Grinding process method for inhibiting grinding spalling damage of surface of bearing raceway
By controlling the tangential grinding load of the grinding wheel abrasive grains and increasing the grinding wheel speed, combined with the control of the maximum undeformed chip thickness, the problem of grinding spalling damage in traditional bearing raceway grinding is solved, and the fatigue life and surface of the bearing are significantly improved. quality.
Patent Information
- Application Number
- CN202410901367.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-15
AI Technical Summary
The traditional bearing raceway grinding process fails to effectively suppress the grinding and spalling damage on the raceway surface, resulting in the fatigue life of domestic bearings being lower than that of internationally renowned brands.
By controlling the tangential grinding load of the grinding wheel abrasive grains within 0.16N, using a grinding wheel speed of no less than 60m/s, and meeting the control requirements for the maximum undeformed chip thickness in the process parameter design, the surface quality of the bearing raceway is ensured.
It significantly reduces the grinding and spalling damage on the bearing raceway surface, improves the fatigue life and performance, and narrows the life gap between domestic bearings and imported bearings.
Smart Images

Figure CN118769075A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of bearing manufacturing, and in particular relates to a grinding process method for suppressing grinding and spalling damage on the surface of a bearing raceway. Background Art
[0002] Bearing raceway grinding is one of the most critical processes in bearing manufacturing. The grinding quality of the raceway will directly affect the performance and fatigue life of the bearing. Traditional bearing raceway grinding usually only considers dimensional tolerances, form and position tolerances, and surface roughness, and does not consider surface integrity issues such as raceway subsurface grinding spalling damage caused by grinding. The surface integrity defects of the raceway will greatly shorten the fatigue life of the bearing. Since traditional bearing manufacturing lacks key surface integrity indicators to control the surface quality of the bearing raceway, and lacks process methods to regulate key indicators, the fatigue life of domestic bearings is much lower than that of internationally renowned brands. Therefore, in response to the demand for improving bearing fatigue life, it is necessary to provide key indicators that affect bearing fatigue life, namely raceway subsurface grinding spalling damage and its characterization parameters, as well as process methods to inhibit grinding spalling damage. Summary of the invention
[0003] In view of the problems existing in the prior art, the present invention provides a grinding process method for suppressing grinding and spalling damage on the surface of a bearing raceway.
[0004] The gist of the present invention includes: (1) a grinding process method for inhibiting the grinding and spalling damage of the bearing raceway surface; the grinding process method for inhibiting the grinding and spalling damage of the bearing raceway surface requires taking the tangential grinding load of the grinding wheel abrasive grains during the grinding process as a key control parameter; under the condition that the bearing material is a high carbon chromium alloy (DIN100Cr6) and a ceramic sintered corundum grinding wheel (Saint-Gobain-Norton), the tangential grinding load F of the grinding wheel abrasive grains should be set to 0.05. tg Controlled in F tg <F tg * , F tg * The value range is F tg * ≤0.16N; (2) The grinding process method for suppressing the grinding and spalling damage on the bearing raceway surface generally has a grinding wheel linear speed of not less than 60m / s; (3) The process parameter design of the grinding process method should meet the control requirements of the maximum undeformed chip thickness.
[0005] Furthermore, (4) the maximum undeformed chip thickness of bearing raceway grinding is expressed as a gmax It is characterized by the fact that the maximum undeformed chip thickness needs to satisfy a gmax <a gmax * , a gmax* The value range is a gmax * ≤1.28μm.
[0006] Furthermore, (5) the process parameter design of the grinding process method should meet the control requirements of the maximum undeformed chip thickness, that is:
[0007]
[0008] In the formula, v s is the grinding wheel speed, v w is the workpiece speed, a p is the grinding depth of cut, λ sl is the distance between the continuous cutting edges of the grinding wheel, d s is the grinding wheel diameter, d w is the workpiece diameter.
[0009] Another object of the present invention is to provide a method for evaluating grinding and spalling damage on the surface of a bearing raceway.
[0010] Furthermore, the measurement index of the grinding and spalling damage on the bearing raceway surface includes the area ratio of the grinding and spalling damage area on the bearing raceway surface δ d , and the length of the grinding and spalling damage on the bearing raceway surface l peel and width b peel .
[0011] Furthermore, the area ratio of the grinding and spalling damage area on the bearing raceway surface is δ d , characterized in that δ d It is used to indicate the ratio of the total grinding and spalling damage area to the total observation area within the observation period.
[0012] Furthermore, the grinding and spalling damage on the bearing raceway surface is characterized in that the grinding and spalling damage is discretely distributed on the bearing raceway surface and has a concave three-dimensional morphology. The grinding and spalling length l peel Generally 30~300μm, grinding peeling width b peel Generally 20 to 50 μm.
[0013] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows:
[0014] First, the present invention includes a grinding process method for suppressing the grinding and spalling damage of the bearing raceway surface and a method for evaluating the grinding and spalling damage of the bearing raceway surface. The grinding process method for suppressing the grinding and spalling damage of the bearing raceway surface mainly includes the control requirements of the grinding load of the grinding wheel abrasive particles during the grinding process, the requirements of the grinding wheel speed, and the control requirements of the maximum undeformed chip thickness.
[0015] Second, the present invention can effectively suppress the surface damage of the bearing raceway grinding, overcome the problems of poor grinding quality of the rolling bearing raceway surface and difficulty in optimizing the grinding process parameters, and lay a foundation for reasonable and effective mechanical processing methods and process parameters to improve the service performance and fatigue life of high-end bearing products. By effectively suppressing the grinding and spalling damage of the bearing raceway surface, the present invention can improve the long-term stability of the actual operation of the bearing and its fatigue life, and narrow the life gap with imported high-end bearings.
[0016] Third, the technical solution of the present invention fills the technical gap in the industry at home and abroad: the technology of the present invention effectively suppresses the grinding and spalling damage on the surface of the bearing raceway, and the fatigue life test verification shows that it significantly improves the fatigue life of the bearing product. Related explanation: The reason why the actual test life range is relatively large is that there are many bearing parts processing and assembly processes, the production environment of each process, the processing errors of bearing-related parts, the stability of the automatic loading and unloading mechanism, the wear of the grinding wheel and other process conditions cause inconsistencies and instabilities.
[0017] The expected benefits and commercial value after the technical solution of the present invention is as follows: Taking the test bearing model 7002P4 used for fatigue life test of the present invention as an example, since the fatigue life of domestic bearings, especially high-end bearings, is very different from that of international famous brand bearings, according to the current market price, the price of international famous brand bearings (such as NSK) is generally 3 times or more than that of domestic bearings. The process method proposed by the present invention will significantly improve the fatigue life of domestic bearings, bringing huge benefits and commercial value to enterprises.
[0018] The technical solution of the present invention solves a technical problem that people have been eager to solve but have never been able to solve successfully: fatigue life tests have shown that the fatigue life of high-end bearings produced in my country is significantly improved.
[0019] The technical solution of the present invention overcomes technical prejudice: the present invention is a breakthrough in the field of new process methods and engineering application technology, breaking the traditional concept and breaking through the existing process technologies and methods.
[0020] Fourth, the present invention significantly solves the spalling damage problem that is prone to occur during the grinding process of the bearing raceway surface in the prior art by introducing key control parameters, such as the tangential grinding load of the grinding wheel abrasive and the high grinding wheel speed. In the traditional grinding process, the grinding load and chip thickness are not effectively controlled, which makes the bearing raceway surface prone to grinding spalling, affecting its service life and performance. The present invention controls the tangential grinding load to ≤0.16N by precisely controlling the grinding load, especially under the conditions of high-carbon chromium alloy and ceramic sintered corundum grinding wheels, effectively reducing the occurrence of spalling during the grinding process.
[0021] In addition, the present invention adopts a high grinding wheel speed of not less than 60m / s, so that the abrasive load of the grinding wheel is strictly controlled within the required range, thereby optimizing the grinding effect. In the traditional method, due to the low grinding wheel speed, the abrasive load is difficult to effectively control, resulting in unstable surface quality and easy peeling damage. The present invention optimizes the grinding parameters by increasing the grinding wheel speed, making the grinding process more stable and significantly improving the surface quality.
[0022] The present invention also ensures that the maximum undeformed chip thickness is controlled within a reasonable range through the careful design of process parameters, further improving the accuracy of the grinding process. The mathematical model is used to describe the relationship between the grinding wheel speed, workpiece speed, grinding depth, the spacing between continuous cutting edges of the grinding wheel, the grinding wheel diameter and the workpiece diameter, and the maximum undeformed chip thickness is accurately calculated, thereby optimizing the grinding parameters and reducing spalling damage. This parameter optimization design based on the mathematical model effectively improves the overall performance and stability of the grinding process.
[0023] In practical applications, the present invention verifies the effectiveness of the process by measuring and analyzing in detail the area ratio of the grinding spalling damage area on the bearing raceway surface and the length and width of the damage. The results show that the spalling damage on the bearing raceway surface is significantly reduced and the surface quality is greatly improved by using the grinding process of the present invention. This grinding process optimization method based on data-driven and mathematical models not only improves the service life and reliability of bearings, but also provides strong support for the surface treatment of other precision mechanical parts. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a flow chart of a grinding process method for suppressing grinding and spalling damage on a bearing raceway surface provided by an embodiment of the present invention;
[0025] Figure 2 is a schematic diagram of grinding and spalling damage on the bearing raceway surface provided by an embodiment of the present invention;
[0026] Figure 3 It is a schematic diagram of the area ratio of the grinding and spalling damage area on the bearing raceway surface provided by an embodiment of the present invention. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0028] The embodiment of the present invention provides a grinding process method for suppressing grinding and spalling damage on the bearing raceway surface. The grinding process method for suppressing grinding and spalling damage on the bearing raceway surface requires taking the tangential grinding load of the grinding wheel abrasive during the grinding process as a key control parameter; the grinding process for suppressing grinding and spalling damage on the bearing raceway surface adopts a high grinding wheel speed; the process parameter design of the grinding process method should meet the control requirements of the maximum undeformed chip thickness.
[0029] It is necessary to control the tangential grinding load of the grinding wheel abrasive during the grinding process. The tangential grinding load of the grinding wheel abrasive is expressed by F. tg It is indicated that it is also affected by the combination of process parameters and the process system. When the bearing material is high carbon chromium alloy (DIN100Cr6) and ceramic sintered corundum grinding wheel (Saint-Gobain-Norton), the tangential grinding load F of the grinding wheel abrasive needs to be tg Controlled in F tg <F tg * , F tg * The value range is F tg * ≤0.16N;
[0030] A high grinding wheel speed of not less than 60m / s is required to keep the grinding wheel abrasive load within the required range;
[0031] The maximum undeformed chip thickness of bearing raceway grinding is represented by agmax. The maximum undeformed chip thickness needs to meet a gmax <a gmax * .a gmax * The value range is a gmax * ≤1.28μm.
[0032] The design of the grinding process parameters should meet the control requirements of the maximum undeformed chip thickness, namely:
[0033]
[0034] In the formula, v s is the grinding wheel speed, v w is the workpiece speed, a p is the grinding depth of cut, λ sl is the distance between the continuous cutting edges of the grinding wheel, d s is the grinding wheel diameter, d w is the workpiece diameter.
[0035] The area ratio of the grinding and spalling damage area on the bearing raceway surface is δ d , and the length of the grinding and spalling damage on the bearing raceway surface lpeel and width b peel .
[0036] δ d It is used to indicate the ratio of the total grinding and spalling damage area to the total observation area within the observation period.
[0037] Grinding spalling damage is discretely distributed on the bearing raceway surface, with a concave three-dimensional morphology. The grinding spalling length is l peel Generally 30~300μm, grinding peeling width b peel Generally 20 to 50 μm.
[0038] like Figure 1 As shown, the high-speed grinding process method for suppressing sub-surface grinding cracks of a bearing raceway provided by an embodiment of the present invention comprises the following steps:
[0039] S101: Use a high grinding wheel speed of not less than 60m / s and a maximum undeformed chip thickness of not more than 1.28μm;
[0040] S102: Control the grinding load of the grinding wheel abrasive to be less than 0.16N.
[0041] Embodiment 1:
[0042] The embodiment of the present invention provides a grinding process method for suppressing grinding and spalling damage on the bearing raceway surface. The grinding process method for suppressing grinding and spalling damage on the bearing raceway surface requires controlling the tangential grinding load of the grinding wheel abrasive during the grinding process; the grinding process for suppressing grinding and spalling damage on the bearing raceway surface adopts a high grinding wheel speed; the grinding process for suppressing grinding and spalling damage on the bearing raceway surface should meet the control requirements of the maximum undeformed chip thickness.
[0043] In the present invention, under the condition that the bearing material is a high carbon chromium alloy (DIN100Cr6) and a ceramic sintered corundum grinding wheel (Saint-Gobain-Norton), the tangential grinding load F of the grinding wheel abrasive grains is reduced by adopting a high grinding wheel speed of not less than 60 m / s and a maximum undeformed chip thickness of not more than 1.28 μm. tg Control it to less than 0.16N to suppress the grinding and spalling damage on the bearing raceway surface.
[0044] It should be noted that the embodiments of the present invention can be implemented by hardware, software, or a combination of software and hardware. The hardware part can be implemented using dedicated logic; the software part can be stored in a memory and executed by an appropriate instruction execution system, such as a microprocessor or dedicated design hardware. It can be understood by a person of ordinary skill in the art that the above-mentioned devices and methods can be implemented using computer executable instructions and / or contained in a processor control code, such as a carrier medium such as a disk, CD or DVD-ROM, a programmable memory such as a read-only memory (firmware), or a data carrier such as an optical or electronic signal carrier. Such code is provided on the carrier medium. The device and its modules of the present invention can be implemented by hardware circuits such as very large-scale integrated circuits or gate arrays, semiconductors such as logic chips, transistors, etc., or programmable hardware devices such as field programmable gate arrays, programmable logic devices, etc., can also be implemented by software executed by various types of processors, and can also be implemented by a combination of the above-mentioned hardware circuits and software, such as firmware.
[0045] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A grinding process method for inhibiting grinding and spalling damage on the surface of a bearing raceway, characterized in that: The grinding process method for suppressing grinding spalling damage on the bearing raceway surface requires taking the tangential grinding load of the grinding wheel abrasive during the grinding process as a key control parameter; the grinding process method for suppressing grinding spalling damage on the bearing raceway surface adopts a high grinding wheel speed; the process parameter design of the grinding process method should meet the control requirements of the maximum undeformed chip thickness.
2. The grinding process method for suppressing grinding and spalling damage on the bearing raceway surface according to claim 1, characterized in that: It is necessary to control the tangential grinding load of the grinding wheel abrasive during the grinding process. The tangential grinding load of the grinding wheel abrasive is expressed by F. tg It is indicated that it is affected by the combination of process parameters and the process system. When the bearing material is high carbon chromium alloy and ceramic sintered corundum grinding wheel, the tangential grinding load F of the grinding wheel abrasive needs to be tg Controlled in F tg <F tg * , F tg * The value range is F tg * ≤0.16N.
3. The grinding process method for suppressing grinding and spalling damage on the bearing raceway surface according to claim 1, characterized in that: A high grinding wheel speed of not less than 60 m / s is required to keep the grinding wheel abrasive load within the required range.
4. The grinding process method for suppressing grinding and spalling damage on the bearing raceway surface according to claim 1, characterized in that: The process parameter design of the grinding process should meet the control requirements of the maximum undeformed chip thickness. The maximum undeformed chip thickness of the bearing raceway grinding is expressed as a gmax Indicates that the maximum undeformed chip thickness needs to satisfy a gmax gmax * , a gmax * The value range is a gmax * ≤1.28μm. 5. The design of the grinding process parameters should meet the control requirements of the maximum undeformed chip thickness, namely: In the formula, v s is the grinding wheel speed, v w is the workpiece speed, a p is the grinding depth of cut, λ sl is the distance between the continuous cutting edges of the grinding wheel, d s is the grinding wheel diameter, d w is the workpiece diameter.
6. The grinding process method for suppressing grinding and spalling damage on the bearing raceway surface according to claim 4, characterized in that: The grinding and spalling damage on the bearing raceway surface includes the area ratio δ of the grinding and spalling damage area on the bearing raceway surface. d , and the length of the grinding and spalling damage on the bearing raceway surface l peel and width b peel .
7. The grinding process method for suppressing grinding and spalling damage on the bearing raceway surface according to claim 4, characterized in that: The area ratio of the grinding and spalling damage area on the bearing raceway surface is d , δ d It is used to indicate the ratio of the total grinding and spalling damage area to the total observation area within the observation period.
8. The grinding process method for suppressing grinding and spalling damage on the bearing raceway surface according to claim 4, characterized in that: The grinding and spalling damage on the bearing raceway surface is discretely distributed on the bearing raceway surface and has a concave three-dimensional morphology. The grinding and spalling length is l peel Generally 30~300μm, grinding peeling width b peel Generally 20 to 50 μm.
Citation Information
Patent Citations
Bearing raceway high-speed grinding method considering surface integrity, parameters and application
CN117161834A