Titanium alloy and preparation method and application thereof

By combining hammer forging processing in titanium alloy additive manufacturing, β crystals are converted into equiaxed crystals, which solves the anisotropy problem in titanium alloy additive manufacturing, improves its mechanical properties, and is suitable for the aviation field.

CN118768877AInactive Publication Date: 2024-10-15HUZHOU INST OF ZHEJIANG UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411269083.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Titanium alloys have large anisotropy problems in the additive manufacturing process, resulting in large differences in their mechanical properties in different directions, making it difficult to meet the requirements of the aviation field.

Method used

The hammer forging process is coupled with the arc additive manufacturing process. By performing hammer forging process on each deposition layer, the deposition thickness is controlled to 1~1.5mm, and the original β grains are transformed into equiaxed crystals, thereby weakening the anisotropy of the material. .

Benefits of technology

It significantly increases the proportion of equiaxed crystals in titanium alloys, achieves equiaxed microstructure, improves the comprehensive mechanical properties of titanium alloys, and meets the requirements of the aviation field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118768877A_ABST
    Figure CN118768877A_ABST
Patent Text Reader

Abstract

The invention provides a titanium alloy and a preparation method and application thereof.The preparation method of the titanium alloy comprises the steps that hammering forging treatment and an electric arc additive manufacturing process are coupled, a titanium alloy welding wire serves as a raw material, the titanium alloy is manufactured through the electric arc additive manufacturing process, and in the electric arc additive manufacturing process of the titanium alloy, the titanium alloy is subjected to heat treatment; a hammering and forging device is adopted for conducting synchronous hammering and forging treatment on each deposition layer till the titanium alloy component is machined; in the machining process, the deposition thickness of each deposition layer is controlled to be 1-1.5 mm. According to the method, the volume fraction of titanium alloy original beta grains converted from columnar crystals to isometric crystals is increased, the anisotropy of the material is weakened, and the comprehensive mechanical property of titanium alloy parts or repaired parts formed through electric arc additive manufacturing can meet the use requirements of the aviation field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal additive manufacturing, and in particular to a titanium alloy and a preparation method and application thereof. Background Art

[0002] Titanium alloys have the following characteristics in the aviation field: (1) high strength and lightweight; (2) strong corrosion resistance; (3) good high-temperature performance. These characteristics make titanium alloys an ideal material choice when manufacturing components such as high-temperature engines and jet engines. Although titanium alloys have irreplaceable advantages in the aerospace field, the high cost of raw materials and processing makes large titanium alloy components an obstacle to aerospace development. Traditional production technologies mostly use casting or forging processes, which usually require the manufacture of complex molds and tools, and have long delivery cycles and high installation costs.

[0003] WAAM (Wire Arc Additive Manufacturing) is a type of directional energy deposition (DED) 3D printing technology. It uses wire as raw material and can use gas metal arc welding (GMAW) to deposit precision parts layer by layer, with a deposition rate of up to 4 kg / hour. Compared with traditional manufacturing methods, WAAM technology has low equipment cost, high material utilization, and flexible forming components. It is a more cost-effective and sustainable solution that is easy to achieve automated control and efficient customization of complex parts. In addition, 3D metal printed parts are usually lighter, which can reduce the fuel consumption of aircraft or vehicles, while also increasing the payload of transport vehicles.

[0004] Arc additive technology has the advantages of high deposition rate (about 5 to 10 times that of laser), high material utilization rate (nearly 100%), and low equipment and material manufacturing costs. Due to its high deposition efficiency, it helps to shorten production time and has been favored by scholars at home and abroad. However, the additive manufacturing process is different from the traditional manufacturing method (casting or forging). It uses layer-by-layer stacking and heat accumulation to make the titanium alloy present columnar β crystals instead of equiaxed β crystals. The microstructure is mainly epitaxially grown columnar crystals, and the performance is high-strength and low-plasticity. Therefore, it shows a large difference in mechanical properties in different directions, that is, the material has large anisotropy. As a result, the comprehensive mechanical properties of titanium alloy parts or repair parts formed by arc additive manufacturing are difficult to meet the use requirements. How to control the process parameters to weaken the anisotropy of the material has always been a technical problem in the field of titanium alloy additive manufacturing technology.

[0005] The Chinese patent document discloses "a 700℃ high temperature resistant titanium alloy for aircraft engines and its preparation method", and its publication number is CN 116770130A. The invention designs a traditional solid solution aging strengthened high temperature titanium alloy, which is different from TiB grain boundary enhanced high temperature titanium alloy, TiAl-based, Ti2AlNb-based and other intermetallic compounds. The final organizational state is a dual-state organization, which increases the service temperature range of the traditional solid solution aging strengthened high temperature titanium alloy to 700℃, and can be used as a high temperature component of an aircraft engine under long-term working conditions of 650-700℃. However, the preparation method of the titanium alloy still adopts the traditional ingot smelting process, which has a high processing cost, and needs to change the composition by adding an intermediate alloy, which will change the composition and other properties of the original material to a certain extent, and the introduced alloy elements will produce a certain degree of segregation during the solidification process of the molten pool, which is also difficult to avoid. In the application field with strict requirements on the composition of titanium alloys, this technology of changing the composition of titanium alloys is limited. Summary of the invention

[0006] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a titanium alloy and a preparation method and application thereof, so as to solve the problem that the titanium alloy obtained by the existing additive manufacturing process has large anisotropy.

[0007] To achieve the above-mentioned purpose and other related purposes, the present invention provides a method for preparing titanium alloy, coupling hammer forging treatment with arc additive manufacturing process, using titanium alloy welding wire as raw material, and adopting arc additive manufacturing process to manufacture titanium alloy. During the arc additive manufacturing process of titanium alloy, a hammer forging device is used to synchronously hammer forge each deposition layer until the titanium alloy component is completed; during the processing, the deposition thickness of each deposition layer is controlled to be 1~1.5mm.

[0008] In the above technical solution of the present application, after the metal is deposited by the arc additive manufacturing process, each deposited layer is hammered forged by a hammer forging device to transform the original β grains in the titanium alloy welding wire from columnar crystals to equiaxed crystals. The hammering action produces a large plastic deformation, and huge energy is stored in these deformed metals, which has a significant promoting effect on the next recrystallization to transform columnar crystals into equiaxed crystals, and significantly weakens the anisotropy of the titanium alloy welding wire. The distribution and transformation of equiaxed crystals are related to the plastic deformation area. The present application unexpectedly found that controlling the height of the titanium alloy deposition layer plays a vital role in the equiaxed crystal result, that is, during the processing process, when the deposition thickness of each deposition layer is controlled to be 1~1.5mm, the proportion of equiaxed crystals can be increased, and the equiaxed grains of the microstructure of the titanium alloy manufactured by arc additive manufacturing can be achieved. When the deposition thickness of each deposition layer is too high (such as 3mm), the original β columnar crystals will not be completely transformed into equiaxed crystals; when the deposition thickness of each deposition layer is 1.5~3mm, most of them will be transformed; when the deposition thickness of each deposition layer is controlled to be 1~1.5mm, most of the original β columnar crystals can be transformed into original β equiaxed crystals and secondary β equiaxed crystals.

[0009] More preferably, the hammer forging device adopts an air hammer. The air hammer has a constant hammering pressure, which can ensure the consistency of each hammer forging process.

[0010] Preferably, during the hammer forging process, the force between the hammer forging device and the deposited layer is controlled to be 0.3~0.9MPa. If the force between the hammer forging device and the deposited layer is too small, it is not easy to complete the transformation of the original β grains from columnar crystals to equiaxed crystals. This is because metal materials have elastic regions and plastic regions. If the force is too small and is only within the elastic region, plastic deformation cannot occur, that is, the metal rebounds to its original state after the action. Especially for titanium alloys, the plastic deformation region is at least 600MPa, so a slightly larger force is required; if the force between the hammer forging device and the deposited layer is too large, it will have a great side effect on the life of the equipment, greatly reducing its life, or even destroying it and causing it to break.

[0011] Preferably, during the hammer forging process, the angle between the hammering direction of the hammer forging device and the deposited layer is controlled to be 30-90°.

[0012] Preferably, the number of hammer forging treatments for each deposition layer is controlled to be 2 to 4 times, and the speed of hammer forging treatment is 3 to 5 times / second. Under a certain welding gun moving speed, if the hammer forging treatment is too slow, some areas will not be hammered, that is, the plastic deformation of the area is uneven; if the speed of hammer forging treatment is too fast, higher requirements will be placed on the equipment, and the life of the equipment will be greatly reduced; when the speed of hammer forging treatment is controlled to be 3 to 5 times / second, the effect is better.

[0013] Preferably, during the hammer forging process of each deposited layer, the number of hammer forging processes is at least twice, and the angle between the hammer forging device and the deposited layer includes at least 90° and 45°. Since the weld surface in the process of arc additive manufacturing of titanium alloy is a curved structure, the hammering effect cannot be guaranteed by only using a single hammering direction. Therefore, in addition to vertical hammering, sufficient hammer forging is required in combination with other hammering angles to achieve the equiaxed grains of the microstructure of the arc additive manufacturing titanium alloy.

[0014] Preferably, the process parameters for arc additive manufacturing of titanium alloy are: welding current is 205~250A; voltage is 18~21V, wire feeding speed is 130~200 cm / min, and welding moving speed is 4~6mm / s.

[0015] Preferably, the titanium alloy welding wire is a TC4 welding wire with an oxygen content of less than 0.1%, which can ensure that the titanium alloy has excellent mechanical properties and relatively stable elongation after the welding process, and will not become brittle due to excessive oxygen content and high oxidation degree.

[0016] The present invention also provides a titanium alloy prepared by the above preparation method.

[0017] Preferably, the crystal phase structure of the titanium alloy includes equiaxed crystals and columnar crystals, and the proportion of the equiaxed crystals is not less than 80%. Controlling the height of the titanium alloy deposition layer plays a vital role in the equiaxed crystal result, that is, during the processing, when the deposition thickness of each deposition layer is controlled to be 1-1.5 mm, the proportion of equiaxed crystals can be not less than 80%, and the equiaxed grains of the titanium alloy microstructure manufactured by arc additive manufacturing are achieved.

[0018] The present invention also provides an application of the titanium alloy in the field of aerospace.

[0019] As described above, the titanium alloy and its preparation method and application of the present invention have the following beneficial effects: (1) After depositing the metal using an arc additive manufacturing system, each deposited layer is hammered using a hammer forging device to transform the original β grains in the titanium alloy welding wire from columnar crystals to equiaxed crystals, significantly weakening the anisotropy of the titanium alloy welding wire; (2) The distribution and transformation of equiaxed crystals are related to the plastic deformation zone. Controlling the height of the titanium alloy deposition layer plays a vital role in the equiaxed crystal results. That is, during the processing process, when the deposition thickness of each deposition layer is controlled to be 1-1.5 mm, the proportion of equiaxed crystals can be no less than 80%, thus achieving the equiaxed grains of the titanium alloy microstructure manufactured by arc additive manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1Shown are the optical microscope image (left) and electron backscatter diffraction (EBSD) image (right) of the titanium alloy columnar grains in the single-layer single-channel non-hammer state in Comparative Example 1.

[0021] Figure 2 Shown are the optical microscope image (left) and electron backscatter diffraction (EBSD) image (right) of the equiaxed grains of titanium alloy in the single-layer single-pass hammering state in Example 1.

[0022] Figure 3 It shows an optical microscope image of the columnar grains of titanium alloy in the multi-layer and multi-channel state without hammering in Comparative Example 1.

[0023] Figure 4 It shows an optical microscope image of the equiaxed grains of the titanium alloy in the multi-layer and multi-pass hammering state in Example 1.

[0024] Figure 5 It shows the KAM local plasticity map of the titanium alloy in the single-layer single-channel electron backscatter diffraction (EBSD) state without hammering in Comparative Example 1.

[0025] Figure 6 It shows the KAM local plastic distribution map of the titanium alloy electron backscatter diffraction (EBSD) under single-layer single-channel hammering state in Example 1.

[0026] Figure 7 Shown is the hardness gradient distribution diagram of the titanium alloy prepared in Example 1 (hammered sample) and Comparative Example 1 (non-hammered sample).

[0027] Figure 8 Shown are stress-strain curves of the titanium alloy prepared in Comparative Example 1 in the horizontal and vertical directions without hammering.

[0028] Fig. 9 Shown are stress-strain curves of the titanium alloy prepared in Example 1 in the horizontal and vertical directions under hammering. DETAILED DESCRIPTION

[0029] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0030] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.

[0031] In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in the present invention does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these explicitly mentioned two devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.

[0032] In the following embodiments of the present application, the following equipment is used: Protective gas tray to speed up cooling and prevent oxidation; Welding robots, TIG arc welders and wire feeding systems; Titanium alloy base plate and TC4 welding wire; Welding tooling platform, used to fix the titanium alloy base plate; The air hammer has a constant hammering pressure and is installed on the welding robot, and can hammer according to the posture of the welding robot.

[0033] Example 1 The present invention provides a method for preparing a titanium alloy, comprising the following steps: (1) TC4 welding wire with an oxygen content of less than 0.1% was used as the raw material for arc additive, the TC4 additive substrate was fixed, a protective gas support box was installed, and a local protective gas was dragged to prevent oxidation of the titanium alloy after welding; the air hammer was installed on the welding robot, and the force between the hammer forging device and the deposited layer was adjusted to 0.6 MPa; (2) A welding robot was used to perform additive manufacturing on a titanium alloy substrate. The process parameters for arc additive manufacturing of titanium alloy were as follows: welding current was 250A; voltage was 20V, wire feeding speed was 189 cm / min, welding moving speed was 5mm / s; interlayer temperature was controlled below 80°C, and the arc starting and extinguishing points of each layer were consistent; In the process of arc additive manufacturing of titanium alloy, each time a layer is deposited, an air hammer is used to perform synchronous hammer forging treatment on each deposited layer 3 times. The speed of hammer forging is 4 times / second, and the force of a single hammer forging is 0.6 MPa. After the hammer forging is completed, arc additive manufacturing of the next layer is carried out. The process parameters of arc additive manufacturing remain consistent until the processing of the titanium alloy component is completed. During the processing, the deposition thickness of each deposited layer is controlled to be 1~1.5mm.

[0034] Example 2 The present invention provides a method for preparing a titanium alloy, comprising the following steps: (1) TC4 welding wire with an oxygen content of less than 0.1% was used as the raw material for arc additive, the TC4 additive substrate was fixed, a protective gas support box was installed, and a local protective gas was dragged to prevent oxidation of the titanium alloy after welding; the air hammer was installed on the welding robot, and the force between the hammer forging device and the deposited layer was adjusted to 0.9 MPa; (2) A welding robot was used to perform additive manufacturing on a titanium alloy substrate. The process parameters for arc additive manufacturing of titanium alloy were as follows: welding current was 250A; voltage was 20V, wire feeding speed was 189 cm / min, welding moving speed was 5mm / s; interlayer temperature was controlled below 80°C, and the arc starting and extinguishing points of each layer were consistent; In the process of arc additive manufacturing of titanium alloy, each time a layer is deposited, an air hammer is used to perform synchronous hammer forging treatment on each deposited layer twice. The speed of hammer forging is 5 times / second, the force of a single hammer forging is 0.9 MPa, and the angles between the air hammer and the deposited layer are 90° and 45° respectively. After the hammer forging is completed, arc additive manufacturing of the next layer is carried out, and the process parameters of arc additive manufacturing remain consistent until the titanium alloy component is processed. During the processing, the deposition thickness of each deposited layer is controlled to be 1~1.5mm.

[0035] Example 3 The present invention provides a method for preparing a titanium alloy, comprising the following steps: (1) TC4 welding wire with an oxygen content of less than 0.1% was used as the raw material for arc additive, the TC4 additive substrate was fixed, a protective gas support box was installed, and a local protective gas was dragged to prevent oxidation of the titanium alloy after welding; the air hammer was installed on the welding robot, and the force between the hammer forging device and the deposited layer was adjusted to 0.3 MPa; (2) A welding robot was used to perform additive manufacturing on a titanium alloy substrate. The process parameters for arc additive manufacturing of titanium alloy were as follows: welding current was 250A; voltage was 20V, wire feeding speed was 189 cm / min, welding moving speed was 5mm / s; interlayer temperature was controlled below 80°C, and the arc starting and extinguishing points of each layer were consistent; In the process of arc additive manufacturing of titanium alloy, each time a layer is deposited, an air hammer is used to perform synchronous hammer forging treatment on each deposited layer 4 times. The speed of hammer forging is 3 times / second, the force of a single hammer forging is 0.3Mpa, and the angles between the air hammer and the deposited layer are 90°, 75°, 45° and 30° respectively. After the hammer forging is completed, arc additive manufacturing of the next layer is carried out, and the process parameters of arc additive manufacturing remain consistent until the titanium alloy component is processed. During the processing, the deposition thickness of each deposited layer is controlled to be 1~1.5mm.

[0036] Example 4 The present invention provides a method for preparing a titanium alloy, comprising the following steps: (1) TC4 welding wire with an oxygen content of less than 0.1% was used as the raw material for arc additive, the TC4 additive substrate was fixed, a protective gas support box was installed, and a local protective gas was dragged to prevent oxidation of the titanium alloy after welding; the air hammer was installed on the welding robot, and the force between the hammer forging device and the deposited layer was adjusted to 0.4 MPa; (2) A welding robot was used to perform additive manufacturing on a titanium alloy substrate. The process parameters for arc additive manufacturing of titanium alloy were as follows: welding current was 205A; voltage was 18V, wire feeding speed was 200 cm / min, welding moving speed was 4mm / s; interlayer temperature was controlled below 80°C, and the arc starting and extinguishing points of each layer were consistent; In the process of arc additive manufacturing of titanium alloy, each time a layer is deposited, an air hammer is used to perform synchronous hammer forging treatment on each deposited layer 4 times. The speed of hammer forging is 3 times / second, the force of a single hammer forging is 0.4Mpa, and the angles between the air hammer and the deposited layer are 90°, 75°, 45° and 30° respectively. After the hammer forging is completed, arc additive manufacturing of the next layer is carried out, and the process parameters of arc additive manufacturing remain consistent until the processing of the titanium alloy component is completed. During the processing, the deposition thickness of each deposited layer is controlled to be 1~1.5mm.

[0037] Example 5 The present invention provides a method for preparing a titanium alloy, comprising the following steps: (1) TC4 welding wire with an oxygen content of less than 0.1% was used as the raw material for arc additive, the TC4 additive substrate was fixed, a protective gas support box was installed, and a local protective gas was dragged to prevent oxidation of the titanium alloy after welding; the air hammer was installed on the welding robot, and the force between the hammer forging device and the deposited layer was adjusted to 0.8 MPa; (2) A welding robot was used to perform additive manufacturing on a titanium alloy substrate. The process parameters for arc additive manufacturing of titanium alloy were as follows: welding current was 240A; voltage was 21V, wire feeding speed was 130 cm / min, welding moving speed was 6 mm / s; interlayer temperature was controlled below 80°C, and the arc starting and extinguishing points of each layer were consistent; In the process of arc additive manufacturing of titanium alloy, each time a layer is deposited, an air hammer is used to perform synchronous hammer forging treatment on each deposited layer 4 times. The speed of hammer forging is 3 times / second, the force of a single hammer forging is 0.8 MPa, and the angles between the air hammer and the deposited layer are 90°, 75°, 45° and 30° respectively. After the hammer forging is completed, arc additive manufacturing of the next layer is carried out, and the process parameters of arc additive manufacturing remain consistent until the titanium alloy component is processed. During the processing, the deposition thickness of each deposited layer is controlled to be 1~1.5mm.

[0038] Comparative Example 1 This comparative example provides a method for preparing a titanium alloy, comprising the following steps: (1) Use TC4 welding wire with an oxygen content of less than 0.1% as the raw material for arc additive, fix the TC4 additive substrate, install a shielding gas support box, and drag the local shielding gas to avoid oxidation of titanium alloy after welding; (2) A welding robot was used to perform additive manufacturing on a titanium alloy substrate. The process parameters for arc additive manufacturing of titanium alloy were as follows: welding current was 250 A; voltage was 20 V, wire feeding speed was 189 cm / min, and welding moving speed was 5 mm / s; interlayer temperature was controlled below 80 °C, the arc starting and extinguishing points of each layer were consistent, and the deposition thickness of each deposition layer was approximately 1.4 mm.

[0039] The KAM diagram of the titanium alloy prepared in this comparative example is as follows: Figure 5 As shown, from Figure 5 It can be seen that the plastic deformation in each region is basically consistent and evenly distributed, without dislocation energy accumulation.

[0040] Comparative Example 2 This comparative example provides a method for preparing a titanium alloy, comprising the following steps: (1) TC4 welding wire with an oxygen content of less than 0.1% was used as the raw material for arc additive, the TC4 additive substrate was fixed, a protective gas support box was installed, and a local protective gas was dragged to prevent oxidation of the titanium alloy after welding; the air hammer was installed on the welding robot, and the force between the hammer forging device and the deposited layer was adjusted to 0.6 MPa; (2) A welding robot was used to perform additive manufacturing on a titanium alloy substrate. The process parameters for arc additive manufacturing of titanium alloy were as follows: welding current was 150A; voltage was 20V, wire feeding speed was 189 cm / min, welding moving speed was 5mm / s; interlayer temperature was controlled below 80°C, and the arc starting and extinguishing points of each layer were consistent; In the process of arc additive manufacturing of titanium alloy, each layer is deposited and hammered forged three times by air hammer. The speed of hammer forging is 4 times / second and the force of single hammer forging is 0.6Mpa. After hammer forging, arc additive manufacturing of the next layer is carried out. The process parameters of arc additive manufacturing are kept consistent until the titanium alloy component is processed. The welding current of this comparative example is small. When other parameters are constant, the molten pool width is small and the layer height is large, reaching 3 mm. The equiaxed crystal transformation effect after hammering is weak.

[0041] Comparative Example 3 This comparative example provides a method for preparing a titanium alloy, comprising the following steps: (1) TC4 welding wire with an oxygen content of less than 0.1% was used as the raw material for arc additive, the TC4 additive substrate was fixed, a protective gas support box was installed, and a local protective gas was dragged to prevent oxidation of the titanium alloy after welding; the air hammer was installed on the welding robot, and the force between the hammer forging device and the deposited layer was adjusted to 0.6 MPa; (2) A welding robot was used to perform additive manufacturing on a titanium alloy substrate. The process parameters for arc additive manufacturing of titanium alloy were as follows: welding current was 200A; voltage was 20V, wire feeding speed was 189 cm / min, welding moving speed was 5mm / s; interlayer temperature was controlled below 80°C, and the arc starting and extinguishing points of each layer were consistent; In the process of arc additive manufacturing of titanium alloy, each layer is deposited and hammered forged three times by air hammer. The speed of hammer forging is 4 times / second and the force of single hammer forging is 0.6Mpa. After hammer forging, arc additive manufacturing of the next layer is carried out. The process parameters of arc additive manufacturing are kept consistent until the titanium alloy component is processed. The welding current of this comparative example is medium, the molten pool width is medium, the layer height is medium, the deposition thickness of each deposition layer is about 2.5 mm, and the equiaxed crystal transformation effect after hammering is average.

[0042] Comparative Example 4 This comparative example provides a method for preparing a titanium alloy, comprising the following steps: (1) TC4 welding wire with an oxygen content of less than 0.1% was used as the raw material for arc additive, the TC4 additive substrate was fixed, a protective gas support box was installed, and a local protective gas was dragged to prevent oxidation of the titanium alloy after welding; the air hammer was installed on the welding robot, and the force between the hammer forging device and the deposited layer was adjusted to 0.6 MPa; (2) A welding robot was used to perform additive manufacturing on a titanium alloy substrate. The process parameters for arc additive manufacturing of titanium alloy were as follows: welding current was 250A; voltage was 20V, wire feeding speed was 125 cm / min, welding moving speed was 5mm / s; interlayer temperature was controlled below 80°C, and the arc starting and extinguishing points of each layer were consistent; In the process of arc additive manufacturing of titanium alloy, each time a layer is deposited, an air hammer is used to perform synchronous hammer forging treatment on each deposited layer 3 times. The speed of hammer forging is 4 times / second, and the force of a single hammer forging is 0.6 MPa. After the hammer forging is completed, arc additive manufacturing of the next layer is carried out. The process parameters of arc additive manufacturing remain consistent until the titanium alloy component is processed.

[0043] The wire feeding speed of this comparative example is too small, the cross-sectional area of ​​the deposit per unit time is reduced, and when the arc remains unchanged, the height of the molten pool becomes very thin, and the deposition thickness of each deposition layer is about 2.2 mm. The equiaxed crystal transformation effect after hammering is average.

[0044] Comparative Example 5 This comparative example provides a method for preparing a titanium alloy, comprising the following steps: (1) TC4 welding wire with an oxygen content of less than 0.1% was used as the raw material for arc additive, the TC4 additive substrate was fixed, a protective gas support box was installed, and a local protective gas was dragged to prevent oxidation of the titanium alloy after welding; the air hammer was installed on the welding robot, and the force between the hammer forging device and the deposited layer was adjusted to 0.6 MPa; (2) A welding robot was used to perform additive manufacturing on a titanium alloy substrate. The process parameters for arc additive manufacturing of titanium alloy were as follows: welding current was 250A; voltage was 20V, wire feeding speed was 189 cm / min, welding moving speed was 7mm / s; interlayer temperature was controlled below 80°C, and the arc starting and extinguishing points of each layer were consistent; In the process of arc additive manufacturing of titanium alloy, each layer is deposited and hammered forged three times by air hammer. The speed of hammer forging is 4 times / second and the force of single hammer forging is 0.6Mpa. After hammer forging, arc additive manufacturing of the next layer is carried out. The process parameters of arc additive manufacturing are kept consistent until the titanium alloy component is processed. In this comparative example, because the welding movement speed is too fast, the deposition amount per unit time is reduced, and the deposition cross-sectional area is reduced, that is, the height becomes shorter and the width becomes narrower. The deposition thickness of each deposition layer is about 1.7 mm. The equiaxed crystal transformation effect after hammering is general, but it has a certain positive effect on the impact after hammering.

[0045] The microstructure of the titanium alloys prepared in Example 1 and Comparative Example 1 was characterized. The test results are as follows: Figure 1 and Figure 2 As shown, Figure 1 is the grain map of the titanium alloy without hammering in Comparative Example 1, Figure 2 This is the grain map of the titanium alloy after hammering in Example 1. Figure 1 and Figure 2 It can be seen that the original β grains of titanium alloy are successfully transformed from columnar grains to equiaxed grains.

[0046] Figure 3 and Figure 4 The multi-layer and multi-pass printing state of the titanium alloy obtained in Example 1 and Comparative Example 1, that is, whether hammering is effective for titanium alloy structural parts with thicker walls. Figure 4 It can be seen that the effect can be seen not only in single-wall but also in multi-layer and multi-channel thick slabs.

[0047] Figure 6 This is an electron backscatter diagram of the distribution of the plastic deformation area of ​​the deposited metal by hammering in Example 1. Figure 6 It can be seen that the thickness of the plastic deformation zone after hammering in this embodiment is 1.5 mm.

[0048] Figure 7 The hardness distribution diagram from the surface to the inside of Example 1 (hammered sample) and Comparative Example 1 (no hammered sample). Figure 7 It can be seen that there is a clear difference in hardness distribution before and after hammering. The hardness after hammering is much higher than that of the unhammered sample on the surface. When the depth reaches 1.5mm, the hardness is consistent with that of the unhammered sample. The reason why the hammered surface hardness is high is that under the action of hammering, the surface has strong plastic deformation, high dislocation density, and large residual stress. However, at a depth of 1.5mm, the hardness returns to normal, that is, the plastic deformation disappears. This depth is the area where the hammer can act. This area is very critical in the process of hammering use conditions and is the core of this application, because if the deposited layer height is controlled to be lower than this depth, more equiaxed crystals can be obtained.

[0049] Figure 8 and Fig. 9 These are stress-strain curves of the mechanical properties of the materials. Figure 8 It is the sample without hammering in comparative example 1, Fig. 9 This is the sample after hammering in Example 1. Figure 8 and Fig. 9 It can be seen that the anisotropy of the mechanical properties of the titanium alloy prepared in Example 1 in the elongation direction is improved from 10% to 3%.

[0050] The deposition thickness (layer height d) and crystal proportion of the single layer of titanium alloy obtained in Examples 1 to 5 and Comparative Examples 1 to 5 were characterized. The crystal proportion refers to the ratio of the volume occupied by atoms contained in a unit cell to the volume of the unit cell. The results are shown in Table 1: Table 1. Layer height and crystal proportion of titanium alloys obtained in Examples 1 to 5 and Comparative Examples 1 to 5 Detection object Layer height d (mm) Equiaxed crystal ratio (%) Example 1 1.4 95 Example 2 1.4 95 Example 3 1.4 80 Example 4 1.5 90 Example 5 1.0 95 Comparative Example 1 1.4 0 Comparative Example 2 3 20 Comparative Example 3 2.5 33 Comparative Example 4 2.2 45 Comparative Example 5 1.7 78 In summary, the present invention couples the hammer forging process with the arc additive manufacturing process, adopts a cross-combination of the hammer forging process and the arc additive manufacturing process, increases the volume fraction of the original β grains of the titanium alloy converted from columnar crystals to equiaxed crystals, weakens the anisotropy of the material, and enables the comprehensive mechanical properties of the titanium alloy parts or repair parts formed by arc additive manufacturing to meet the requirements of the aviation field. By comparing the data of Example 1 with Comparative Example 1, it can be seen that under the same deposition parameter conditions, although the deposition thickness of the two is the same, because Comparative Example 1 does not have a hammer forging process, combined with Figure 5 It can be seen that the plastic deformation of each region is basically the same, evenly distributed, and there is no dislocation energy accumulation, indicating that it still retains the original β grains and cannot complete the transformation of the original β grains from columnar crystals to equiaxed crystals, resulting in equiaxed crystals accounting for 0%; by comparing the data of Example 1 with Comparative Examples 2 to 5, it can be seen that the process parameters of the hammer forging process and the arc additive manufacturing process need to be taken into account at the same time to achieve the technical effect of the present application, that is, the deposition parameters need to be strictly controlled, and the change of any parameter will affect the deposition thickness and crystal form proportion of the single layer. Therefore, the present invention effectively overcomes the various shortcomings of the prior art and has a high industrial utilization value.

[0051] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for preparing a titanium alloy, characterized in that: The hammer forging process is coupled with the arc additive manufacturing process. Titanium alloy welding wire is used as raw material and the arc additive process is adopted to manufacture titanium alloy. During the arc additive manufacturing process of titanium alloy, a hammer forging device is used to synchronously hammer forge each deposition layer until the titanium alloy component is completed. During the processing, the deposition thickness of each deposition layer is controlled to be 1~1.5mm.

2. The preparation method according to claim 1, characterized in that: During the hammer forging process, the force between the hammer forging device and the deposited layer is controlled to be 0.3~0.9MPa.

3. The preparation method according to claim 1, characterized in that: During the hammer forging process, the angle between the hammer forging device and the deposited layer is controlled to be 30~90°.

4. The preparation method according to claim 3, characterized in that: The number of hammer forging treatments for each deposition layer is controlled to be 2 to 4 times, and the speed of the hammer forging treatment is controlled to be 3 to 5 times per second.

5. The preparation method according to claim 4, characterized in that: In the process of controlling the hammer forging treatment of each deposition layer, the number of hammer forging treatments is at least twice, and the angle between the hammering direction of the hammer forging device and the deposition layer includes at least 90° and 45°.

6. The preparation method according to claim 1, characterized in that: The process parameters of arc additive manufacturing of titanium alloy are: welding current is 205~250A; voltage is 18~21V, wire feeding speed is 130~200 cm / min, and welding moving speed is 4~6mm / s.

7. The preparation method according to claim 1, characterized in that: The titanium alloy welding wire is a TC4 welding wire with an oxygen content of less than 0.1%.

8. A titanium alloy prepared by the preparation method according to any one of claims 1 to 7.

9. The titanium alloy according to claim 8, characterized in that: The crystal phase structure of the titanium alloy includes equiaxed crystals and columnar crystals, and the proportion of the equiaxed crystals is not less than 80%.

10. Use of the titanium alloy according to claim 8 or 9 in the field of aerospace.

Citation Information

Patent Citations

  • Forging and pressing thermal treatment integration device for additive manufacturing

    CN107584118A

  • Robot equal material manufacturing and ultrasonic multi-head peening device and method

    CN108517479A

  • Method for refining additive manufactured titanium alloy grains

    CN109128172A

  • Large part 3D printing method

    CN109332851A

  • Additive manufacturing equipment and manufacturing method for titanium alloy structural part

    CN112427649A