High-wear-resistance antibacterial jean fabric as well as preparation method and application thereof

By using a multi-layer structure of cuprous oxide-redox graphene polyester and spandex covered yarn, nano-silver and polyvinyl alcohol composite layer and cotton and viscose blended yarn in denim fabrics, the problem that traditional denim fabrics are prone to wrinkles is solved , easy shrinkage and strong hygroscopicity, it achieves high wear resistance, breathability and antibacterial properties, improving wearing comfort and durability.

CN118769644AActive Publication Date: 2024-10-15GUANGDONG ASIATEX TEXTILES CO LTD

Patent Information

Application Number
CN202410948988.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-15
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

Traditional pure cotton denim fabrics are prone to wrinkles and shrinkage. They have strong hygroscopicity but poor shape retention. They are difficult to wick away when sweating a lot, causing stickiness and stuffiness, and can easily accelerate the formation of bacteria.

Method used

It uses a highly wear-resistant antibacterial fabric woven from cuprous oxide-redox graphene polyester and spandex covered yarn, nano-silver and polyvinyl alcohol composite layer and cotton and viscose blended yarn. Through cuprous oxide-redox graphene The preparation method of polyester and electrospinning technology form a multi-layer structure to improve the wear resistance and antibacterial properties of the fabric.

Benefits of technology

It achieves high wear resistance, breathability and antibacterial properties of the fabric, improves wearing comfort and durability, and is suitable for long-term wear, especially in labor-intensive occupations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118769644A_ABST
    Figure CN118769644A_ABST
Patent Text Reader

Abstract

The invention relates to a highly wear-resistant antibacterial jean fabric as well as a preparation method and application thereof, and belongs to the technical field of jean fabrics. The fabric comprises a first wear-resistant antibacterial layer, a bonding layer, a second wear-resistant antibacterial layer and a breathable layer which are sequentially arranged, wherein the first wear-resistant antibacterial layer is formed by weaving covered yarns of cuprous oxide-redox graphene terylene and spandex; the wrap yarn takes spandex as a core yarn and cuprous oxide-redox graphene terylene as an outer wrapping fiber; the second wear-resistant antibacterial layer is a composite layer of nano-silver and polyvinyl alcohol; the breathable layer is formed by weaving cotton and viscose blended yarn. The fabric is good in wear resistance, good in air permeability and moisture absorption and good in comfort.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of denim fabrics, and in particular to a highly wear-resistant and antibacterial denim fabric and a preparation method and application thereof. Background Art

[0002] Traditional denim fabrics are mostly pure cotton, and the warp and weft yarns are all woven with pure cotton yarns. Cotton fiber is the most common natural cellulose fiber, slender and soft, with a multi-layered structure with a central cavity, and a natural "twist" in the longitudinal direction. There are many hydrophilic groups (-OH) on the cellulose macromolecules, which are highly hygroscopic, so cotton fabrics are soft and skin-friendly, and have good hygroscopicity and dyeability. Pure cotton denim fabrics have strong hygroscopicity, are comfortable to wear, have bright colors, and have a rich variety of patterns. However, pure cotton denim fabrics are easy to wrinkle, shrink, and have poor shape retention. When the human body sweats a lot, the sweat absorbed by the fabric is not easy to be discharged, and the clothes become thick and heavy. Wearing for a long time will make you feel sticky and stuffy, and it will also accelerate the formation of harmful bacteria. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a highly wear-resistant and antibacterial denim fabric and a preparation method and application thereof, which can improve the wear resistance of the fabric, and has good air permeability and moisture absorption, and has good comfort.

[0004] To achieve the above object, the technical solution adopted by the present invention is:

[0005] In a first aspect, the present invention provides a highly wear-resistant and antibacterial denim fabric, comprising a first wear-resistant and antibacterial layer, an adhesive layer, a second wear-resistant and antibacterial layer, and a breathable layer arranged in sequence; wherein the first wear-resistant and antibacterial layer is woven from coated yarns of cuprous oxide-redox graphene polyester and spandex; the coated yarn has spandex as a core yarn and cuprous oxide-redox graphene polyester as an outer fiber; the second wear-resistant and antibacterial layer is a composite layer of nanosilver and polyvinyl alcohol; and the breathable layer is woven from a blended yarn of cotton and viscose.

[0006] Preferably, the method for preparing the cuprous oxide-redox graphene polyester comprises the following steps:

[0007] (1) mixing polyester fabric with dopamine (DA) under alkaline conditions to carry out in-situ polymerization reaction, and obtaining polydopamine (PDA)-polyester (PET) fabric after the reaction;

[0008] (2) immersing the polydopamine-polyester fabric in a graphene oxide (GO) dispersion, taking out the fabric and drying it to obtain a graphene oxide-polydopamine-polyester fabric;

[0009] (3) immersing the graphene oxide-polydopamine-polyester fabric in a copper sulfate solution, then dropping an alkali solution and a reducing agent, taking out the fabric and drying it to obtain the cuprous oxide (Cu2O)-redox graphene (rGO) polyester.

[0010] Cuprous oxide (Cu2O) is a common antibacterial agent, but the copper ion release rate of cuprous oxide is uncontrollable, which limits its application in antibacterial materials. Redox graphene has high conductivity and carrier mobility. As a carrier of cuprous oxide, it can improve the dispersibility of cuprous oxide in water and prevent its agglomeration, thereby improving the sustained release performance of cuprous oxide in water. The polydopamine layer formed by the oxidative self-polymerization of dopamine has good interfacial adhesion, so that cuprous oxide can be evenly attached to the surface of polyester (PET), thus giving the polyester material a long-lasting antibacterial property.

[0011] Preferably, the mass concentration of the dopamine solution is 0.2-0.5 g / L.

[0012] Preferably, the mass concentration of the graphene oxide dispersion is 1 to 3 g / L.

[0013] Preferably, the molar concentration of the copper sulfate solution is 0.005-0.01 mol / L.

[0014] Preferably, the molar concentration of the alkaline solution is 1 to 2 mol / L, and the molar concentration of the reducing agent is 1 to 2 mol / L.

[0015] Preferably, the linear density of the coated yarn is 20-40 tex, and the linear density of the spandex is 3-4 tex.

[0016] Preferably, the linear density of the cotton is 20-40 tex, and the linear density of the viscose fiber is 20-30 tex.

[0017] Preferably, the mass ratio of cotton to viscose is (40-60): (40-60). Cotton fiber has high strength and wear resistance, while viscose fiber increases the softness and drape of the fabric. The combination of the two can improve the overall durability of the fabric. Within the above range, a fabric with high strength and moisture absorption effect can be obtained.

[0018] In a second aspect, the present invention provides a method for preparing the highly wear-resistant and antibacterial denim fabric, comprising the following steps:

[0019] S1 uses spandex as the core yarn and cuprous oxide-redox graphene polyester as the outer fiber to form a coated yarn, and then weaves the coated yarn into a fabric to obtain the first wear-resistant and antibacterial layer;

[0020] S2 weaves the blended yarn of cotton and viscose into fabric to obtain a breathable layer;

[0021] S3 mixes nanosilver and polyvinyl alcohol to prepare an electrospinning solution;

[0022] S4: spraying the electrospinning solution onto the surface of the breathable layer by using electrospinning technology to solidify the solution, thereby obtaining the second wear-resistant and antibacterial layer;

[0023] S5: coating glue on the surface of the second wear-resistant and antibacterial layer, and then bonding the second wear-resistant and antibacterial layer to the first wear-resistant and antibacterial layer through an adhesive layer to obtain the highly wear-resistant and antibacterial denim fabric.

[0024] Preferably, the electrospinning solution comprises the following components by weight: 1-3 parts of nanosilver, 7-9 parts of polyvinyl alcohol, 5-8 parts of formic acid, 10-15 parts of acetic acid, 10-15 parts of glue and 260-440 parts of water. The present invention adopts electrospinning technology to physically composite nanosilver and polyvinyl alcohol, which has a simple process, is non-toxic and pollution-free. Then, in order to make the composite layer of nanosilver and polyvinyl alcohol better composite with the breathable layer, glue is added to the electrospinning solution, and then the electrospinning solution is electrospun and deposited on the breathable layer to form a composite layer of nanosilver and polyvinyl alcohol, which is the second wear-resistant and antibacterial layer.

[0025] Preferably, in step S4, the electrospinning parameters are: spinning speed 0.2-1 mL / h, spinning distance 10-15 cm, and spinning voltage 20-30 kV.

[0026] In a third aspect, the present invention provides the use of highly wear-resistant and antibacterial denim fabric in the preparation of denim clothing. Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The first wear-resistant and antibacterial layer in the denim fabric of the present invention is a coated yarn of cuprous oxide-redox graphene polyester and spandex, so that the yarn not only has the wear-resistant characteristics of the spandex core yarn, but also can improve its wear resistance and comfort performance by utilizing the characteristics of the outer fiber of cuprous oxide-redox graphene polyester. The second wear-resistant and antibacterial layer is a composite layer of nanosilver and polyvinyl alcohol. Nanosilver can play a good antibacterial effect. Since polyvinyl alcohol has high strength and high modulus, adding it to the fabric can improve the mechanical strength and durability of the fabric. The breathable layer is the innermost layer. Cotton fiber is well-known for its softness, breathability and good hygroscopicity, while viscose fiber has good softness and smooth feel. This composite fabric can provide higher wearing comfort. Therefore, when wearing this fabric, the human body can sweat and discharge moisture in time, thereby improving the wearing comfort and avoiding the growth of bacteria in sweat.

[0028] (2) The denim fabric of the present invention is comfortable, durable, and antibacterial, and is suitable for long-term wear, especially for front-line workers and other occupations with high labor intensity. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a layered structure diagram of the denim fabric of the present invention;

[0030] In the figure: 1. first wear-resistant and antibacterial layer; 2. adhesive layer; 3. second wear-resistant and antibacterial layer; 4. breathable layer. DETAILED DESCRIPTION

[0031] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0032] The reagents used in the following examples and comparative examples are as follows, wherein:

[0033] Graphene oxide: manufacturer is Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., brand number 103080;

[0034] Nano silver (powder): manufacturer is Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., brand number 100937;

[0035] Glue: water-based polyurethane glue, the manufacturer is Hefei Dibang Nanotechnology Co., Ltd., brand name is QTJS-1671;

[0036] Dopamine: The manufacturer is Henan Puhui Tiancheng Biotechnology Co., Ltd.;

[0037] Polyvinyl alcohol: The manufacturer is Shanghai Yanze Chemical Co., Ltd.

[0038] Formic acid: manufacturer is Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0039] Acetic acid: The manufacturer is Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0040] Cuprous oxide: The manufacturer is Taixing Smelter Co., Ltd., the brand is: Cuprous oxide (calcination method);

[0041] Anhydrous copper sulfate: the manufacturer is Taixing Smelter Co., Ltd.;

[0042] Pyrrole: The manufacturer is Henan Wanxiang Chemical Co., Ltd.

[0043] Unless otherwise specified, other materials, reagents, etc. used in the examples can be obtained from commercial sources.

[0044] Example 1

[0045] A highly wear-resistant and antibacterial denim fabric, such as Figure 1As shown, it includes a first wear-resistant antibacterial layer 1, an adhesive layer 2, a second wear-resistant antibacterial layer 3, and a breathable layer 4 arranged in sequence; wherein the first wear-resistant antibacterial layer 1 is woven from a coated yarn of cuprous oxide-redox graphene polyester and spandex (3tex / 10F); the coated yarn is spandex as the core yarn and cuprous oxide-redox graphene polyester as the outer fiber; the second wear-resistant antibacterial layer 3 is a composite layer of nanosilver and polyvinyl alcohol; the breathable layer 4 is woven from a blended yarn of cotton (25tex) and viscose (25tex). The mass ratio of cotton to viscose is 50:50. The linear density of the coated yarn is 30tex.

[0046] Wherein, the preparation method of the cuprous oxide-redox graphene polyester comprises the following steps:

[0047] (1) Polyester fabric and dopamine are mixed at pH = 13, and an in-situ polymerization reaction is carried out to obtain polydopamine-polyester fabric after 5 hours of reaction; the mass concentration of the dopamine solution is 0.3 g / L.

[0048] (2) immersing the polydopamine-polyester fabric in a graphene oxide dispersion, taking out the fabric and drying it to obtain a graphene oxide-polydopamine-polyester fabric; the mass concentration of the graphene oxide dispersion is 2 g / L.

[0049] (3) Immersing the graphene oxide-polydopamine-polyester fabric in a copper sulfate solution, then dripping an alkali solution and a reducing agent, taking out the fabric and drying it to obtain the cuprous oxide-redox graphene polyester. The molar concentration of the copper sulfate solution is 0.006 mol / L. The molar concentration of the alkali solution is 1-2 mol / L, and the reducing agent is a pyrrole solution, and its molar concentration is 1.1 mol / L.

[0050] The method for preparing the highly wear-resistant and antibacterial denim fabric comprises the following steps:

[0051] S1 uses spandex as the core yarn and cuprous oxide-redox graphene polyester as the outer fiber to form a coated yarn, and then the coated yarn is woven into a fabric to obtain the first wear-resistant and antibacterial layer 1;

[0052] S2 weaves the blended yarn of cotton and viscose into a fabric to obtain a breathable layer 4;

[0053] S3: mixing nanosilver and polyvinyl alcohol to prepare an electrospinning solution; wherein the electrospinning solution comprises the following components in parts by weight: 2 parts of nanosilver, 8 parts of polyvinyl alcohol, 6 parts of formic acid, 12 parts of acetic acid, 12 parts of glue and 300 parts of water.

[0054] S4 sprays the electrospinning solution onto the surface of the breathable layer 4 by using the electrospinning technology for curing to obtain the second wear-resistant and antibacterial layer 3; the electrospinning parameters are: spinning speed 0.5 mL / h, spinning distance 12 cm, spinning voltage 25 kV.

[0055] S5: coating glue on the surface of the second wear-resistant and antibacterial layer 3, and then laminating the second wear-resistant and antibacterial layer 3 with the first wear-resistant and antibacterial layer 1 through the adhesive layer 2 to obtain the highly wear-resistant and antibacterial denim fabric.

[0056] Example 2

[0057] A highly wear-resistant and antibacterial denim fabric, such as Figure 1 As shown, it includes a first wear-resistant antibacterial layer 1, an adhesive layer 2, a second wear-resistant antibacterial layer 3, and a breathable layer 4 arranged in sequence; wherein the first wear-resistant antibacterial layer 1 is woven from a coated yarn of cuprous oxide-redox graphene polyester and spandex (3tex / 10F); the coated yarn is spandex as the core yarn and cuprous oxide-redox graphene polyester as the outer fiber; the second wear-resistant antibacterial layer 3 is a composite layer of nanosilver and polyvinyl alcohol; the breathable layer 4 is woven from a blended yarn of cotton (20tex) and viscose (20tex). The mass ratio of cotton to viscose is 40:60. The linear density of the coated yarn is 20tex.

[0058] Wherein, the preparation method of the cuprous oxide-redox graphene polyester comprises the following steps:

[0059] (1) Polyester fabric and dopamine are mixed under alkaline conditions to carry out in-situ polymerization reaction, and polydopamine-polyester fabric is obtained after the reaction; the mass concentration of the dopamine solution is 0.2 g / L.

[0060] (2) immersing the polydopamine-polyester fabric in a graphene oxide dispersion, taking out the fabric and drying it to obtain a graphene oxide-polydopamine-polyester fabric; the mass concentration of the graphene oxide dispersion is 1 g / L.

[0061] (3) Immersing the graphene oxide-polydopamine-polyester fabric in a copper sulfate solution, then dripping an alkali solution and a reducing agent, taking out the fabric and drying it to obtain the cuprous oxide-redox graphene polyester. The molar concentration of the copper sulfate solution is 0.005 mol / L. The molar concentration of the alkali solution is 1 mol / L, and the reducing agent is a pyrrole solution, and its molar concentration is 1 mol / L.

[0062] The method for preparing the highly wear-resistant and antibacterial denim fabric comprises the following steps:

[0063] S1 uses spandex as the core yarn and cuprous oxide-redox graphene polyester as the outer fiber to form a coated yarn, and then the coated yarn is woven into a fabric to obtain the first wear-resistant and antibacterial layer 1;

[0064] S2 weaves the blended yarn of cotton and viscose into a fabric to obtain a breathable layer 4;

[0065] S3: mixing nanosilver and polyvinyl alcohol to prepare an electrospinning solution; wherein the electrospinning solution comprises the following components in parts by weight: 3 parts of nanosilver, 9 parts of polyvinyl alcohol, 8 parts of formic acid, 15 parts of acetic acid, 15 parts of glue and 440 parts of water.

[0066] S4 sprays the electrospinning solution onto the surface of the breathable layer 4 by using the electrospinning technology for curing to obtain the second wear-resistant and antibacterial layer 3; the electrospinning parameters are: spinning speed 1 mL / h, spinning distance 15 cm, spinning voltage 30 kV.

[0067] S5: coating glue on the surface of the second wear-resistant and antibacterial layer 3, and then laminating the second wear-resistant and antibacterial layer 3 with the first wear-resistant and antibacterial layer 1 through the adhesive layer 2 to obtain the highly wear-resistant and antibacterial denim fabric.

[0068] Example 3

[0069] A highly wear-resistant and antibacterial denim fabric, such as Figure 1 As shown, it includes a first wear-resistant antibacterial layer 1, an adhesive layer 2, a second wear-resistant antibacterial layer 3, and a breathable layer 4 arranged in sequence; wherein the first wear-resistant antibacterial layer 1 is woven from a coated yarn of cuprous oxide-redox graphene polyester and spandex (4tex / 10F); the coated yarn is spandex as the core yarn and cuprous oxide-redox graphene polyester as the outer fiber; the second wear-resistant antibacterial layer 3 is a composite layer of nanosilver and polyvinyl alcohol; the breathable layer 4 is woven from a blended yarn of cotton (40tex) and viscose (40tex). The linear density of the coated yarn is 40tex. The mass ratio of cotton to viscose is 60:40.

[0070] Wherein, the preparation method of the cuprous oxide-redox graphene polyester comprises the following steps:

[0071] (1) Polyester fabric and dopamine are mixed at pH = 13 to perform an in-situ polymerization reaction to obtain polydopamine-polyester fabric; the mass concentration of the dopamine solution is 0.5 g / L.

[0072] (2) immersing the polydopamine-polyester fabric in a graphene oxide dispersion, taking out the fabric and drying it to obtain a graphene oxide-polydopamine-polyester fabric; the mass concentration of the graphene oxide dispersion is 3 g / L.

[0073] (3) Immersing the graphene oxide-polydopamine-polyester fabric in a copper sulfate solution, then dripping an alkali solution and a reducing agent, taking out the fabric and drying it to obtain the cuprous oxide-redox graphene polyester. The molar concentration of the copper sulfate solution is 0.01 mol / L. The molar concentration of the alkali solution is 2 mol / L, and the reducing agent is a pyrrole solution, and its molar concentration is 2 mol / L.

[0074] The method for preparing the highly wear-resistant and antibacterial denim fabric comprises the following steps:

[0075] S1 uses spandex as the core yarn and cuprous oxide-redox graphene polyester as the outer fiber to form a coated yarn, and then the coated yarn is woven into a fabric to obtain the first wear-resistant and antibacterial layer 1;

[0076] S2 weaves the blended yarn of cotton and viscose into a fabric to obtain a breathable layer 4;

[0077] S3: mixing nanosilver and polyvinyl alcohol to prepare an electrospinning solution; wherein the electrospinning solution comprises the following components in parts by weight: 1 part of nanosilver, 7 parts of polyvinyl alcohol, 5 parts of formic acid, 10 parts of acetic acid, 10 parts of glue and 260 parts of water.

[0078] S4 sprays the electrospinning solution onto the surface of the breathable layer 4 by using the electrospinning technology for curing to obtain the second wear-resistant and antibacterial layer 3; the electrospinning parameters are: spinning speed 0.2 mL / h, spinning distance 10 cm, spinning voltage 20 kV.

[0079] S5: coating glue on the surface of the second wear-resistant and antibacterial layer 3, and then laminating the second wear-resistant and antibacterial layer 3 with the first wear-resistant and antibacterial layer 1 through the adhesive layer 2 to obtain the highly wear-resistant and antibacterial denim fabric.

[0080] Example 4

[0081] The difference between Example 4 and Example 1 is that the mass ratio of cotton to viscose in the breathable layer 4 of Example 4 is 30:70.

[0082] Example 5

[0083] The difference between Example 5 and Example 1 is that the mass ratio of cotton to viscose in the breathable layer 4 of Example 5 is 70:30.

[0084] Example 6

[0085] The difference between Example 6 and Example 1 is that the preparation method of cuprous oxide-redox graphene polyester in Example 6 does not contain step (1), that is, the polyester fabric does not undergo an in-situ polymerization reaction of dopamine.

[0086] Comparative Example 1

[0087] The difference between Comparative Example 1 and Example 1 is that the denim fabric of Comparative Example 1 is not provided with the first wear-resistant antibacterial layer 1 and the adhesive layer 2 .

[0088] Comparative Example 2

[0089] The difference between Comparative Example 2 and Example 1 is that the denim fabric of Comparative Example 2 is not provided with the second wear-resistant and antibacterial layer 3 .

[0090] Comparative Example 3

[0091] The difference between Comparative Example 3 and Example 1 is that the denim fabric of Comparative Example 3 is not provided with a breathable layer 4 .

[0092] Comparative Example 4

[0093] The difference between Comparative Example 4 and Example 1 is that the first wear-resistant antibacterial layer 1 of Comparative Example 4 is woven from a blended yarn of cuprous oxide-redox graphene polyester and spandex.

[0094] Comparative Example 5

[0095] The difference between Comparative Example 5 and Example 1 is that the first wear-resistant antibacterial layer 1 of Comparative Example 5 is woven from cuprous oxide polyester and spandex coated yarn, that is, the polyester does not contain redox graphene.

[0096] Comparative Example 6

[0097] The difference between Comparative Example 6 and Example 1 is that the first wear-resistant antibacterial layer 1 of Comparative Example 6 is woven from polyester and spandex coated yarns.

[0098] Comparative Example 7

[0099] The difference between Comparative Example 7 and Example 1 is that the covering yarn of the first wear-resistant antibacterial layer 1 of Comparative Example 7 is cuprous oxide-redox graphene polyester as the core yarn and spandex as the outer covering fiber.

[0100] Comparative Example 8

[0101] The difference between Comparative Example 8 and Example 1 is that nanosilver is not added to the second wear-resistant antibacterial layer 3 of Comparative Example 8.

[0102] Comparative Example 9

[0103] The difference between Comparative Example 9 and Example 1 is that: Comparative Example 9 does not have the second wear-resistant antibacterial layer 3, and the breathable layer 4 is immersed in the nanosilver solution, and the mass concentration of the nanosilver solution is the same as that of Example 1.

[0104] Performance Testing

[0105] 1. Antibacterial performance test

[0106] Referring to GB / T209443-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method", the denim fabrics of Examples 1 to 6 and Comparative Examples 1 to 9 were tested for antibacterial effects, and the test strains were Candida albicans (ATCC10231) and Staphylococcus aureus (ATCC6538), respectively. Specific data are shown in Table 1.

[0107] Table 1 Antibacterial performance data of each group of samples

[0108]

[0109]

[0110] As can be seen from Table 1, the denim fabric of Example 1 has the best antibacterial performance. The antibacterial performance of Examples 2 to 4 is relatively similar. In Example 6, the cuprous oxide-redox graphene polyester does not contain polydopamine, resulting in poor adhesion of cuprous oxide to polyester, thereby significantly reducing the antibacterial performance. The first wear-resistant antibacterial layer 1 of Comparative Example 4 is woven from a blended yarn of cuprous oxide-redox graphene polyester and spandex, resulting in a reduction in the contact area between the cuprous oxide-redox graphene polyester and the germs, thereby reducing the antibacterial performance. The first wear-resistant antibacterial layer 1 of Comparative Example 5 does not contain redox graphene, and cuprous oxide lacks a carrier, which makes it difficult to disperse evenly in polyester, so its antibacterial performance is also significantly reduced. The polyester in the first wear-resistant antibacterial layer 1 of Comparative Example 6 is not modified, and its antibacterial performance is similar to that of the first wear-resistant antibacterial layer 1 in Comparative Example 1, which shows that the polyester modified with cuprous oxide and redox graphene is the key to improving the antibacterial performance of the fabric.

[0111] Comparative Example 2 does not have a second wear-resistant antibacterial layer 3, and its antibacterial performance is similar to that of Comparative Example 8, indicating that the addition of nanosilver in the second wear-resistant antibacterial layer 3 is an important factor in its antibacterial performance. Comparative Example 9 does not have a second wear-resistant antibacterial layer 3, but directly immerses the breathable layer 4 in the nanosilver solution, and its antibacterial performance is also reduced. This is because nanosilver is not well dispersed on the cotton / viscose composite fiber, and electrostatic spinning of nanosilver and polyvinyl alcohol can promote the uniform adhesion of nanosilver on the breathable layer 4 to improve the antibacterial performance.

[0112] 2. Moisture absorption and quick drying performance test

[0113] The moisture absorption and quick drying performance of the denim fabrics of Examples 1 to 6 and Comparative Examples 1 to 9 were tested respectively with reference to GB / T21655.1-2008 "Evaluation of moisture absorption and quick drying performance Part 1: Single item combination test method". Specific data are shown in Table 2.

[0114] Table 2 Moisture absorption and quick drying performance data of each group of samples

[0115]

[0116] As can be seen from Table 2, compared with Examples 4 and 5, Example 1 has significantly improved moisture absorption and quick-drying performance, indicating that the mass ratio of cotton to viscose is limited to (40-60): (40-60) to make the fabric have the best air permeability. The first wear-resistant antibacterial layer 1 of Example 6 does not contain polydopamine, resulting in a decrease in the adhesion between cuprous oxide and redox graphene, and poor dispersion, which affects the air permeability of the fabric. In Comparative Examples 1-2, due to the lack of the first wear-resistant antibacterial layer 1 and the second wear-resistant antibacterial layer 3, the air permeability is not much different from that of Example 1, indicating that the first wear-resistant antibacterial layer 1 and the second wear-resistant antibacterial layer 3 have no significant effect on the moisture absorption effect of the fabric.

[0117] In Comparative Example 3, due to the lack of breathable layer 4, its moisture absorption and air permeability are significantly reduced, indicating that the breathable layer 4 is the main parameter affecting the breathability and moisture absorption performance of the fabric.

[0118] The moisture absorption properties of Comparative Examples 4 to 6 are not much different from those of Example 1, indicating that the type of yarn in the first wear-resistant antibacterial layer 1, whether it contains redox graphene, and whether it contains cuprous oxide have little effect on the air permeability of the fabric.

[0119] In Comparative Example 7, cuprous oxide-redox graphene polyester is used as the core fiber and spandex is used as the outer fiber. Its hygroscopicity is significantly lower than that of Example 1, because spandex fabric has the disadvantages of poor hygroscopicity and slow water evaporation. Therefore, in Example 1, polyester is selected as the outer fiber, which improves the wear resistance and antibacterial properties, and the moisture of polyester is easy to evaporate, so it has the characteristics of quick drying.

[0120] The performance of Comparative Example 8 is similar to that of Example 1, indicating that the addition of nanosilver does not affect the moisture absorption and breathability of the fabric.

[0121] Comparative Example 9 is to directly immerse the breathable layer 4 in the nanosilver solution. Its moisture absorption and quick-drying performance is better than that of Example 1, but the other wear resistance and antibacterial properties are reduced.

[0122] 3. Mechanical properties test

[0123] According to GB / T 3917.1-2009 "Tear properties of textile fabrics", the tear strength of the denim fabrics of Examples 1 to 6 and Comparative Examples 1 to 9 was tested by the impact pendulum method, and the wear resistance of the denim fabrics of Examples 1 to 6 and Comparative Examples 1 to 9 was tested according to GB / T 4802.2-2008 "Determination of pilling properties of textile fabrics Part 2: Modified Martindale method", and each sample was rated. The rating table is shown in Table 3. The specific test data is shown in Table 4.

[0124] Table 3 Wear resistance rating table

[0125]

[0126] Table 4 Mechanical strength data of each group of samples

[0127]

[0128]

[0129] As can be seen from Table 4, Example 1 is the example with the best mechanical properties. In Example 6, the cuprous oxide-redox graphene polyester does not contain polydopamine, resulting in poor adhesion of cuprous oxide and redox graphene to the polyester, and its mechanical properties are also slightly reduced.

[0130] The first wear-resistant antibacterial layer 1 of comparative example 4 is woven from a blended yarn of cuprous oxide-redox graphene polyester and spandex, resulting in a reduction in the contact area between the cuprous oxide-redox graphene polyester and the friction surface, thereby reducing the mechanical properties. The first wear-resistant antibacterial layer 1 of comparative example 5 does not contain redox graphene, and cuprous oxide lacks a carrier, so its stability in polyester is reduced, which slightly affects the mechanical properties. The polyester in the first wear-resistant antibacterial layer 1 of comparative example 6 is not modified, and its mechanical properties are close to those in Example 1, indicating that the modified polyester can improve the mechanical properties of the fabric to a certain extent. The coated yarn of the first wear-resistant antibacterial layer 1 of comparative example 7 is cuprous oxide-redox graphene polyester as the core yarn and spandex as the outer fiber. Because the strength of spandex itself is better than that of polyester, and its antibacterial properties are combined, it is appropriate to use spandex as the core yarn to provide strength in the coated yarn, and cuprous oxide-redox graphene polyester as the outer fiber to provide hygroscopicity and antibacterial properties.

[0131] Comparative Example 1 does not have the first wear-resistant antibacterial layer 1, and its mechanical properties are significantly reduced, because polyester and spandex have good strength and wear resistance. Similarly, Comparative Examples 2 and 9 do not have the second wear-resistant antibacterial layer 3, and their mechanical properties are also significantly reduced, because polyvinyl alcohol has high strength and high modulus, and adding it to the fabric can improve the mechanical strength and durability of the fabric.

[0132] In summary, the denim fabric of the present invention can provide a high wearing comfort. Therefore, when wearing the fabric, the human body can sweat and be discharged in time, thereby improving the wearing comfort and preventing the growth of bacteria in the sweat. In addition, the denim fabric has good wear resistance and is suitable for long-term wear, especially for front-line workers and other occupations with high labor intensity.

[0133] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A highly wear-resistant and antibacterial denim fabric, characterized in that: It comprises a first wear-resistant antibacterial layer, an adhesive layer, a second wear-resistant antibacterial layer and a breathable layer which are arranged in sequence; wherein the first wear-resistant antibacterial layer is woven from coated yarns of cuprous oxide-redox graphene polyester and spandex; the coated yarns are made of spandex as core yarn and cuprous oxide-redox graphene polyester as outer covering fiber; the second wear-resistant antibacterial layer is a composite layer of nano-silver and polyvinyl alcohol; the breathable layer is woven from cotton and viscose blended yarn.

2. The highly wear-resistant and antibacterial denim fabric according to claim 1, characterized in that: The preparation method of the cuprous oxide-redox graphene polyester comprises the following steps: (1) mixing polyester fabric and dopamine under alkaline conditions to perform an in-situ polymerization reaction to obtain polydopamine-polyester fabric; (2) immersing the polydopamine-polyester fabric into a graphene oxide dispersion, taking out the fabric and drying it to obtain a graphene oxide-polydopamine-polyester fabric; (3) immersing the graphene oxide-polydopamine-polyester fabric in a copper sulfate solution, then dropping an alkali solution and a reducing agent, taking out the fabric and drying it to obtain the cuprous oxide-redox graphene polyester.

3. The highly wear-resistant and antibacterial denim fabric according to claim 2, characterized in that: Including at least one of (I) to (III): (I) The mass concentration of the dopamine solution is 0.2 to 0.5 g / L; (II) the mass concentration of the graphene oxide dispersion is 1 to 3 g / L; (III) the molar concentration of the copper sulfate solution is 0.005 to 0.01 mol / L; (V) The molar concentration of the alkaline solution is 1 to 2 mol / L, and the molar concentration of the reducing agent is 1 to 2 mol / L.

4. The highly wear-resistant and antibacterial denim fabric according to claim 1, characterized in that: The linear density of the coated yarn is 20-40 tex, and the linear density of the spandex is 3-4 tex.

5. The highly wear-resistant and antibacterial denim fabric according to claim 1 or 2, characterized in that: The linear density of the cotton is 20-40 tex, and the linear density of the viscose fiber is 20-30 tex.

6. The highly wear-resistant and antibacterial denim fabric according to claim 1, characterized in that: The mass ratio of cotton to viscose is (40-60): (40-60).

7. The method for preparing the highly wear-resistant and antibacterial denim fabric according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1 uses spandex as the core yarn and cuprous oxide-redox graphene polyester as the outer fiber to form a coated yarn, and then weaves the coated yarn into a fabric to obtain the first wear-resistant and antibacterial layer; S2 weaves the blended yarn of cotton and viscose into fabric to obtain a breathable layer; S3 mixes nanosilver and polyvinyl alcohol to prepare an electrospinning solution; S4: spraying the electrospinning solution onto the surface of the breathable layer by using electrospinning technology to solidify the solution, thereby obtaining the second wear-resistant and antibacterial layer; S5: coating glue on the surface of the second wear-resistant and antibacterial layer, and then bonding the second wear-resistant and antibacterial layer to the first wear-resistant and antibacterial layer through an adhesive layer to obtain the highly wear-resistant and antibacterial denim fabric.

8. The method for preparing the highly wear-resistant and antibacterial denim fabric according to claim 7, characterized in that: The electrostatic spinning solution comprises the following components in parts by weight: 1-3 parts of nano silver, 7-9 parts of polyvinyl alcohol, 5-8 parts of formic acid, 10-15 parts of acetic acid, 10-15 parts of glue and 260-440 parts of water.

9. The method for preparing the highly wear-resistant and antibacterial denim fabric according to claim 7, characterized in that: In the step S4, the electrospinning parameters are: spinning speed 0.2-1 mL / h, spinning distance 10-15 cm, and spinning voltage 20-30 kV.

10. Use of the highly wear-resistant and antibacterial denim fabric according to any one of claims 1 to 6 in the preparation of denim clothing.

Citation Information

Patent Citations

  • Dual-layer double-faced four-side elastic fabric

    CN104313760A

  • Antimicrobial waterborne polyurethane nanofiber film and preparation method

    CN106988016A

  • Antistatic graphene coating fabric and preparation method thereof

    CN108625158A

  • Antibacterial insole with polyvinyl alcohol nano fiber film containing nano silver particles and preparation method of antibacterial insole

    CN109330099A

  • Preparation method of antibacterial, antistatic and anti-ultraviolet polyurethane synthetic leather

    CN115283227A

Cited By

  • Wear-resistant antibacterial jean fabric and treatment method thereof

    CN120719539A