High-magnesium aluminum alloy ring piece, preparation method and application
Through the smelting and injection casting of high magnesium alloy combined with homogenization treatment, the problems of long cycle time and cracking in the production process of high magnesium aluminum alloy rings are solved, the efficient preparation and performance improvement of the rings are achieved, and the obtained high magnesium aluminum alloy rings are Has excellent tensile properties and yield.
Patent Information
- Application Number
- CN202410703791.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-10-15
AI Technical Summary
The existing production process of high-magnesium aluminum alloy rings has problems such as long production cycle, complex process, high cost and low material utilization rate. Moreover, the increase in magnesium content causes the ingot to easily crack during pressure processing, affecting the yield.
The aluminum alloy melt is smelted with high magnesium alloy composition and sprayed into the annular mold for cooling and solidification. It is combined with homogenization treatment and aging heat treatment, eliminating the traditional pressure processing and machining links. Through the cooperation of temperature, injection pressure and movement speed, it is formed Dense, fine and uniform grain structure.
It shortens the production process, improves production efficiency, and avoids cracking. The obtained high-magnesium aluminum alloy ring has high longitudinal and transverse tensile ultimate strength and yield strength, dense structure, fine and uniform grains, and excellent tensile properties. higher.
Smart Images

Figure CN118768539A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of aluminum alloy materials for aerospace, and specifically relates to a high-magnesium aluminum alloy ring, a preparation method and an application thereof. Background Art
[0002] Aluminum alloys are widely used in the aerospace field due to their low density, high strength, and good plasticity. With the increasing development of the national aerospace science and technology project, the new generation of launch vehicles has an increasingly urgent need for large-scale overall lightweight materials. High-magnesium aluminum alloys refer to aluminum alloys with a magnesium content between 5% and 10%. Compared with ordinary aluminum alloys, high-magnesium aluminum alloys have lower density, higher strength and hardness, and can better meet the lightweight needs of the aerospace field. At the same time, high-magnesium aluminum alloys also have better strength, better corrosion resistance and excellent thermal properties. Therefore, the research on high-magnesium aluminum alloy materials is a top priority in the field of aluminum alloy materials for aerospace.
[0003] At present, the production process of high-magnesium aluminum alloy rings for aerospace use is mostly smelting → casting → heat treatment → blanking → primary heating → blanking (upsetting, punching) → secondary heating → ring rolling or forging → heat treatment → machining → testing and analysis → finished parts. This process not only has a long production cycle, complex process, high production cost and low material utilization rate, but more importantly, when producing high-magnesium aluminum alloy in this way, the increase in magnesium content not only aggravates the element segregation of the aluminum alloy ingot, but also increases the deformation resistance, making the ingot prone to cracking in the subsequent pressure processing process, thereby greatly reducing the yield rate of high-magnesium aluminum alloy products. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention aims to provide a high-magnesium aluminum alloy ring, a preparation method and an application thereof.
[0005] One of the purposes of the present invention is to provide a method for preparing a high-magnesium aluminum alloy ring, the preparation method comprising:
[0006] S1 firstly melts the alloy according to the high magnesium alloy composition to obtain an aluminum alloy melt;
[0007] S2: the aluminum alloy melt is sprayed from above into the annular mold, the temperature of the aluminum alloy melt is 660-720°C, the spraying pressure is 10-35Kpa, the rotation angular velocity of the annular mold is 10-40° / s, and the aluminum alloy melt is cooled and solidified in the annular mold to obtain an aluminum alloy annular ingot;
[0008] The aluminum alloy annular ingot in S3 is subjected to homogenization treatment and aging heat treatment in sequence to obtain a high-magnesium aluminum alloy ring.
[0009] Preferably, the high magnesium alloy composition includes:
[0010] Si≤0.10%, Fe≤0.12%, Mg 7.4~9.2%, Cu 0~0.6%, Mn 0.4~0.6%, Zn0.4~2.1%, Zr 0.10~0.20%, Sc 0.10~0.20%, other impurities total not more than 0.15%, and the rest is Al.
[0011] Preferably, the smelting temperature is 700-750°C.
[0012] Preferably, step S1 further comprises refining, degassing and filtering the aluminum alloy melt in sequence after smelting to obtain the aluminum alloy melt.
[0013] Preferably, the aluminum alloy melt has a hydrogen content of less than 0.12 ml / 100 gAl, and a slag content of N20≤20K / kg.
[0014] Preferably, a cooling system is provided at the bottom of the annular mold.
[0015] Preferably, the cooling system is a water cooling system, the cooling water temperature is lower than 30°C, and the flow rate is 200-500 L / min.
[0016] Preferably, the aluminum alloy melt is sprayed into the annular mold through a plurality of nozzles, and there is a preset distance between the bottom end of the nozzle and the liquid surface of the aluminum alloy melt in the annular mold, and the preset distance is 100-300 mm.
[0017] Preferably, the plurality of nozzles are arranged radially along the annular mold, the inner diameter of the nozzle increases successively in the direction away from the center of the annular mold, the inner diameter of the nozzle is 2 to 5 mm, and the distance between adjacent nozzles is 5 to 20 mm.
[0018] Preferably, step S2 is performed under an inert atmosphere.
[0019] Preferably, the homogenization treatment includes: first performing a primary treatment and then performing a secondary treatment.
[0020] The primary treatment is to keep the temperature at 400-430°C for 2-4 hours;
[0021] The secondary treatment is to keep the temperature at 440-470°C for 6-12 hours.
[0022] Preferably, the aging heat treatment comprises: keeping the aluminum alloy annular ingot warm at 130-160° C. for 20-30 hours.
[0023] A second object of the present invention is to provide a high-magnesium aluminum alloy ring, which is prepared by the above-mentioned preparation method.
[0024] A third object of the present invention is to provide an application of a high-magnesium aluminum alloy ring, wherein the high-magnesium aluminum alloy ring is used for connecting structural parts of aerospace equipment.
[0025] The beneficial effects of the present invention include:
[0026] The present invention proposes a method for preparing a high-magnesium aluminum alloy ring, including smelting, casting aluminum alloy ring ingots, homogenization and aging heat treatment. During the casting process, the aluminum alloy melt temperature is 660-720°C, the injection pressure is 10-35Kpa, and the annular mold rotation angular velocity is 10-40° / s. On the one hand, the method eliminates the pressure processing and machining links in the traditional ring preparation process, shortens the production process, realizes short-process operation, and improves production efficiency; on the other hand, it can also avoid the cracking phenomenon that is easy to occur in the pressure processing of high-magnesium alloys; thirdly, through the mutual coordination of the aluminum alloy melt temperature, injection pressure and movement speed, the high-magnesium aluminum alloy ring obtained has a dense structure, fine and uniform grains and high tensile properties. The high-magnesium aluminum alloy ring obtained by the present invention has a longitudinal tensile ultimate strength of up to 460.2MPa, a transverse tensile ultimate strength of up to 458.5MPa, a longitudinal tensile yield strength of up to 254MPa, and a transverse tensile yield strength of up to 252.7MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0028] Figure 1 This is a schematic diagram of the printing area of the ring part;
[0029] Figure 2 It is a schematic diagram of the cross section of the printing area of the ring part;
[0030] Figure 3 The ring microstructure diagram obtained for Example 2;
[0031] Figure 4 The ring microstructure diagram obtained for Example 4;
[0032] Figure 5 The ring microstructure diagram obtained for Example 7;
[0033] Figure 6 The ring microstructure diagram was obtained for Comparative Example 1;
[0034] Figure 7 The ring microstructure diagram was obtained for Comparative Example 2;
[0035] Figure 8 The ring microstructure diagram was obtained for Comparative Example 3.
[0036] Icons: 1-nozzle; 2-ring mold; 3-semi-solid aluminum alloy melt; 4-solid aluminum alloy; 5-cooling system; 6-motion platform. DETAILED DESCRIPTION
[0037] According to a first aspect of the present invention, a method for preparing a high-magnesium aluminum alloy ring is provided, the method comprising:
[0038] S1 firstly melts the alloy according to the high magnesium alloy composition to obtain an aluminum alloy melt;
[0039] S2 Figure 1 As shown, the aluminum alloy melt is sprayed from above into the annular mold 2, the temperature of the aluminum alloy melt is 660-720°C, the spraying pressure is 10-35Kpa, the rotation angular velocity of the annular mold is 10-40° / s, and the aluminum alloy melt is cooled and solidified in the annular mold to obtain an aluminum alloy annular ingot;
[0040] The aluminum alloy annular ingot in S3 is subjected to homogenization treatment and aging heat treatment in sequence to obtain a high-magnesium aluminum alloy ring.
[0041] This method eliminates the pressure processing and machining steps in the traditional ring preparation process, avoiding the cracking phenomenon that occurs in high-magnesium alloys during pressure processing. The fluidity of the aluminum alloy melt is enhanced at 660-720°C, the gas dissolution is low, and gas inclusions are avoided to improve the quality, density and surface quality of the casting. The nozzle injection pressure is 10-35Kpa, such as Figure 2 As shown, the aluminum alloy melt sprayed from above impacts the semi-solid aluminum alloy melt 3 in the annular mold below. The impact force provided by the spray pressure can break the dendrites and the second phase in the semi-solid aluminum alloy melt 3, and then when the solid aluminum alloy 4 is formed, its crystal phase structure is finer and more uniform, thereby obtaining an aluminum alloy annular ingot with a fine and uniform structure. While impacting, the mold rotates at a speed of 10 to 40° / s, which can ensure the stability of the liquid supply and ensure that the two layers of melt are combined in the semi-solid state to obtain a ring with good quality.
[0042] Through the coordination of temperature, injection pressure and movement speed, it can be ensured that the previous layer of aluminum alloy melt is combined with the next layer of aluminum alloy melt in a semi-solid state, with good interface bonding strength and obvious impact effect, so that the high-magnesium aluminum alloy material has a dense structure, fine and uniform grains and high tensile properties.
[0043] In the present invention, the aluminum alloy melt is sprayed into the annular mold through a nozzle, and the spraying pressure is, for example, 10Kpa, 15Kpa, 20Kpa, 25Kpa, 30Kpa or 35Kpa.
[0044] In the present invention, if Figure 2 As shown, a moving platform 6 is provided below the annular mold to drive the mold to rotate. The annular mold rotation angular velocity is, for example, 10° / s, 15° / s, 20° / s, 25° / s, 30° / s, 35° / s or 40° / s. The aluminum alloy melt temperature is, for example, 660°C, 670°C, 680°C, 690°C, 700°C, 710°C or 720°C.
[0045] In a preferred embodiment of the present invention, the high magnesium alloy composition includes:
[0046] Si≤0.10%, Fe≤0.12%, Mg 7.4~9.2%, Cu 0~0.6%, Mn 0.4~0.6%, Zn0.4~2.1%, Zr 0.10~0.20%, Sc 0.10~0.20%, other impurities total not more than 0.15%, and the rest is Al.
[0047] The high-magnesium aluminum alloy prepared by the present invention refers to an aluminum alloy in which the content of the main alloying element Mg is increased and a certain amount of Zn and Mn elements are added, thereby ensuring the strengthening effect of the alloy during the subsequent heat treatment process. In addition, by adding microalloying elements Zr and Sc, the grain structure is refined and the strengthening effect is further increased.
[0048] In a preferred embodiment of the present invention, the smelting temperature is 700-750°C.
[0049] In the present invention, a smelting temperature higher than 750°C will cause excessive burning, increase costs, produce oxidation, and reduce quality. The solubility of gases in the air in molten aluminum increases, and gas precipitates during solidification to form bubbles, resulting in waste products. The shrinkage during solidification increases, making it impossible to ensure the density of the structure. A temperature lower than 700°C is not conducive to the dissolution of alloy elements and the discharge of gases and inclusions, and increases the tendency to form segregation, cold shut, and undercasting.
[0050] In the present invention, the melting temperature is, for example, 700°C, 705°C, 710°C, 715°C, 720°C, 725°C, 730°C, 735°C, 740°C, 745°C or 750°C.
[0051] Preferably, step S1 further comprises melt refining, degassing and filtering treatments in sequence after smelting to obtain an aluminum alloy melt.
[0052] Preferably, the aluminum alloy melt has a hydrogen content of less than 0.12 ml / 100 gAl, and a slag content of N20≤20K / kg.
[0053] In the present invention, the slag content refers to that the content of slag with a size greater than 20 microns in each kilogram of aluminum liquid is no more than 20,000.
[0054] In a preferred embodiment of the present invention, Figure 2 As shown, a cooling system 5 is provided at the bottom of the annular mold.
[0055] Preferably, the cooling system is a water cooling system, the cooling water temperature is lower than 30°C, and the flow rate is 200-500 L / min.
[0056] In the present invention, the cooling system is a cooling water pipe arranged below the annular mold 2, and the cooling water flow rate is 200-500L / min. The cooling speed is adjusted by controlling the cooling water flow rate. A flow rate lower than 200L / min results in insufficient cooling intensity, the semi-solid melt 3 is still close to liquid, the number of crystal nuclei is small, and the impact effect is weak, resulting in a coarse ingot structure. A flow rate higher than 500L / min causes the aluminum alloy ingot to cool too quickly, thereby causing excessive internal stress in the structure. At the same time, the semi-solid melt 3 is already close to solid, and the bonding effect with the new melt is poor, and defects such as cold shut are prone to occur.
[0057] In the present invention, the cooling water flow rate is, for example, 200 L / min, 250 L / min, 300 L / min, 350 L / min, 400 L / min, 450 L / min, or 500 L / min.
[0058] In a preferred embodiment of the present invention, Figure 2 As shown, the aluminum alloy melt is sprayed into the annular mold through multiple nozzles 1, and the bottom end of the nozzle 1 has a preset distance from the liquid surface of the aluminum alloy melt in the annular mold, and the preset distance is 100-300 mm.
[0059] Preferably, the preset distance remains fixed during the printing process.
[0060] In the present invention, if the preset distance is less than 100 mm, uneven spraying will occur, splashing will occur, and the surface quality of the ingot will be poor; if the preset distance is greater than 300 mm, the volatilization amount of the aluminum alloy melt during the spraying process will increase, affecting the stability of the ingot composition.
[0061] In the present invention, the preset distance is, for example, 100 mm, 110 mm, 120 mm, 130 mm, 140 mm, 150 mm, 160 mm, 170 mm, 180 mm, 190 mm, 210 mm, 220 mm, 230 mm, 240 mm, 250 mm, 260 mm, 270 mm, 280 mm, 290 mm or 300 mm.
[0062] In a preferred embodiment of the present invention, Figure 1 and Figure 2 As shown, multiple nozzles 1 are arranged radially along the annular mold. To ensure matching of the aluminum alloy melt flow rates between the inner and outer diameters of the annular part, the inner diameter of the nozzle increases successively in the direction away from the center of the annular mold. The inner diameter of the nozzle is 2 to 5 mm, and the distance between adjacent nozzles is 5 to 20 mm.
[0063] In the present invention, when the nozzle diameter is less than 2 mm, the aluminum alloy melt is easily blocked inside the nozzle, affecting the casting continuity; when the nozzle diameter is greater than 5 mm, the flow rate of the aluminum alloy melt will increase, resulting in instability of the aluminum alloy melt during the casting process, resulting in uneven shape or loose structure. In order to meet the annular shape requirements of the casting and ensure the balance of liquid supply at each position, the inner diameter of the nozzle increases in sequence in the direction away from the center of the annular mold, and the distance between adjacent nozzles is equal.
[0064] In the present invention, the nozzle diameter is, for example, 2.0 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm, 2.5 mm, 2.6 mm, 2.7 mm, 2.8 mm, 2.9 mm, 3.0 mm, 3.1 mm, 3.2 mm, 3.3 mm, 3.4 mm, 3.5 mm, 3.6 mm, 3.7 mm, 3.8 mm, 3.9 mm, 4.0 mm, 4.1 mm, 4.2 mm, 4.3 mm, 4.4 mm, 4.5 mm, 4.6 mm, 4.7 mm, 4.8 mm, 4.9 mm or 5.0 mm. The distance between adjacent nozzles is, for example, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, 15 mm, 16 mm, 17 mm, 18 mm, 19 mm or 20 mm.
[0065] In a preferred embodiment of the present invention, step S2 is performed under an inert atmosphere.
[0066] In the present invention, inert gas covers the surface of molten metal during the casting process to avoid oxidation of the metal surface and prevent other impurities, gases or particles from entering the molten metal, so that the structure of the aluminum alloy ingot is dense and uniform, and the purity and surface quality of the metal are maintained. At the same time, the inert gas environment can stabilize the chemical reaction and physical properties of the metal during the casting process, reduce the influence of temperature changes and unstable factors on the quality of the aluminum alloy ingot, and ensure the consistency and stability of the aluminum alloy ingot. The inert gas is, for example, argon or nitrogen.
[0067] In a preferred embodiment of the present invention, the homogenization treatment includes: first performing a primary treatment and then performing a secondary treatment; the primary treatment is to keep warm at 400-430°C for 2-4h; the primary treatment temperature is, for example, 400°C, 410°C, 420°C or 430°C, and the holding time is, for example, 2h, 2.5h, 3h, 3.5h or 4h; the secondary treatment is to keep warm at 440-470°C for 6-12h; the secondary treatment temperature is, for example, 440°C, 450°C, 460°C or 470°C, and the holding time is, for example, 6h, 7h, 8h, 9h, 10h, 11h or 12h.
[0068] In a preferred embodiment of the present invention, the aging heat treatment comprises: keeping the aluminum alloy ring-shaped ingot at 130-160° C. for 20-30 hours. The aging heat treatment temperature is, for example, 130° C., 140° C., 150° C. or 160° C. The holding time is, for example, 20 hours, 22 hours, 24 hours, 26 hours, 28 hours or 30 hours.
[0069] In the present invention, the preparation method of the high magnesium aluminum alloy ring specifically includes:
[0070] S1 smelting: according to the formula of Si≤0.10%, Fe≤0.12%, Mg7.4~9.2%, Cu0~0.6%, Mn0.4~0.6%, Zn0.4~2.1%, Zr0.10~0.20%, Sc0.10~0.20%, other impurities totaling not more than 0.15%, and the rest is Al, smelting is carried out at a smelting temperature of 700~750℃.
[0071] Then, the aluminum is refined, degassed and filtered in sequence, the hydrogen content is controlled within 0.12 ml / 100 gAl, and the slag content N20 ≤ 20 K / kg (the content of slag with a size of > 20 microns is less than 20,000 per kilogram of aluminum liquid).
[0072] S2 casting high magnesium aluminum alloy ring ingot: Figure 2As shown, the aluminum alloy melt enters the annular mold 2 through the nozzle 1, the preset distance between the bottom end of the nozzle 1 and the aluminum alloy melt liquid surface 3 in the lower annular mold is 100-300mm, the injection pressure is 10-35Kpa, and the aluminum alloy melt temperature is 660-720℃. The nozzle diameter is 2-5mm, and the distance between the nozzles is 5-20mm. The annular mold 2 rotates in one direction at an angular velocity of 10-40° / s, and the cooling water flow rate is 200-500L / min. The aluminum alloy melt impacting the mold is cooled and solidified to obtain an aluminum alloy annular ingot.
[0073] S3 homogenization treatment: first carry out primary treatment, keep warm at 400-430℃ for 2-4h, then carry out secondary treatment, keep warm at 440-470℃ for 6-12h.
[0074] S4 aging heat treatment: keep the aluminum alloy ring ingot at 130-160°C for 20-30h.
[0075] After being air-cooled out of the furnace, high-magnesium aluminum alloy rings can be obtained.
[0076] According to a second aspect of the present invention, a high-magnesium aluminum alloy ring is provided. The high-magnesium aluminum alloy ring is prepared by the above-mentioned preparation method.
[0077] According to a third aspect of the present invention, there is provided an application of a high-magnesium aluminum alloy ring as a connecting structural member for aerospace equipment. The high-magnesium aluminum alloy ring is used in key important structural members such as connecting frames, transition rings, adapter frames between rocket compartments, and connecting rings of fuel tanks.
[0078] Example 1
[0079] The preparation of high magnesium aluminum alloy rings includes the following specific steps:
[0080] S1 smelting: according to the formula of Si≤0.10%, Fe≤0.12%, Mg 8.2%, Cu≤0.05, Mn 0.5%, Zn 1.0%, Zr 0.15%, Sc 0.15%, other impurities totaling not more than 0.15%, and the rest being Al, smelting is carried out at a smelting temperature of 730°C.
[0081] The aluminum alloy melt is refined, degassed and filtered, the hydrogen content is controlled within 0.12ml / 100gAl, and the slag content N20≤20K / kg.
[0082] S2 casting high magnesium aluminum alloy ring ingot: Figure 2 As shown, the aluminum alloy melt enters the annular mold 2 through the nozzle 1, the distance between the bottom end of the nozzle 1 and the liquid surface 3 of the aluminum alloy melt in the lower annular mold is 200 mm, the injection pressure is 25 Kpa, and the temperature of the aluminum alloy melt is 660°C.
[0083] The nozzles are set as follows: the nozzle spacing is 10 mm, the number of nozzles is 15, and the nozzles are numbered in sequence in the direction away from the center of the annular mold, wherein the diameters of nozzles No. 1 to 3 are 2.5 mm, the diameters of nozzles No. 4 to 6 are 2.6 mm, the diameters of nozzles No. 7 to 8 are 2.7 mm, the diameters of nozzles No. 9 to 10 are 2.8 mm, the diameters of nozzles No. 11 to 12 are 2.9 mm, and the diameters of nozzles No. 13 to 15 are 3.0 mm. The final specifications of the annular ingot are: outer diameter inner diameter Height 150mm.
[0084] The annular mold rotates in one direction at an angular velocity of 25° / s, the cooling water temperature is 25°C, and the flow rate is 350L / min. The aluminum alloy melt impacting the mold is cooled and solidified to obtain an aluminum alloy annular ingot;
[0085] S3 homogenization treatment: firstly carry out primary treatment at 418℃ for 4h, then carry out secondary treatment at 442℃ for 8h.
[0086] S4 aging heat treatment: keep the ingot at 150℃ for 24h. After air cooling, the high magnesium aluminum alloy ring can be obtained.
[0087] Example 2
[0088] The preparation of high magnesium aluminum alloy rings includes the following specific steps:
[0089] S1 smelting: the steps and parameters are the same as those in Example 1.
[0090] S2 casting of high magnesium aluminum alloy ring ingot: the aluminum alloy melt temperature is 700°C, the injection pressure is 25Kpa, the ring mold angular velocity is 25° / s, and the remaining steps and parameters are consistent with Example 1. The aluminum alloy melt impacting the mold is cooled and solidified to obtain an aluminum alloy ring ingot.
[0091] S3 homogenization treatment: the steps and parameters are the same as those in Example 1.
[0092] S4 aging heat treatment: the steps and parameters are the same as those in Example 1. After the aluminum alloy ring ingot is taken out of the furnace and air-cooled, a high-magnesium aluminum alloy ring can be obtained.
[0093] The microstructure of the aluminum alloy ring obtained in Example 2 is shown in FIG. Figure 3 As shown, Figure 3 (a) is the grain structure diagram, magnified 100 times; Figure 3 (b) is a microstructure diagram, magnified 25 times. Figure 3 It can be seen that the aluminum alloy ring has fine grains and a dense structure, without defects such as cold shut, looseness, and pores.
[0094] Example 3
[0095] The preparation of high magnesium aluminum alloy rings includes the following specific steps:
[0096] The S1 smelting steps and parameters are consistent with those in Example 1.
[0097] S2 casting of high magnesium aluminum alloy ring ingot: the aluminum alloy melt temperature is 720°C, the injection pressure is 25Kpa, the ring mold angular velocity is 25° / s, and the remaining steps and parameters are consistent with Example 1. The aluminum alloy melt impacting the mold is cooled and solidified to obtain an aluminum alloy ring ingot.
[0098] S3 homogenization treatment: the steps and parameters are the same as those in Example 1.
[0099] S4 aging heat treatment: the steps and parameters are the same as those in Example 1. After the aluminum alloy ring ingot is taken out of the furnace and air-cooled, a high-magnesium aluminum alloy ring can be obtained.
[0100] Example 4
[0101] The preparation of high magnesium aluminum alloy rings includes the following specific steps:
[0102] The S1 smelting steps and parameters are consistent with those in Example 1.
[0103] S2 casting of high magnesium aluminum alloy ring ingot: the aluminum alloy melt temperature is 700°C, the injection pressure is 10Kpa, the ring mold angular velocity is 25° / s, and the remaining steps and parameters are consistent with Example 1. The aluminum alloy melt impacting the mold is cooled and solidified to obtain an aluminum alloy ring ingot.
[0104] S3 homogenization treatment: the steps and parameters are the same as those in Example 1.
[0105] S4 aging heat treatment: the steps and parameters are the same as those in Example 1. After the aluminum alloy ring ingot is taken out of the furnace and air-cooled, a high-magnesium aluminum alloy ring can be obtained.
[0106] The microstructure of the aluminum alloy ring obtained in Example 4 is shown in FIG. Figure 4 As shown, Figure 4 (a) is the grain structure diagram, magnified 100 times; Figure 4 (b) is a microstructure diagram, magnified 25 times. Figure 4 It can be seen that the aluminum alloy ring has fine grains and a dense structure, without defects such as cold shut, looseness, and pores.
[0107] Example 5
[0108] The preparation of high magnesium aluminum alloy rings includes the following specific steps:
[0109] The S1 smelting steps and parameters are consistent with those in Example 1.
[0110] S2 casting of high magnesium aluminum alloy ring ingot: the aluminum alloy melt temperature is 700°C, the injection pressure is 35Kpa, the ring mold angular velocity is 25° / s, and the remaining steps and parameters are consistent with Example 1. The aluminum alloy melt impacting the mold is cooled and solidified to obtain an aluminum alloy ring ingot.
[0111] S3 homogenization treatment: the steps and parameters are consistent with those in Example 1.
[0112] S4 aging heat treatment: the steps and parameters are the same as those in Example 1. After the aluminum alloy ring ingot is taken out of the furnace and air-cooled, a high-magnesium aluminum alloy ring can be obtained.
[0113] Example 6
[0114] The preparation of high magnesium aluminum alloy rings includes the following specific steps:
[0115] The S1 smelting steps and parameters are consistent with those in Example 1.
[0116] S2 casting of high magnesium aluminum alloy ring ingot: the aluminum alloy melt temperature is 700°C, the injection pressure is 25Kpa, the ring mold angular velocity is 10° / s, and the remaining steps and parameters are consistent with Example 1. The aluminum alloy melt impacting the mold is cooled and solidified to obtain an aluminum alloy ring ingot.
[0117] S3 homogenization treatment: the steps and parameters are consistent with those in Example 1.
[0118] S4 aging heat treatment: the steps and parameters are the same as those in Example 1. After the aluminum alloy ring ingot is taken out of the furnace and air-cooled, a high-magnesium aluminum alloy ring can be obtained.
[0119] Example 7
[0120] The preparation of high magnesium aluminum alloy rings includes the following specific steps:
[0121] The S1 smelting steps and parameters are consistent with those in Example 1.
[0122] S2 casting of high magnesium aluminum alloy ring ingot: the aluminum alloy melt temperature is 700°C, the injection pressure is 25Kpa, the ring mold angular velocity is 40° / s, and the remaining steps and parameters are consistent with Example 1. The aluminum alloy melt impacting the mold is cooled and solidified to obtain an aluminum alloy ring ingot.
[0123] S3 homogenization treatment: the steps and parameters are consistent with those in Example 1.
[0124] S4 aging heat treatment: the steps and parameters are the same as those in Example 1. After the aluminum alloy ring ingot is taken out of the furnace and air-cooled, a high-magnesium aluminum alloy ring can be obtained.
[0125] The microstructure of the aluminum alloy ring obtained in Example 7 is shown in FIG. Figure 5 As shown, Figure 5(a) is the grain structure diagram, magnified 100 times; Figure 5 (b) is a microstructure diagram, magnified 25 times. Figure 5 It can be seen that the aluminum alloy ring has fine grains and a dense structure, without defects such as cold shut, looseness, and pores.
[0126] Comparative Example 1
[0127] The preparation of high magnesium aluminum alloy rings includes the following specific steps:
[0128] The S1 smelting steps and parameters are consistent with those in Example 1.
[0129] S2 casting of high magnesium aluminum alloy ring ingot: the aluminum alloy melt temperature is 750°C, the injection pressure is 25Kpa, the ring mold angular velocity is 25° / s, and the remaining steps and parameters are consistent with Example 1. The aluminum alloy melt impacting the mold is cooled and solidified to obtain an aluminum alloy ring ingot.
[0130] S3 homogenization treatment: the steps and parameters are consistent with those in Example 1.
[0131] S4 aging heat treatment: the steps and parameters are the same as those in Example 1. After the aluminum alloy ring ingot is taken out of the furnace and air-cooled, a high-magnesium aluminum alloy ring can be obtained.
[0132] The microstructure of the aluminum alloy ring obtained in Comparative Example 1 is shown in FIG. Figure 6 As shown, Figure 6 (a) is the grain structure diagram, magnified 100 times; Figure 6 (b) is a microstructure diagram, magnified 25 times. Figure 6 It can be seen that the grains of the aluminum alloy rings have become coarser, the density of the organizational structure is poor, and there are a large number of loose defects, which seriously affect the performance of the rings.
[0133] Comparative Example 2
[0134] The preparation of high magnesium aluminum alloy rings includes the following specific steps:
[0135] The S1 smelting steps and parameters are consistent with those in Example 1.
[0136] S2 casting of high magnesium aluminum alloy ring ingot: the aluminum alloy melt temperature is 700°C, the injection pressure is 5Kpa, the ring mold angular velocity is 5° / s, and the remaining steps and parameters are consistent with Example 1. The aluminum alloy melt impacting the mold is cooled and solidified to obtain an aluminum alloy ring ingot.
[0137] S3 homogenization treatment: the steps and parameters are consistent with those in Example 1.
[0138] S4 aging heat treatment: the steps and parameters are the same as those in Example 1. After the aluminum alloy ring ingot is taken out of the furnace and air-cooled, a high-magnesium aluminum alloy ring can be obtained.
[0139] The microstructure of the aluminum alloy ring obtained in Comparative Example 2 is shown in FIG. Figure 7 As shown, Figure 7 (a) is the grain structure diagram, magnified 100 times; Figure 7 (b) is a microstructure diagram, magnified 25 times. Figure 7 It can be seen that the aluminum alloy ring has fine grains, but poor structural density and a large number of cold shut defects, which seriously affect the performance of the ring.
[0140] Comparative Example 3
[0141] The preparation of high magnesium aluminum alloy rings includes the following specific steps:
[0142] The S1 smelting steps and parameters are consistent with those in Example 1.
[0143] S2 casting of high magnesium aluminum alloy ring ingot: the aluminum alloy melt temperature is 700°C, the injection pressure is 40Kpa, the ring mold angular velocity is 50° / s, and the remaining steps and parameters are consistent with Example 1. The aluminum alloy melt impacting the mold is cooled and solidified to obtain an aluminum alloy ring ingot.
[0144] S3 homogenization treatment: the steps and parameters are the same as those in Example 1.
[0145] S4 aging heat treatment: the steps and parameters are the same as those in Example 1. After the aluminum alloy ring ingot is taken out of the furnace and air-cooled, a high-magnesium aluminum alloy ring can be obtained.
[0146] The microstructure of the aluminum alloy ring obtained in Comparative Example 3 is shown in FIG. Figure 8 As shown, Figure 8 (a) is the grain structure diagram, magnified 100 times; Figure 8 (b) is a microstructure diagram, magnified 25 times. Figure 8 It can be seen that the aluminum alloy ring has coarse grains, poor structural density, and a large number of loose defects, which seriously affect the performance of the ring.
[0147] Performance Testing
[0148] The tensile properties of the product were tested in accordance with the national standard GB / T 228.1-2010. Table 1 shows the tensile properties test data of Examples 1 to 7 and Comparative Examples 1 to 3.
[0149] Table 1 Tensile properties test of Examples 1 to 7 and Comparative Examples 1 to 3
[0150]
[0151]
Claims
1. A method for preparing a high-magnesium aluminum alloy ring, characterized in that: The preparation method comprises: S1 firstly melts the alloy according to the high magnesium alloy composition to obtain an aluminum alloy melt; S2: the aluminum alloy melt is sprayed from above into the annular mold, the temperature of the aluminum alloy melt is 660-720°C, the spraying pressure is 10-35Kpa, the rotation angular velocity of the annular mold is 10-40° / s, and the aluminum alloy melt is cooled and solidified in the annular mold to obtain an aluminum alloy annular ingot; The aluminum alloy annular ingot in S3 is subjected to homogenization treatment and aging heat treatment in sequence to obtain a high-magnesium aluminum alloy ring.
2. The method for preparing a high magnesium aluminum alloy ring according to claim 1, characterized in that: The high magnesium alloy composition includes: Si≤0.10%, Fe≤0.12%, Mg 7.4~9.2%, Cu 0~0.6%, Mn 0.4~0.6%, Zn0.4~2.1%, Zr 0.10~0.20%, Sc 0.10~0.20%, other impurities total not more than 0.15%, and the rest is Al.
3. The method for preparing a high magnesium aluminum alloy ring according to claim 1, characterized in that: The smelting temperature is 700-750°C; Preferably, step S1 further comprises melt refining, degassing and filtering in sequence after smelting to obtain an aluminum alloy melt; Preferably, the aluminum alloy melt has a hydrogen content of less than 0.12 ml / 100 gAl, and a slag content of N20≤20K / kg.
4. The method for preparing a high magnesium aluminum alloy ring according to claim 1, characterized in that: A cooling system is provided at the bottom of the annular mold; Preferably, the cooling system is a water cooling system, the cooling water temperature is lower than 30°C, and the flow rate is 200-500 L / min.
5. The method for preparing a high magnesium aluminum alloy ring according to claim 1, characterized in that: The aluminum alloy melt is sprayed into the annular mold through a plurality of nozzles, and there is a preset distance between the bottom end of the nozzle and the liquid surface of the aluminum alloy melt in the annular mold, and the preset distance is 100-300 mm.
6. The method for preparing a high magnesium aluminum alloy ring according to claim 5, characterized in that: The plurality of nozzles are arranged radially along the annular mold, the inner diameter of the nozzle increases successively in the direction away from the center of the annular mold, the inner diameter of the nozzle is 2 to 5 mm, and the distance between adjacent nozzles is 5 to 20 mm.
7. The method for preparing a high magnesium aluminum alloy ring according to claim 1, characterized in that: Step S2 is performed under an inert atmosphere.
8. The method for preparing a high magnesium aluminum alloy ring according to claim 1, characterized in that: The homogenization treatment includes: firstly performing a primary treatment and then performing a secondary treatment; The primary treatment is to keep the temperature at 400-430°C for 2-4 hours; The secondary treatment is to keep the temperature at 440-470°C for 6-12 hours; Preferably, the aging heat treatment comprises: keeping the aluminum alloy annular ingot warm at 130-160° C. for 20-30 hours.
9. A high-magnesium aluminum alloy ring obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the high-magnesium aluminum alloy ring as claimed in claim 9 as a connecting structural member of aerospace equipment.
Citation Information
Cited By
Aviation aluminum alloy manufacturing device and annular piece preparation method
CN119304150A
Gradient alloy preparation device and method
CN121607610A
Gradient alloy preparation apparatus and method
CN121607610B