After each floating sulfur concentration, the concentrated concentrate and the concentrated tailings are separated, and the concentrated concentrate separated after the first and second concentrations is subjected to floating sulfur concentration again, and each concentrated tailing is returned to the previous level of mineral processing.
[0042] S031, First Selection
[0043] In an optional embodiment, the first concentration includes subjecting the roughing concentrate to floating sulfur concentration with a collector and a defoamer to obtain a concentrate and a concentrate tailings, and the concentrate tailings are returned to the floating sulfur roughing.
[0044] It is understandable that when the first concentrate tailings are returned to the floating sulfur roughing, the scavenging concentrate should also be returned to the floating sulfur roughing. Therefore, the raw materials for the floating sulfur roughing include the pulp of the desulfurized concentrate, the scavenging concentrate and the first concentrate tailings, as well as the collector and the defoamer. Preferably, the pulp concentration of the roughing concentrate of the first selection is 30-60%, the mass ratio of the added collector to the dry basis of the desulfurized concentrate is 4-7 g / t, and the mass ratio of the defoamer to the dry basis of the desulfurized concentrate is 1-12 g / t.
[0045] S032, Second Selection
[0046] In an optional embodiment, the second concentration includes flotation sulfur concentration of the first concentrate with a collector and a defoamer to obtain a second concentrate and a second tailings, and the second tailings are returned to the first concentration.
[0047] It can be understood that when the secondary concentrate tailings are returned to the first concentration, the raw materials for the first concentration include the slurry of the roughing concentrate and the secondary concentrate tailings as well as the collector and defoamer.
[0048] Preferably, the pulp concentration of the second concentrated concentrate is 30-60%, the mass ratio of the added collector to the dry basis of the desulfurized concentrate is 2-5 g / t, and the mass ratio of the defoaming agent to the dry basis of the desulfurized concentrate is 1-7 g / t.
[0049] S033, The Third Selection
[0050] In an optional embodiment, the third concentration includes flotation sulfur concentration of the refined secondary concentrate with a collector and a defoamer to obtain refined tertiary concentrate and refined tertiary tailings, and the refined tertiary tailings are returned to the second concentration.
[0051] It can be understood that when the three-concentrate tailings are returned to the second concentration, the raw materials for the second concentration include the slurry of the first concentrate and the three-concentrate tailings as well as the collector and defoamer.
[0052] Preferably, the pulp concentration of the third concentrated secondary concentrate is 25-55%, the mass ratio of the added collector to the dry basis of the desulfurized concentrate is 1-3 g / t, and the mass ratio of the defoaming agent to the dry basis of the desulfurized concentrate is 0.3-4 g / t.
[0053] In a second aspect, the present invention provides an application of a method as described in any one of the aforementioned embodiments in reducing the generation of hydrogen sulfide gas during mineral processing.
[0054] Example 1
[0055] This embodiment provides a method for avoiding the generation of hydrogen sulfide in the flotation sulfur process of iron ore tailings. The ore sample used in this embodiment is desulfurized concentrate, including S: 8.67%, TiO2: 11.94%, H2O: 14.67%; the collector is diesel, the defoamer is defoamer DU207 (manufacturer: Dongguan Guozhong New Materials Research Institute Co., Ltd.), and the concentration of the defoamer is 5%. For specific steps, please refer to Figure 1 And the following:
[0056] S01, floating titanium desulfurization
[0057] The iron-separation tailings of vanadium-titanium magnetite are subjected to titanium flotation desulfurization to obtain desulfurized concentrate and desulfurized tailings. The desulfurized concentrate is used in subsequent processes, and the desulfurized tailings directly enter the titanium flotation process.
[0058] S02, floating sulfur roughing
[0059] Weigh 330g of the desulfurized concentrate sample from step S01 and add it to the flotation tank. Then add 300ml of the supernatant after the desulfurized concentrate slurry from the previous process of floating titanium desulfurization into the flotation tank, and stir and beat the slurry to obtain the raw ore slurry for floating sulfur roughing. The slurry concentration is 44.65%, the pH value is 4.24, and the concentration of butyl ammonium black medicine is 100mg / L.
[0060] 6.6 g / t diesel and 20.5 g / t defoamer DU207 were added to the slurry of the desulfurized concentrate to carry out flotation sulfur roughing to obtain roughing concentrate and roughing tailings.
[0061] S03. Add 2.2 g / t diesel to the roughing tailings of step S02 for scavenging, separate the scavenging concentrate and scavenging tailings, return the scavenging concentrate to the starting point of step S02 for floating sulfur roughing, and return the scavenging tailings to floating titanium desulfurization for titanium recovery.
[0062] S04, floating sulfur concentration: The rough concentrate is subjected to floating sulfur concentration three times.
[0063] S041, First Selection
[0064] 6.6 g / t of diesel and 10.25 g / t of defoamer DU207 were added to the roughing concentrate (pH=4.53) in step S02 for the first concentration to obtain the first concentrate and the first concentrate tailings, wherein the first concentrate tailings were returned to the starting point of step S02 for floating sulfur roughing.
[0065] S042, Second Selection
[0066] 4.4 g / t of diesel and 6.83 g / t of defoamer DU207 were added to the first concentrate (pH=4.52) in step S041 for a second concentration to obtain second concentrate and second concentrate tailings, wherein the second concentrate tailings were returned to step S041 for the first concentration.
[0067] S043, The Third Selection
[0068] 2.2 g / t of diesel and 3.42 g / t of defoaming agent DU207 are added to the refined second concentrate (pH=4.53) in step S042 for the third concentration to obtain refined third concentrate and refined third tailings. Among them, the refined third tailings are returned to step S042 for the second concentration. The refined third concentrate is the sulfur concentrate product finally obtained by flotation and can be sold as a processing by-product.
[0069] During the whole flotation process, the pH value in the pulp was monitored in real time by a pH meter, and the H2S gas content in the environment was monitored in real time by a gas meter. The flotation parameters were sorted out as shown in Table 1.
[0070] Table 1 Flotation parameters and H2S content of the method of Example 1
[0071]
[0072]
[0073] As can be seen from Table 1, the method provided by the embodiment of the present invention does not generate hydrogen sulfide gas throughout the whole process, the flotation operation environment is safer, the S grade of the sulfur concentrate is 31.29%, and the S yield is 90.82%.
[0074] Comparative Example 1
[0075] This comparative example provides a method for avoiding the generation of hydrogen sulfide during the flotation sulfur selection process of iron ore tailings. The steps are similar to those of Example 1, with the only difference being that only a defoaming agent is added during the S02 step, the flotation sulfur roughing selection, and the flotation sulfur selection step S04.
[0076] During the entire flotation process, the pH value in the pulp was monitored in real time using an acidity meter, and the H2S gas content in the environment was monitored in real time using a gas meter. The flotation parameters were organized as shown in Table 2.
[0077] Table 2 Flotation parameters and H2S content of the method of comparative example 1
[0078]
[0079] As can be seen from Table 2, the method provided in this comparative example does not generate hydrogen sulfide gas throughout the whole process, the flotation operation environment is safe, the S grade of the concentrate is 31.25%, and the S yield is only 81.40%.
[0080] Comparative Example 2
[0081] This comparative example provides a method for avoiding the generation of hydrogen sulfide during the flotation sulfur selection process of iron ore tailings. The steps are similar to those of Example 1, with the only difference being that only diesel is added during the S02 step, the flotation sulfur roughing selection, and the flotation sulfur selection selection process of the S04 step.
[0082] During the whole flotation process, the pH value in the pulp was monitored in real time by a pH meter, and the H2S gas content in the environment was monitored in real time by a gas meter. The flotation parameters were sorted out as shown in Table 3.
[0083] Table 3 Flotation parameters and H2S content of the method of comparative example 2
[0084]
[0085] As shown in Table 3, the method provided in this comparative example does not generate hydrogen sulfide gas throughout the whole process, the flotation operation environment is safe, the S grade of the concentrate is only 28.86%, the S yield is 92.16%, and the diesel consumption is greatly increased.
[0086] Comparative Example 3
[0087] This comparative example provides a method for avoiding the generation of hydrogen sulfide during the flotation sulfur process of iron ore tailings. The steps are similar to those of Example 1, with the only difference being that during the flotation sulfur roughing process in step S02 and the flotation sulfur concentration process in step S04, the defoaming agent CI-596 is used to replace the defoaming agent DU207.
[0088] During the entire flotation process, the pH value in the pulp was monitored in real time using an acidity meter, and the H2S gas content in the environment was monitored in real time using a gas meter. The flotation parameters were sorted out as shown in Table 4.
[0089] Table 4 Flotation parameters and H2S content of the method of comparative example 3
[0090]
[0091]
[0092] As shown in Table 4, the method provided in this comparative example does not generate hydrogen sulfide gas throughout the whole process, the flotation operation environment is safe, the S grade of the concentrate is 31.25%, the S yield is only 86.21%, and the amount of defoaming agent used is greatly increased.
[0093] Comparative Example 4
[0094] This comparative example provides a method for flotation desulfurization of iron ore tailings with the production of hydrogen sulfide. The steps are similar to those of Example 1, with the only difference being that during the rough flotation sulfur selection in step S02 and the flotation sulfur selection in step S04, sulfuric acid is used to replace the defoaming agent and diesel.
[0095] During the entire flotation process, the pH value in the pulp was monitored in real time using an acidity meter, and the H2S gas content in the environment was monitored in real time using a gas meter. The flotation parameters were organized as shown in Table 5.
[0096] Table 5 Flotation parameters and H2S content of the method of comparative example 4
[0097]
[0098] As can be seen from Table 5, the method provided in this comparative example uses sulfuric acid for flotation, the pH is low, and the amount of hydrogen sulfide gas is large, >200pm, which exceeds the range of the gas detector, affecting the safety of the flotation operation environment and the health of the operators. The S grade of the concentrate is 30.54%, and the S yield is 86.95%.
[0099] Test Example 1
[0100] The sulfur concentrate products obtained by the method of avoiding the production of hydrogen sulfide in the iron ore tailings flotation sulfur process provided in Example 1 and Comparative Examples 1 to 4 were tested for S grade and yield, and the reagent cost of each method was calculated. The reagent cost was calculated based on the desulfurized concentrate desulfurized by titanium flotation, and the results shown in Table 6 were obtained.
[0101] Table 6 Performance and cost evaluation of sulfur concentrate products
[0102] S grade (%) S yield (%) Drug cost (yuan / t) Example 1 31.29 90.82 0.831 Comparative Example 1 31.25 81.40 0.515 Comparative Example 2 28.86 92.16 1.108 Comparative Example 3 31.25 88.21 8.275 Comparative Example 4 30.54 86.95 8.967
[0103] It can be seen from Table 6 that the method of the embodiment of the present invention can improve the grade and yield of sulfur in the sulfur concentrate product, while the reagent cost is low and no hydrogen sulfide gas is generated in the production process. After diesel was omitted in Comparative Example 1, although the reagent cost decreased accordingly, the yield of sulfur in the sulfur concentrate product also decreased significantly. After the defoamer was omitted in Comparative Example 2, although the yield increased, the grade of the concentrate was unqualified and the reagent cost was higher than that of the embodiment. Comparative Example 4 uses CI-596 to replace DU207, and the amount of defoamer is significantly increased, so the cost of the reagent is also significantly increased, and the yield and grade of sulfur are also slightly decreased. Comparative Example 4 uses sulfuric acid to replace diesel and defoamer. The amount of sulfuric acid used is large, the reagent cost is also significantly increased, and the yield and grade of sulfur are also slightly decreased. According to the records in Table 5, this comparative example will also produce a large amount of hydrogen sulfide gas, affecting the flotation working environment.
[0104] A method for preventing the generation of hydrogen sulfide in the flotation sulfur process of iron ore tailings provided in an embodiment of the present invention and its application have at least the following advantages:
[0105] 1. The invention study found that in order to reduce the sulfur content in titanium concentrate, sulfur must be floated before flotation of titanium concentrate, using butyl ammonium black medicine and sulfuric acid as flotation reagents, and sulfuric acid is used in a higher amount as a regulator. Metal sulfides will undergo chemical reactions in an acidic environment to produce hydrogen sulfide gas. The specific chemical equation is: MeS+H2SO4→H2S+MeSO4, where Me is a metal ion. Therefore, it is necessary to optimize the sulfur floating process to ensure the quality of sulfur concentrate while eliminating the harm caused by hydrogen sulfide gas. This is one of the technical problems that are difficult to solve in this field.
[0106] The inventors adopted a method of replacing sulfuric acid with a defoaming agent and diesel in combination, and successfully achieved the goal of eliminating the generation of hydrogen sulfide gas during the flotation sulfur concentration process in conjunction with a "one roughing, one sweeping and three refining" flotation process, thus solving the problem of hydrogen sulfide industrial gas from the source. Compared with terminal treatment or comprehensive utilization methods, the present invention can reduce the treatment cost and complexity of hydrogen sulfide gas.
[0107] 2. Since the method of the present invention does not generate hydrogen sulfide gas during the flotation desulfurization process, it can effectively prevent the occurrence of hydrogen sulfide injuries, protect the health of employees and environmental safety, and improve the working and living environment.
[0108] 3. Compared with wet and dry treatment methods, the method of the present invention does not require the use of absorbents, oxidants, specific materials or microorganisms during the treatment process, thus avoiding technical and environmental issues in the selection of treatment materials and waste disposal.
[0109] 4. While avoiding the generation of hydrogen sulfide gas, the method of the present invention has mild process conditions and is easy to use. While ensuring the yield of sulfur concentrate, it is more efficient and environmentally friendly and can meet industrial production needs.
[0110] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for avoiding the generation of hydrogen sulfide in the flotation sulfur process of iron ore tailings, characterized in that: The method comprises the following steps: desulfurizing the iron tailings of vanadium-titanium magnetite by titanium flotation, obtaining a desulfurized concentrate; adding a collector and a defoamer to the slurry of the desulfurized concentrate for flotation sulfur roughing to obtain a roughing concentrate and a roughing tailing; adding the collector and the defoamer to the roughing concentrate for multiple flotation sulfur selections; and adding the collector to the roughing tailing for scavenging. Wherein, the defoaming agent includes any one of an organosilicon defoaming agent, a polyether defoaming agent, a mineral oil defoaming agent and a silicone oil defoaming agent, and the collector is diesel.
2. The method according to claim 1, characterized in that During the floating sulfur concentration and the scavenging concentration, the pH value of the slurry is 3 to 6; Preferably, the concentration of the defoaming agent is 0.5-6%.
3. The method according to claim 1, characterized in that In the process of flotation sulfur roughing, the concentration of the ore pulp is 20-55%, the mass ratio of the added collector to the dry basis of the desulfurized concentrate is 5-10 g / t, and the mass ratio of the defoaming agent to the dry basis of the desulfurized concentrate is 2-25 g / t.
4. The method according to claim 1, characterized in that: Adding the collector to the roughing tailings for scavenging, separating to obtain scavenging concentrate and scavenging tailings, the scavenging concentrate is returned for the floating sulfur roughing, and the scavenging tailings are returned for floating titanium desulfurization; Preferably, the pulp concentration of the rougher tailings in the scavenging process is 15-45%, and the mass ratio of the added collector to the dry basis of the desulfurized concentrate is 1-4 g / t.
5. The method according to claim 1, characterized in that The floating sulfur concentration is performed three times, and after each floating sulfur concentration, a concentrated ore and a concentrated tailings are separated. The concentrated ore separated after each floating sulfur concentration is subjected to floating sulfur concentration again, and the concentrated tailings are returned to the previous level of mineral processing.
6. The method according to claim 5, characterized in that The first concentration includes subjecting the roughing concentrate to floating sulfur concentration with a collector and a defoamer to obtain a first concentrate and a first concentrate tailings, and the first concentrate tailings are returned to the floating sulfur roughing; Preferably, during the first concentration process, the pulp concentration of the roughing concentrate is 30-60%, the mass ratio of the added collector to the dry basis of the desulfurized concentrate is 4-7 g / t, and the mass ratio of the defoaming agent to the dry basis of the desulfurized concentrate is 1-12 g / t.
7. The method according to claim 6, characterized in that The second concentration includes flotation sulfur concentration of the first concentrate with a collector and a defoamer to obtain a second concentrate and a second concentrate tailings, and the second concentrate tailings are returned to the first concentration; Preferably, during the second concentration process, the pulp concentration of the first concentrate is 30-60%, the mass ratio of the added collector to the dry basis of the desulfurized concentrate is 2-5 g / t, and the mass ratio of the defoaming agent to the pulp of the desulfurized concentrate is 1-7 g / t.
8. The method according to claim 7, characterized in that The third concentration includes flotation sulfur concentration of the refined second concentrate with a collector and a defoamer to obtain a refined third concentrate and a refined third tailings, and the refined third tailings are returned to the second concentration; Preferably, the pulp concentration of the third concentrated secondary concentrate is 25-55%, the mass ratio of the added collector to the dry basis of the desulfurized concentrate is 1-3 g / t, and the mass ratio of the defoaming agent to the dry basis of the desulfurized concentrate is 0.3-4 g / t.
9. The method according to claim 1, characterized in that: The slurry of the desulfurized concentrate also includes butyl ammonium black powder.
10. Use of the method according to any one of claims 1 to 9 in preventing the generation of hydrogen sulfide gas during mineral processing.