Method for purifying low-grade crystalline flake graphite ore through combination of ultrasonic pretreatment and cationic activation
Through the combined use of ultrasonic pretreatment and cationic activator, the problem of insufficient dissociation of graphite ore and impurities in the flotation process of low-grade flake graphite ore is solved, the fixed carbon content and graphite recovery rate are improved, and the number of selection times is reduced. and grinding process, achieving more efficient flake graphite purification and environmental protection effects.
Patent Information
- Application Number
- CN202410982731.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-22
AI Technical Summary
For low-grade flake graphite ore, the graphite ore and impurities are not fully dissociated in the conventional flotation process, resulting in serious inclusions in the flotation process, multiple selection times, a long process, and multi-stage grinding causing damage to large-sized flake graphite.
Ultrasonic pretreatment combined with cationic activation is used to purify low-grade flake graphite ore. Through ultrasonic pretreatment and the use of cationic activators, the dissociation of graphite ore and impurities is promoted, the fixed carbon content of the rough concentrate is increased, and the number of selection times is reduced. , protect large size graphite flakes.
It increases the fixed carbon content of the flotation concentrate, reduces the number of selections and grinding processes, reduces the amount of chemicals used, increases the graphite recovery rate and production efficiency, and reduces environmental pollution.
Smart Images

Figure CN118771369A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mineral processing, and in particular relates to a method for purifying low-grade flake graphite ore by combining ultrasonic pretreatment with cationic activation. Background Art
[0002] As a strategic resource, graphite is widely used in new energy, electronics, medical treatment, metallurgy, aerospace and other fields due to its unique structure and characteristics of thermal conductivity, electrical conductivity, lubrication, high temperature resistance and stable chemical properties. It has become an indispensable non-metallic material in the development of modern industry and high-tech industries, and occupies an increasingly important position in the global economic development.
[0003] Natural graphite ore is mainly divided into flake graphite and microcrystalline graphite. Flake graphite is mainly used as battery raw materials and cutting-edge technology raw materials such as atomic energy. With the continuous development of science and technology, high-grade flake graphite ore is becoming increasingly scarce. At the same time, many countries have listed flake graphite ore as a strategic resource to restrict its export. Therefore, the development and utilization of low-grade flake graphite ore is particularly important.
[0004] At present, flake graphite mainly adopts flotation as the first step of purification. Impurities in low-grade graphite ore are often embedded with graphite. Researchers often use multiple grinding in stages to promote impurity dissociation. However, multiple grinding reduces the size of large-sized flake graphite, which is not conducive to the development and utilization of back-end products. At the same time, due to the low grade and high impurity content, the fixed carbon content of the concentrate in the roughing process is low. Therefore, multiple selections are often used for flotation purification. However, multiple selections lead to long experimental processes, which not only makes the flotation process inefficient, but also uses a large amount of flotation reagents, which will also lead to a series of problems such as environmental pollution. Therefore, it is particularly important to explore a process to solve the problems of protecting large-sized flakes, reducing inclusions, and the flotation process. The number of selections and long processes are particularly important.
[0005] Ultrasonic technology is a method that emerged in the 20th century. It is a very effective auxiliary strengthening method and has also been developed in ore processing in recent years. Ultrasonic waves can cause thermal effects, mechanical effects, cavitation effects, etc. in aqueous solutions. Before flotation, the use of ultrasonic technology can effectively improve the true display state of ore particles. For example, ultrasound can remove impurities on the surface of the ore, expose the ore to a new surface, and adsorb with the flotation agent, reduce impurity inclusions in the flotation process, and promote the dissociation of impurities from the target mineral.
[0006] CN115025876A A graphite ore dressing process, wherein the graphite ore is crushed by a jaw crusher, crushed by a roller crusher, and then screened, the sieved material is returned to the roller crusher, and the sieved material is dried in an oven to a constant weight, to obtain a coarse ore: S2: the coarse ore is subjected to coarse grinding, rough selection and scavenging; S3: the coarse concentrate obtained by the rough selection in step S2 is subjected to four grindings and eight selections, and S4: the medium ore is concentrated and re-grinded and re-selected, and the process flow is returned in batches. The method adopts a multi-crushing and multi-grinding method to dissociate the impurities therein, which is easy to damage large-sized flake graphite, and the method adopts one rough selection and eight fine selections, the flotation process is long, the efficiency is low, and the reagents are used multiple times, causing environmental load.
[0007] Yang Jianwen published an article in Mining Machinery titled "Experimental Study on the Dressing of Low-Grained Fine-Grained Flake Graphite in Hunan". The article mainly targeted a low-grade flake graphite with a fixed carbon content of 4.56%. Sodium hexametaphosphate and water glass were used as dispersants and inhibitors, kerosene was used as a collector, and No. 2 oil was used as a frother. After a roughing operation, the fixed carbon content was increased to 21.06%. Finally, through a closed-circuit test of one roughing and five fines, a graphite concentrate with a fixed carbon content of 92.53% was obtained. Zhang Tao et al. published an article in Comprehensive Utilization of Minerals titled "Experimental Study on the Dressing of Low-Grade Large-Grained Flake Graphite Ore in Inner Mongolia". The article mainly targeted a large-scale flake graphite ore with a fixed carbon content of 3.55% in Inner Mongolia Autonomous Region. Coal was used to select the graphite concentrate. Oil was used as a collector and 2# oil was used as a frother for a rough selection. The fixed carbon content of the rough concentrated ore was increased to 18.25%. Finally, under the rough selection conditions, a graphite concentrate with a fixed carbon content of 95.44% was obtained by adopting 2 stages of rough grinding and selection, 1 stage of scavenging selection, 6 stages of regrinding and 7 times of concentration; Wang Jinling et al. published an article in "China Mining" entitled "Experimental Research on Mineral Processing of a Low-Grade Large-Flake Graphite Ore". The article mainly conducted a mineral processing test study on a low-grade large-flake graphite ore with a fixed carbon content of 2.05%. The fixed carbon content was increased to 33.67% through a rough selection. Finally, a graphite concentrate with a fixed carbon content of 95% was obtained through a one-stage rod mill coarse grinding, a one-stage ball mill for the rough concentrate, a five-stage stirred mill regrinding, and nine times of concentration in a closed-circuit process.
[0008] The above three articles all use low-grade flake graphite for flotation test research. A rougher concentrate with a maximum fixed carbon content of 33.67% is obtained after a rougher selection. Due to the low fixed carbon content of the rougher concentrate, multiple concentrations and multiple grindings are used for flotation in the back end. Although about 95% of the graphite concentrate is finally obtained, such a long and complicated experimental process will not only lead to an increase in the amount of reagents used, thereby increasing the environmental load, but also reduce production efficiency. At the same time, multiple grindings will also destroy large-sized flake graphite. Summary of the invention
[0009] In view of the above-mentioned existing low-grade natural flake graphite, the graphite ore and impurities are not fully dissociated in the conventional flotation process, resulting in serious inclusions in the flotation process. At the same time, the flotation process of low-grade natural flake graphite has many selection times, a long flotation process, and multi-stage grinding seriously damages large-sized flake graphite. The present invention provides a method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation, which aims to fully dissociate the graphite ore from impurities and reduce inclusions, and to increase the fixed carbon content of the concentrate in the roughing process, thereby reducing the number of selections and shortening the flotation process. The present invention adopts ultrasonic pretreatment, which can reduce the multi-stage grinding process and protect large-sized flake graphite. In order to achieve the above-mentioned purpose of the present invention, the following technical scheme is specially adopted:
[0010] The present invention discloses a method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation, comprising the following steps:
[0011] Step 1
[0012] Crushing and grinding the flake graphite ore until the grinding particle size of -100 mesh accounts for more than 90%, thereby obtaining flake graphite ore;
[0013] Step 2
[0014] The flake graphite ore and water are mixed evenly at a pulp concentration ratio of 8wt.% to 25wt.% to obtain a pulp; then an ultrasonic pretreatment is performed for at least 10 minutes to obtain a pulp after ultrasonic pretreatment; during the ultrasonic pretreatment, the ultrasonic frequency is controlled to be 18-22KHz;
[0015] Step 3
[0016] The pH of the ore pulp after ultrasonic pretreatment is adjusted to 6-9; and a cationic activator is added at a ratio of 80-160 g / t and stirred evenly for a stirring time of greater than or equal to 1 min to obtain a ore pulp after cationic activation; the cationic activator is selected from at least one of NaCl and KCl;
[0017] Step 4
[0018] Add inhibitors, collectors and frothers to the cation activated pulp for roughing to obtain roughing concentrate and roughing tailings; add inhibitors at a dosage of 600-1200 g / t, add collectors at a dosage of 280-400 g / t, and add frothers at a dosage of 160-280 g / t.
[0019] Preferably, the present invention provides a method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation.
[0020] The flake graphite ore with a fixed carbon content of 2.68% to 8.48% is coarsely crushed by a crusher to 8 to 35 mm, accounting for more than 80%, to obtain a coarse crushed product, and then finely crushed by a crushing and screening machine to 0.1 to 3 mm, accounting for more than 80%, to obtain a fine crushed product;
[0021] The obtained finely crushed product is ground with a pulverizer for 2 to 5 minutes, and the grinding particle size of -100 mesh accounts for more than 90%, thereby obtaining flake graphite ore.
[0022] Preferably, the present invention provides a method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation, wherein the obtained flake graphite ore is mixed with water at a ratio of 8% to 25% of the slurry concentration, and stirred for 3 to 5 minutes to obtain the slurry;
[0023] The obtained ore pulp is subjected to ultrasonic pretreatment, and the ultrasonic treatment time is 15 to 40 minutes.
[0024] Preferably, the present invention provides a method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation.
[0025] The ore pulp after ultrasonic pretreatment is transferred to a flotation tank and stirred for 1 to 3 minutes; then a pH adjuster is added to adjust the pH of the ore pulp to 6 to 9, preferably 7.5 to 8.5, and stirred for 2 to 5 minutes.
[0026] Preferably, the present invention provides a method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation.
[0027] Add 80-160 g / t of cationic activator to the slurry after pH adjustment and stir for 1-3 min; then add 600-1200 g / t of inhibitor and stir for 2-5 min; then add 280-400 g / t of collector and stir for 2-5 min; after adding collector and stirring, add 160-280 g / t of frother, after stirring for 1-3 min, turn on the aeration switch, and scrape the foam for 4-9 min, filter and dry the scraped foam to obtain flake graphite concentrate, and the rest is tailings. That is, to the ore pulp after pH adjustment, a cationic activator is added at a ratio of 80 to 160 g per ton of ore pulp, and stirred for 1 to 3 minutes; then, an inhibitor is added at a ratio of 600 to 1200 g per ton of ore pulp, and stirred for 2 to 5 minutes; then, a collector is added at a ratio of 280 to 400 g per ton of ore pulp, and stirred for 2 to 5 minutes; after adding the collector and stirring, a foaming agent is added at a ratio of 160 to 280 g per ton of ore pulp, and after stirring for 1 to 3 minutes, an aeration switch is turned on, and then scraping and foaming is performed for 4 to 9 minutes, and the scraped foam is filtered and dried to obtain flake graphite concentrate, and the rest is tailings.
[0028] As a further preference, a cationic activator is added to the ore pulp after pH adjustment in an amount of 105-145 g / t. As a further preference, a cationic activator is added to the ore pulp after pH adjustment in an amount of 109-125 g / t.
[0029] As a further preference, the inhibitor is added in an amount of 600-1000 g / t, and as a further preference, the inhibitor is added in an amount of 800-1000 g / t. In the present invention, if the amount of the inhibitor is too small, such as 500 g / t, the fixed carbon content of the product will be low and the graphite recovery rate will not be high.
[0030] As a further preference, the collector is added in an amount of 285-360 g / t. As a further preference, the collector is added in an amount of 315-355 g / t. In the present invention, excessive use of the collector will not only fail to increase the recovery rate of graphite, but also reduce the content of fixed carbon.
[0031] As a further preference, a foaming agent is added in an amount of 160-260 g / t. As a further preference, an inhibitor is added in an amount of 175-265 g / t. In the present invention, too little amount of the foaming agent, such as 140 g / t, will also result in a low fixed carbon content in the product and a low graphite recovery rate.
[0032] The crusher used in the present invention comprises a jaw crusher, and the crushing and screening machine is a roller crushing and screening machine.
[0033] The water used in the present invention includes deionized water.
[0034] The power of ultrasound is 60~150W.
[0035] The flotation machines used include XFG5-35 hanging trough flotation machines.
[0036] During the flotation process, the flotation machine impeller is used for stirring, and the rotation speed is 1000-1500r / min.
[0037] The pH adjusters used were HCl and NaOH.
[0038] The inhibitor used is one or more of water glass, CaO and sodium carboxymethyl cellulose.
[0039] The collector used is one of kerosene and diesel.
[0040] The foaming agent used is one of terpineol, methyl isobutyl carbinol and sec-octanol.
[0041] After turning on the air intake switch, the air intake volume is 30~60L / h.
[0042] The fixed carbon content in the graphite concentrate obtained by the primary roughing can reach 75-80%, and the recovery rate of the graphite is greater than or equal to 89%, and the recovery rate of the optimized graphite is greater than or equal to 91%.
[0043] Compared with the prior art, the present invention has the following beneficial effects:
[0044] The present invention adopts ultrasonic equipment to perform ultrasonic pretreatment on natural flake graphite ore, promotes the dissociation of graphite ore and impurities, and increases the fixed carbon content in the flotation concentrate during the roughing process; at the same time, the activation treatment of the graphite ore with a cationic activator enhances the hydrophobicity of the graphite ore, is conducive to separating the graphite ore from impurities, and increases its fixed carbon content, thereby reducing the number of flotation concentrations and reducing the use of various flotation agents. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 .A flow chart of a specific implementation of the present invention. DETAILED DESCRIPTION
[0046] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, the conventional conditions or the conditions recommended by the manufacturer are followed. The reagents or instruments used without indicating the manufacturer are all conventional products that can be obtained commercially.
[0047] A method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation comprises the following steps:
[0048] (1) crushing the natural flake graphite ore with a fixed carbon content of 2.68% to 8.48% by a crusher to 8 to 35 mm, accounting for more than 80%, to obtain a coarse crushed product, and then crushing it by a crushing and screening machine to 0.1 to 3 mm, accounting for more than 80%, to obtain a fine crushed product;
[0049] (2) grinding the finely crushed product with a sample preparation mill for 2 to 5 minutes, wherein the grinding particle size of -100 mesh accounts for more than 90%, thereby obtaining flake graphite ore;
[0050] (3) mixing the flake graphite ore obtained in step (2) with water at a ratio of 8% to 25% of the slurry concentration, and stirring for 3 to 5 minutes to obtain a slurry;
[0051] (4) subjecting the slurry obtained in step (3) to ultrasonic pretreatment, wherein the ultrasonic treatment time is 15 to 40 minutes;
[0052] (5) transferring the slurry after the ultrasonic pretreatment to a flotation tank and stirring for 1 to 3 minutes;
[0053] (6) adding a pH adjuster to the slurry obtained in step (5) to adjust the pH of the slurry to 6 to 9, and stirring for 2 to 5 minutes;
[0054] (7) adding a cationic activator in an amount of 80 to 160 g / t to the pH-adjusted slurry and stirring for 1 to 3 minutes;
[0055] (8) adding an inhibitor in an amount of 600 to 1200 g / t to the slurry to which the cationic activator has been added, and stirring for 2 to 5 minutes;
[0056] (9) Adding a collector at a dosage of 280-400 g / t to the slurry to which the inhibitor has been added, and stirring for 2-5 min;
[0057] (10) Add a foaming agent in an amount of 160-280 g / t to the ore pulp to which the collector has been added. After stirring for 1-3 minutes, turn on the aeration switch and then scrape the foam for 4-9 minutes. The scraped foam is filtered and dried to obtain flake graphite concentrate, and the rest is tailings.
[0058] In a specific embodiment, the crusher in step (1) is a jaw crusher, and the crushing and screening machine is a roller crushing and screening machine.
[0059] In one specific embodiment, the aqueous solution used in step (3) is deionized water.
[0060] In a specific embodiment, the ultrasonic equipment used in step (4) is an intelligent digitally controlled ultrasonic generator, the power of which is set to 60 to 150 W, and the ultrasonic treatment is performed at room temperature.
[0061] In a specific embodiment, the flotation machine used in step (5) is a XFG5-35 hanging tank flotation machine.
[0062] In a specific embodiment, the stirring process in steps (5) to (10) is carried out by using a flotation machine impeller with a rotation speed of 1000 to 1500 r / min.
[0063] In one specific embodiment, the pH adjuster used in step (6) is HCl and NaOH.
[0064] In one specific embodiment, the cationic activator used in step (7) is one of NaCl and KCl.
[0065] In a specific embodiment, the inhibitor used in step (8) is one or more of water glass, CaO, and sodium carboxymethyl cellulose, and the agent is selected according to the types of impurities in different minerals.
[0066] In a specific embodiment, the collector used in step (9) is one of kerosene and diesel.
[0067] In a specific embodiment, the foaming agent used in step (10) is one of terpineol, methyl isobutyl carbinol and octanol.
[0068] In a specific embodiment, the air intake volume in step (10) is 30 to 60 L / h.
[0069] In one specific embodiment, the fixed carbon content of the graphite concentrate obtained in step (10) can reach 78.93%.
[0070] The specific implementation modes of the present invention are further described below in conjunction with embodiments, but the present invention is not limited to the scope of the embodiments.
[0071] Example 1
[0072] The XRD test results of natural flake graphite produced in the mining area of Inner Mongolia Autonomous Region show that the impurities are mainly mica and quartz, and its composition is shown in Table 1.
[0073] Table 1 Composition of natural flake graphite in a mining area in Inner Mongolia Autonomous Region
[0074]
[0075] The natural flake graphite ore is first crushed by an XPC-100X60 jaw crusher to 8-35 mm, accounting for more than 80%, to obtain a coarse crushed product, and then finely crushed by an XPS-Ф250×150 roller crusher and screener to 0.1-3 mm, accounting for more than 80%, to obtain a finely crushed product, and the obtained finely crushed product is ground by a sample preparation mill for 3 minutes, and the grinding particle size of -100 mesh accounts for more than 90%, to obtain flake graphite ore;
[0076] The obtained flake graphite ore was mixed with water at a ratio of 20% of the pulp concentration, and stirred for 3 minutes to obtain a pulp, and then ultrasonically pretreated with an intelligent numerically controlled ultrasonic generator for 30 minutes at a power of 100 W and a frequency of 20 KHz;
[0077] After the ultrasonic pretreatment, the pulp was transferred to the flotation cell of the XFG5-35 hanging cell flotation machine and stirred at 1200r / min for 3min. Then, HCl was added to adjust the pulp pH to 8 and the stirring was continued for 3min. Then, the cationic activator NaCl was added at a dosage of 110g / t and stirred for 1min.
[0078] To the ore pulp with the cationic activator added thereto, 800 g / t of water glass as an inhibitor was added, and after stirring for 3 minutes, 320 g / t of kerosene as a collector was added, and stirring was continued for 3 minutes, and then 180 g / t of pine alcohol as a foaming agent was added. After stirring for 3 minutes, the aeration switch was turned on, the air intake was set to 40 L / h, and then the foam was scraped for 7 minutes. The scraped foam was filtered and dried at 105°C to obtain flake graphite concentrate.
[0079] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 76.53% and recovery rate of 92.14%.
[0080] The graphite concentrate obtained by rough selection was refined in the presence of 400 g / t of water glass as an inhibitor, 160 g / t of kerosene as a collector and 90 g / t of pine alcohol as a foaming agent. After three rounds of refinement, the fixed carbon content in the graphite concentrate increased to 94.85%.
[0081] Example 2
[0082] The XRD test results of natural flake graphite produced in a mining area in Henan Province show that the impurities are mainly mica, quartz, feldspar and pyrite. Its composition is shown in Table 2.
[0083] Table 2 Composition of natural flake graphite in a mining area in Henan Province
[0084]
[0085] The natural flake graphite ore is first crushed by an XPC-100X60 jaw crusher to 8-35 mm, accounting for more than 80%, to obtain a coarse crushed product, and then finely crushed by an XPS-Ф250×150 roller crusher and screener to 0.1-3 mm, accounting for more than 80%, to obtain a finely crushed product, and the obtained finely crushed product is ground by a sample preparation mill for 5 minutes, and the grinding particle size of -100 mesh accounts for more than 90%, to obtain flake graphite ore;
[0086] The obtained flake graphite ore was mixed with water at a ratio of 18% slurry concentration, and stirred for 3 minutes to obtain slurry, and then ultrasonically pretreated with an intelligent numerically controlled ultrasonic generator for 30 minutes at a power of 150W and a frequency of 21KHz;
[0087] After the ultrasonic pretreatment, the pulp was transferred to the flotation cell of the XFG5-35 hanging cell flotation machine and stirred at 1400r / min for 3min. Then, HCl was added to adjust the pulp pH to 8 and the stirring was continued for 3min. Then, the cationic activator KCl was added at a dosage of 120g / t and stirred for 1min.
[0088] To the ore pulp to which the cationic activator is added, 600 g / t water glass as an inhibitor and 400 g / t calcium oxide are added. After stirring for 3 minutes, 350 g / t of diesel as a collector is added, and stirring is continued for 3 minutes. Then 260 g / t of methyl isobutyl carbinol as a foaming agent is added. After stirring for 3 minutes, the aeration switch is turned on, the air intake is set to 50 L / h, and then scraping and foaming is performed for 6 minutes. The scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.
[0089] During the flotation process, the roughing flotation of natural flake graphite ore was carried out at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 78.93% and recovery rate of 91.27%.
[0090] The graphite concentrate obtained by rough selection is refined in the presence of 300g / t water glass and 200g / t calcium oxide as inhibitors, 180g / t diesel as collector and 130g / t methyl isobutyl carbinol as foaming agent. After three refinements, the fixed carbon content in the graphite concentrate is increased to 95.37%.
[0091] Example 3
[0092] The XRD test results of natural flake graphite produced in a mining area in Yunnan Province show that the impurities are mainly mica, quartz, feldspar and pyrite. Its composition is shown in Table 3.
[0093] Table 3 Composition of natural flake graphite in a mining area in Yunnan Province
[0094]
[0095]
[0096] The natural flake graphite ore is first crushed by an XPC-100X60 jaw crusher to 8-35 mm, accounting for more than 80%, to obtain a coarse crushed product, and then finely crushed by an XPS-Ф250×150 roller crusher and screener to 0.1-3 mm, accounting for more than 80%, to obtain a finely crushed product, and the obtained finely crushed product is ground by a sample preparation mill for 3 minutes, and the grinding particle size of -100 mesh accounts for more than 90%, to obtain flake graphite ore;
[0097] The obtained flake graphite ore was mixed with water at a ratio of 25% of the pulp concentration, and stirred for 3 minutes to obtain the pulp, and then ultrasonically pretreated with an intelligent numerically controlled ultrasonic generator at a power of 80W and a frequency of 20KHz for 30 minutes;
[0098] After the ultrasonic pretreatment, the pulp was transferred to the flotation cell of the XFG5-35 hanging cell flotation machine and stirred at 1500r / min for 3min. Then NaOH was added to adjust the pulp pH to 9 and the stirring was continued for 3min. Then, the cationic activator NaCl was added at a dosage of 140g / t and stirred for 1min.
[0099] To the ore pulp with the cationic activator added, add 650 g / t water glass as an inhibitor and 500 g / t sodium carboxymethyl cellulose, stir for 3 minutes, add 300 g / t of diesel as a collector, and continue stirring for 3 minutes, then add 200 g / t of octanol as a foaming agent, after stirring for 3 minutes, turn on the aeration switch, set the air intake to 45 L / h, and then scrape and foam for 7 minutes, filter the scraped foam and dry it at 105°C to obtain flake graphite concentrate.
[0100] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 74.93% and recovery rate of 91.21%.
[0101] The graphite concentrate obtained by rough selection was refined in the presence of 320g / t water glass as a depressant, 250g / t sodium carboxymethyl cellulose, 150g / t diesel as a collector, and 100g / t octanol as a foaming agent. After four refinements, the fixed carbon content in the graphite concentrate increased to 95.13%.
[0102] Example 4
[0103] The XRD test results of natural flake graphite produced in a mining area in Henan Province show that the impurities are mainly mica, quartz and feldspar, and its composition is shown in Table 4.
[0104] Table 4 Composition of natural flake graphite in a mining area in Henan Province
[0105]
[0106] The natural flake graphite ore is first crushed by an XPC-100X60 jaw crusher to 8-35 mm, accounting for more than 80%, to obtain a coarse crushed product, and then finely crushed by an XPS-Ф250×150 roller crusher and screener to 0.1-3 mm, accounting for more than 80%, to obtain a finely crushed product, and the obtained finely crushed product is ground by a sample preparation mill for 3 minutes, and the grinding particle size of -100 mesh accounts for more than 90%, to obtain flake graphite ore;
[0107] The obtained flake graphite ore was mixed with water at a ratio of 23% of the pulp concentration, and stirred for 3 minutes to obtain the pulp, and then ultrasonically pretreated with an intelligent numerically controlled ultrasonic generator for 30 minutes at a power of 60W and a frequency of 22KHz;
[0108] After the ultrasonic pretreatment, the pulp was transferred to the flotation cell of the XFG5-35 hanging cell flotation machine and stirred at 1400r / min for 3min. Then, HCl was added to adjust the pH of the pulp to 7 and the stirring was continued for 3min. Then, the cationic activator KCl was added at a dosage of 130g / t and stirred for 1min.
[0109] To the ore pulp to which the cationic activator was added, 400 g / t water glass as an inhibitor and 480 g / t sodium carboxymethyl cellulose were added, and after stirring for 3 minutes, 290 g / t of kerosene as a collector was added, and stirring was continued for 3 minutes. Then, 160 g / t of pine oil as a foaming agent was added. After stirring for 3 minutes, the aeration switch was turned on, the air intake was set to 60 L / h, and then scraping was performed for 8 minutes. The scraped foam was filtered and dried at 105°C to obtain flake graphite concentrate.
[0110] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 75.14% and recovery rate of 89.37%.
[0111] The graphite concentrate obtained by rough selection is refined in the presence of 200g / t water glass and 240g / t sodium carboxymethyl cellulose as inhibitors, 150g / t kerosene as collector and 800g / t pinene alcohol as foaming agent. After three refinements, the fixed carbon content in the graphite concentrate is increased to 94.62%.
[0112] Comparative Example 1
[0113] The other conditions are the same as those in the roughing process of Example 2, except that no ultrasonic treatment is performed; that is:
[0114] The obtained flake graphite ore was mixed with water at a pulp concentration of 18%, and stirred for 3 minutes to obtain pulp; the pulp was transferred to the flotation tank of the XFG5-35 hanging tank flotation machine, stirred at a speed of 1400r / min for 3 minutes, and then HCl was added to adjust the pulp pH to 8, and the stirring was continued for 3 minutes; then the cationic activator KCl was added at an amount of 120g / t, and stirred for 1 minute;
[0115] To the ore pulp to which the cationic activator is added, 600 g / t water glass as an inhibitor and 400 g / t calcium oxide are added. After stirring for 3 minutes, 350 g / t of diesel as a collector is added, and stirring is continued for 3 minutes. Then 260 g / t of methyl isobutyl carbinol as a foaming agent is added. After stirring for 3 minutes, the aeration switch is turned on, the air intake is set to 40 L / h, and then scraping and foaming is performed for 6 minutes. The scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.
[0116] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 72.33% and recovery rate of 81.52%.
[0117] Comparative Example 2
[0118] The other conditions are the same as those in the roughing process of Example 2, except that no cationic activator is added; that is:
[0119] The obtained flake graphite ore was mixed with water at a ratio of 18% slurry concentration, and stirred for 3 minutes to obtain slurry, and then ultrasonically pretreated with an intelligent numerically controlled ultrasonic generator for 30 minutes at a power of 150W and a frequency of 21KHz;
[0120] After the ultrasonic pretreatment, the pulp was transferred to the flotation cell of the XFG5-35 hanging cell flotation machine and stirred at 1400 r / min for 3 min. Then HCl was added to adjust the pulp pH to 8 and stirring was continued for 3 min.
[0121] Add 600 g / t water glass and 400 g / t calcium oxide as inhibitors to the above slurry, stir for 3 minutes, add 350 g / t of collector diesel, continue stirring for 3 minutes, then add 260 g / t of foaming agent methyl isobutyl carbinol, after stirring for 3 minutes, turn on the inflation switch, set the air intake to 40 L / h, then scrape and foam for 6 minutes, filter the scraped foam and dry it at 105°C to obtain flake graphite concentrate.
[0122] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 58.70% and recovery rate of 87.26%.
[0123] Comparative Example 3
[0124] The other conditions are the same as those in the roughing process of Example 2, except that no ultrasonic pretreatment is performed and no cationic activator is added; that is:
[0125] The obtained flake graphite ore was mixed with water at a pulp concentration of 18%, and stirred for 3 minutes to obtain pulp; the pulp was transferred to the flotation cell of the XFG5-35 hanging tank flotation machine, stirred at a speed of 1400r / min for 3 minutes, and then HCl was added to adjust the pulp pH to 8, and the stirring was continued for 3 minutes;
[0126] Add 600 g / t water glass and 400 g / t calcium oxide as inhibitors to the above slurry, stir for 3 minutes, add 350 g / t of collector diesel, continue stirring for 3 minutes, then add 260 g / t of foaming agent methyl isobutyl carbinol, after stirring for 3 minutes, turn on the inflation switch, set the air intake to 40 L / h, then scrape and foam for 6 minutes, filter the scraped foam and dry it at 105°C to obtain flake graphite concentrate.
[0127] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 47.39% and recovery rate of 68.71%.
[0128] Comparative Example 4
[0129] The other conditions are the same as those in the roughing process of Example 2, except that the dosage range of the inhibitor is not within the protection range of the present invention of 600 to 1200 g / t, that is:
[0130] The obtained flake graphite ore was mixed with water at a ratio of 18% slurry concentration, and stirred for 3 minutes to obtain slurry, and then ultrasonically pretreated with an intelligent numerically controlled ultrasonic generator for 30 minutes at a power of 150W and a frequency of 21KHz;
[0131] After the ultrasonic pretreatment, the pulp was transferred to the flotation cell of the XFG5-35 hanging cell flotation machine and stirred at 1400r / min for 3min. Then, HCl was added to adjust the pulp pH to 8 and the stirring was continued for 3min. Then, the cationic activator KCl was added at a dosage of 120g / t and stirred for 1min.
[0132] To the ore pulp with the cationic activator added, 300 g / t water glass as an inhibitor and 200 g / t calcium oxide were added. After stirring for 3 minutes, 350 g / t of diesel as a collector was added, and stirring was continued for 3 minutes. Then, 260 g / t of methyl isobutyl carbinol as a foaming agent was added. After stirring for 3 minutes, the aeration switch was turned on, the air intake was set to 40 L / h, and then scraping was performed for 6 minutes. The scraped foam was filtered and dried at 105°C to obtain flake graphite concentrate.
[0133] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 38.27% and recovery rate of 53.21%.
[0134] Comparative Example 5
[0135] The other conditions are the same as those in the roughing process of Example 2, except that the amount of the collector is not within the protection range of the present invention of 280 to 400 g / t, that is:
[0136] The obtained flake graphite ore was mixed with water at a ratio of 18% slurry concentration, and stirred for 3 minutes to obtain slurry, and then ultrasonically pretreated with an intelligent numerically controlled ultrasonic generator for 30 minutes at a power of 150W and a frequency of 21KHz;
[0137] After the ultrasonic pretreatment, the pulp was transferred to the flotation cell of the XFG5-35 hanging cell flotation machine and stirred at 1400r / min for 3min. Then, HCl was added to adjust the pulp pH to 8 and the stirring was continued for 3min. Then, the cationic activator KCl was added at a dosage of 120g / t and stirred for 1min.
[0138] To the ore pulp to which the cationic activator was added, 600 g / t water glass as an inhibitor and 400 g / t calcium oxide were added. After stirring for 3 minutes, 500 g / t of diesel as a collector was added, and stirring was continued for 3 minutes. Then, 260 g / t of methyl isobutyl carbinol as a foaming agent was added. After stirring for 3 minutes, the aeration switch was turned on, the air intake was set to 40 L / h, and then scraping was performed for 6 minutes. The scraped foam was filtered and dried at 105°C to obtain flake graphite concentrate.
[0139] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 49.37% and recovery rate of 56.87%.
[0140] Comparative Example 6
[0141] The other conditions are the same as those in the roughing process of Example 2, except that the amount of the foaming agent is not within the protection range of the present invention of 160 to 280 g / t, that is:
[0142] The obtained flake graphite ore was mixed with water at a ratio of 18% slurry concentration, and stirred for 3 minutes to obtain slurry, and then ultrasonically pretreated with an intelligent numerically controlled ultrasonic generator for 30 minutes at a power of 150W and a frequency of 21KHz;
[0143] After the ultrasonic pretreatment, the pulp was transferred to the flotation cell of the XFG5-35 hanging cell flotation machine and stirred at 1400r / min for 3min. Then, HCl was added to adjust the pulp pH to 8 and the stirring was continued for 3min. Then, the cationic activator KCl was added at a dosage of 120g / t and stirred for 1min.
[0144] To the ore pulp to which the cationic activator is added, 600 g / t water glass as an inhibitor and 400 g / t calcium oxide are added. After stirring for 3 minutes, 350 g / t of diesel as a collector is added, and stirring is continued for 3 minutes. Then, 140 g / t of methyl isobutyl carbinol as a foaming agent is added. After stirring for 3 minutes, the aeration switch is turned on, the air intake is set to 40 L / h, and then scraping and foaming is performed for 6 minutes. The scraped foam is filtered and dried at 105°C to obtain flake graphite concentrate.
[0145] In the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 61.59% and recovery rate of 42.98%.
Claims
1. A method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation, characterized in that: The following steps are involved: Step 1 Crushing and grinding the flake graphite ore until the grinding particle size of -100 mesh accounts for more than 90%, thereby obtaining flake graphite ore; Step 2 The flake graphite ore and water are mixed evenly at a pulp concentration ratio of 8wt.% to 25wt.% to obtain a pulp; then an ultrasonic pretreatment is performed for at least 10 minutes to obtain a pulp after ultrasonic pretreatment; during the ultrasonic pretreatment, the ultrasonic frequency is controlled to be 18-22KHz; Step 3 The pH of the ore pulp after ultrasonic pretreatment is adjusted to 6-9; and a cationic activator is added at a ratio of 80-160 g / t and stirred evenly for a stirring time of greater than or equal to 1 min to obtain a ore pulp after cationic activation; the cationic activator is selected from at least one of NaCl and KCl; Step 4 Add inhibitors, collectors and frothers to the cation activated pulp for roughing to obtain roughing concentrate and roughing tailings; add inhibitors at a dosage of 600-1200 g / t, add collectors at a dosage of 280-400 g / t, and add frothers at a dosage of 160-280 g / t.
2. The method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation according to claim 1, characterized in that: The flake graphite ore with a fixed carbon content of 2.68% to 8.48% is coarsely crushed by a crusher to 8 to 35 mm, accounting for more than 80%, to obtain a coarse crushed product, and then finely crushed by a crushing and screening machine to 0.1 to 3 mm, accounting for more than 80%, to obtain a fine crushed product; The obtained finely crushed product is ground with a pulverizer for 2 to 5 minutes, and the grinding particle size of -100 mesh accounts for more than 90%, thereby obtaining flake graphite ore.
3. The method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation according to claim 1, characterized in that: The obtained flake graphite ore is mixed with water at a ratio of 8wt.% to 25wt.% of the slurry concentration, and stirred for 3 to 5 minutes to obtain the slurry; The obtained ore pulp is subjected to ultrasonic pretreatment, and the ultrasonic treatment time is 15 to 40 minutes.
4. The method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation according to claim 3, characterized in that: The ore pulp after ultrasonic pretreatment is transferred to a flotation tank and stirred for 1 to 3 minutes; then a pH adjuster is added to adjust the pH of the ore pulp to 6 to 9, preferably 7.5 to 8.5, and stirred for 2 to 5 minutes.
5. The method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation according to claim 4, characterized in that: Add 80-160 g / t of cationic activator to the slurry after pH adjustment and stir for 1-3 min; then add 600-1200 g / t of inhibitor and stir for 2-5 min; then add 280-400 g / t of collector and stir for 2-5 min; after adding collector and stirring, add 160-280 g / t of frother, after stirring for 1-3 min, turn on the aeration switch, and scrape the foam for 4-9 min, filter and dry the scraped foam to obtain flake graphite concentrate, and the rest is tailings.
6. The method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation according to claim 5, characterized in that: A cationic activator is added to the ore pulp after pH adjustment in an amount of 105-145 g / t. As a further preferred method, a cationic activator is added to the ore pulp after pH adjustment in an amount of 109-125 g / t.
7. The method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation according to claim 5, characterized in that: The inhibitor is added in an amount of 600-1000 g / t, and as a further preferred amount, the inhibitor is added in an amount of 800-1000 g / t; the collector is added in an amount of 285-360 g / t, and as a further preferred amount, the inhibitor is added in an amount of 315-355 g / t; The foaming agent is added in an amount of 160-260 g / t. For further preference, the inhibitor is added in an amount of 175-265 g / t.
8. The method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation according to claim 5, characterized in that: The power of ultrasound is 60 to 150W; During the flotation process, the stirring speed is 1000-1500r / min; The pH adjuster used is selected from at least one of HCl and NaOH; The inhibitor used is one or more of water glass, CaO, and sodium carboxymethyl cellulose; The collector used is one of kerosene and diesel; The foaming agent used is one of terpineol, methyl isobutyl carbinol and sec-octanol.
9. The method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation according to claim 5, characterized in that: After turning on the air intake switch, the air intake volume is 30~60L / h.
10. The method for purifying low-grade flake graphite ore by ultrasonic pretreatment combined with cationic activation according to claim 5, characterized in that: The fixed carbon content in the graphite concentrate obtained by the primary roughing can reach 75-80%, and the recovery rate of graphite is greater than or equal to 89%.
Citation Information
Patent Citations
Short process purification method of graphite
CN109647630A
Short-process beneficiation method of low-grade fine flake graphite
CN112206926A
AU2020104144A4