Preservative and preparation method thereof
Through the combination of water-soluble polyaniline and other ingredients as a preservative, the problem of wood being susceptible to decay is solved, the anti-mildew and anti-corrosion effect is significantly improved, and the service life of the wood is extended.
Patent Information
- Application Number
- CN202410572334.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-10
- Publication Date
- 2024-10-15
AI Technical Summary
Wood is susceptible to damage by bacteria, insects and microorganisms, leading to discoloration, decay and insect infestation. Existing technologies fail to effectively utilize polyaniline for wood preservation.
A combination preservative of water-soluble polyaniline, triethanolamine, Tween-20, lignin and diatomaceous earth is used to improve the anti-mildew and anti-corrosion effect by mixing and soaking the furniture boards.
It significantly extends the anti-mildew and anti-corrosion life of wood. Boards without water-soluble polyaniline will show mildew and rot within 1 month, but only appear after 3 months of use. This significantly improves the anti-mildew and anti-corrosion effect.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wood antiseptic, in particular to an antiseptic and a preparation method thereof. Background Art
[0002] Wood is used in various occasions such as structural materials, civil engineering materials, etc. It is an important raw material to promote economic development. However, wood is extremely susceptible to damage by fungi, insects and microorganisms, which can cause discoloration, decay and insect infestation, seriously affecting the use of wood and thus causing huge economic losses.
[0003] Wooden furniture is made of solid wood as the main material. Wooden furniture has a long service life. In addition to the hardness and crack resistance of the board itself, it also has high requirements for its mildew and anti-corrosion performance. In some warm and humid places, ordinary wooden furniture is particularly prone to mold and rot. The current method for treating wood mildew and anti-corrosion is usually to apply a layer of moisture-proof and mildew-proof water-based paint on the surface of the wood. There is no prior art on the application of polyaniline in wood anti-corrosion. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a preservative and a preparation method thereof. The present invention applies water-soluble polyaniline to the mildew and corrosion prevention of furniture boards, thereby improving the mildew and corrosion prevention effect of the boards.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] The present invention provides a preservative, which is prepared from the following components in parts by weight:
[0007] 90-110 parts of water, 15-25 parts of water-soluble polyaniline, 10-15 parts of triethanolamine, 1-3 parts of Tween-20, 3-8 parts of lignin and 3-8 parts of diatomaceous earth.
[0008] Preferably, it is prepared from the following components in parts by weight:
[0009] 100 parts of water, 20 parts of water-soluble polyaniline, 12 parts of triethanolamine, 2 parts of Tween-20, 5 parts of lignin and 5 parts of diatomaceous earth.
[0010] The present invention also provides a method for preparing the preservative described in the above technical solution, comprising the following steps:
[0011] The water, water-soluble polyaniline, triethanolamine, Tween-20, lignin and diatomaceous earth are mixed to obtain a preservative.
[0012] Preferably, the mixing conditions include: a rotation speed of 4000 to 5000 rpm and a time of 30 to 40 minutes.
[0013] The present invention also provides the use of the preservative described in the above technical solution in the mildew and corrosion prevention of furniture boards.
[0014] Preferably, the applying comprises: completely immersing the furniture board in a preservative.
[0015] Preferably, the complete immersion time is 12 to 15 hours.
[0016] Preferably, the temperature of the preservative is 35-40°C.
[0017] The beneficial effects of the present invention are:
[0018] When water-soluble polyaniline is used in the mildew and corrosion prevention of furniture boards, mildew and rot will not appear until 3 months later, while boards that do not use water-soluble polyaniline will show mildew and rot within 1 month. DETAILED DESCRIPTION
[0019] The present invention provides a preservative, which is prepared from the following components in parts by weight: 90-110 parts of water, 15-25 parts of water-soluble polyaniline, 10-15 parts of triethanolamine, 1-3 parts of Tween-20, 3-8 parts of lignin and 3-8 parts of diatomaceous earth; more preferably, it is prepared from the following components in parts by weight: 100 parts of water, 20 parts of water-soluble polyaniline, 12 parts of triethanolamine, 2 parts of Tween-20, 5 parts of lignin and 5 parts of diatomaceous earth. In the present invention, the role of the lignin and diatomaceous earth is to improve the adhesion of the water-soluble polyaniline on the board, so as to achieve better anti-corrosion and anti-mildew effects.
[0020] The present invention also provides a method for preparing the preservative described in the above technical solution, comprising the following steps: mixing the water, water-soluble polyaniline, triethanolamine, Tween-20, lignin and diatomaceous earth to obtain the preservative. In the present invention, the mixing conditions preferably include: a rotation speed of 4000-5000 rpm and a time of 30-40 min.
[0021] The present invention also provides the use of the preservative described in the above technical solution in the mildew and corrosion prevention of furniture boards. In the present invention, the use preferably includes: completely immersing the furniture board in the preservative. In the present invention, the time of complete immersion is preferably 12 to 15 hours. In the present invention, the temperature of the preservative is preferably 35 to 40°C. The present invention does not specifically limit the type of the furniture board.
[0022] In order to further illustrate the present invention, the present invention is described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0023] Example 1
[0024] A method for preparing a preservative, comprising the following steps:
[0025] 100 parts of water, 20 parts of water-soluble polyaniline, 12 parts of triethanolamine, 2 parts of Tween-20, 5 parts of lignin and 5 parts of diatomaceous earth are mixed to obtain a preservative, wherein the mixing conditions are: a rotation speed of 5000 rpm and a time of 30 minutes.
[0026] Example 2
[0027] A method for preparing a preservative, comprising the following steps:
[0028] 90 parts of water, 25 parts of water-soluble polyaniline, 15 parts of triethanolamine, 1 part of Tween-20, 3 parts of lignin and 8 parts of diatomaceous earth are mixed to obtain a preservative, wherein the mixing conditions are: a rotation speed of 4500 rpm and a mixing time of 35 minutes.
[0029] Example 3
[0030] A method for preparing a preservative, comprising the following steps:
[0031] 110 parts of water, 15 parts of water-soluble polyaniline, 10 parts of triethanolamine, 3 parts of Tween-20, 8 parts of lignin and 3 parts of diatomaceous earth are mixed to obtain a preservative, wherein the mixing conditions are: a rotation speed of 4000 rpm and a time of 40 minutes.
[0032] Example 4
[0033] A method for preparing a preservative, comprising the following steps:
[0034] 90 parts of water, 15 parts of water-soluble polyaniline, 15 parts of triethanolamine, 1 part of Tween-20, 3 parts of lignin and 8 parts of diatomaceous earth are mixed to obtain a preservative, wherein the mixing conditions are: a rotation speed of 4000 rpm and a mixing time of 30 minutes.
[0035] Example 5
[0036] A method for preparing a preservative, comprising the following steps:
[0037] 105 parts of water, 22 parts of water-soluble polyaniline, 10 parts of triethanolamine, 2.5 parts of Tween-20, 6 parts of lignin and 7 parts of diatomaceous earth are mixed to obtain a preservative, wherein the mixing conditions are: a rotation speed of 5000 rpm and a time of 30 minutes.
[0038] Example 6
[0039] A method for preparing a preservative, comprising the following steps:
[0040] 95 parts of water, 16 parts of water-soluble polyaniline, 15 parts of triethanolamine, 1.5 parts of Tween-20, 4 parts of lignin and 6 parts of diatomaceous earth are mixed to obtain a preservative, wherein the mixing conditions are: a rotation speed of 4500 rpm and a mixing time of 35 minutes.
[0041] Comparative Example 1
[0042] A method for preparing a preservative, comprising the following steps:
[0043] 100 parts of water, 12 parts of triethanolamine, 2 parts of Tween-20, 5 parts of lignin and 5 parts of diatomaceous earth were mixed to obtain a preservative, wherein the mixing conditions were: a rotation speed of 5000 rpm and a time of 30 minutes.
[0044] Comparative Example 2
[0045] A method for preparing a preservative, comprising the following steps:
[0046] 90 parts of water, 15 parts of triethanolamine, 1 part of Tween-20, 3 parts of lignin and 8 parts of diatomaceous earth were mixed to obtain a preservative, wherein the mixing conditions were: a rotation speed of 4500 rpm and a mixing time of 35 minutes.
[0047] Comparative Example 3
[0048] A method for preparing a preservative, comprising the following steps:
[0049] 110 parts of water, 10 parts of triethanolamine, 3 parts of Tween-20, 8 parts of lignin and 3 parts of diatomaceous earth were mixed to obtain a preservative, wherein the mixing conditions were: a rotation speed of 4000 rpm and a time of 40 minutes.
[0050] The preservatives prepared in Examples 1 to 6 and Comparative Examples 1 to 3 were soaked in furniture boards, and the specific method was as follows:
[0051] The furniture board was completely immersed in the preservative for 15 hours at a temperature of 40°C and naturally air-dried. The air-dried board was then stored in an environment at a temperature of 35°C and an ambient humidity of 85%. The anti-mildew and anti-corrosion results are shown in Table 1.
[0052] Table 1 Anticorrosion and anti-mildew results of the board
[0053] Mildew and rot occur / d Example 1 128d Example 2 105d Example 3 110d Example 4 102d Example 5 113d Example 6 107d Comparative Example 1 30d Comparative Example 2 28d Comparative Example 3 25d
[0054] It can be seen from the above embodiments and comparative examples that when water-soluble polyaniline is used in the mildew and corrosion prevention of furniture boards, mildew and rot will not occur until 3 months later, while boards without water-soluble polyaniline will mildew and rot within 1 month.
[0055] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A preservative, characterized in that It is prepared from the following components in parts by weight: 90-110 parts of water, 15-25 parts of water-soluble polyaniline, 10-15 parts of triethanolamine, 1-3 parts of Tween-20, 3-8 parts of lignin and 3-8 parts of diatomaceous earth.
2. The preservative according to claim 1, characterized in that It is prepared from the following components in parts by weight: 100 parts of water, 20 parts of water-soluble polyaniline, 12 parts of triethanolamine, 2 parts of Tween-20, 5 parts of lignin and 5 parts of diatomaceous earth.
3. A method for preparing the preservative according to claim 1 or 2, characterized in that: The following steps are involved: The water, water-soluble polyaniline, triethanolamine, Tween-20, lignin and diatomaceous earth are mixed to obtain a preservative.
4. The preparation method according to claim 3, characterized in that: The mixing conditions include: a rotation speed of 4000 to 5000 rpm and a mixing time of 30 to 40 minutes.
5. Use of the preservative according to claim 1 or 2 in the mildew and corrosion prevention of furniture boards.
6. The use according to claim 5, characterized in that: The application comprises: completely immersing the furniture board in a preservative.
7. The use according to claim 6, characterized in that: The complete immersion time is 12 to 15 hours.
8. The use according to claim 6, characterized in that: The temperature of the preservative is 35-40°C.
Citation Information
Patent Citations
Long-acting wood preservative
CN102069517A
Drug-carrying polymer wood / bamboo modifier, and production and application methods thereof
CN105622828A
Anti-corrosion adhesive for finger-jointed board wood and preparation method of anti-corrosion adhesive
CN113249069A
Lignin-based wood reinforcing preservative as well as preparation method and application thereof
CN115556205A