A method for preparing boron-doped diamond
By using graphene, nano-boron nitride, and o-carborane as raw materials, and combining sol-coagulation technology with electric field-assisted sintering, high boron-doped diamond was prepared, solving the problems of small active area and insufficient conductivity in existing BDD technologies, and achieving high-efficiency electrochemical performance and industrialization potential.
Patent Information
- Application Number
- CN202411122380.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-08-15
AI Technical Summary
In existing technologies, BDD produced by CVD method has a small active area, slow mass transfer rate, low efficiency and high energy consumption, which limits its industrialization and promotion. BDD prepared by HPHT method has low boron doping concentration and insufficient conductivity, which affects electrochemical performance.
Using graphene, nano-boron nitride, and o-carborane as raw materials, metal catalysts were prepared in situ through sol-coagulation technology. Combined with electric field-assisted sintering, boron-doped diamond with high boron doping was prepared. Highly active graphite columns were then synthesized under high temperature and high pressure using a six-sided press.
The prepared boron-doped diamond has high thermal shock strength, wear resistance, chemical inertness and electrical conductivity, making it suitable for wastewater treatment in the electrochemical field and improving the electrochemical performance of electrodes.
Smart Images

Figure CN118771371B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of superhard materials technology, and particularly relates to a method for preparing boron-doped diamond. Background Technology
[0002] Because boron-containing diamond (BDD) outperforms ordinary diamond in terms of heat resistance, wear resistance, chemical inertness, oxidation resistance, and compressive strength, it has shown great application potential in various industries in recent years, driven by the rapid development of modern industry. It has gradually become an ideal material for developing equipment such as electron emission electrodes, photodetectors, field-effect transistors, and vacuum tunneling microscope probes. The discovery of its superconducting properties has further expanded the application prospects of boron-containing diamond. Its excellent wear resistance and abrasion resistance also make BDD highly valuable in the processing of hard and tough materials.
[0003] BDD, as a high-performance electrode material, can oxidize water molecules under an electric field to generate a large number of hydroxyl radicals (·OH) with high oxidation sites. Therefore, researchers have applied BDD electrodes as anodes in advanced electrochemical oxidation technologies to the field of environmental pollution control. Similar to other advanced oxidation technologies, such as catalytic ozone oxidation, Fenton oxidation, and photocatalytic oxidation, the hydroxyl radicals generated during the reaction thoroughly mineralize and oxidize various organic pollutants or microorganisms in water to generate carbon dioxide, water, and inorganic ions, achieving the goal of degrading various high-concentration, toxic, and recalcitrant wastewater. In recent years, research on the electrochemical treatment of organic pollutants based on BDD anodes has been extensive, involving phenols, fuels, surfactants, pesticides, organic acids, pharmaceuticals, and biochemical pretreatment of wastewater. There are also reports in the literature on the use of BDD for treating cyanide anodes in wastewater containing heavy metal ions. Currently, high-temperature high-pressure (HPHT) and low-pressure chemical vapor deposition (CVD) are commonly used methods for preparing BDD electrodes. CVD preparation of BDD has advantages such as easy control of boron doping concentration and good diamond purity. The boron doping concentration can reach 1020 mg / L, and the hole mobility can reach 1500 cm⁻¹ at room temperature. 2 v -1 s -1 The resistivity is 10 -2 The high boron doping concentration (Ω·cm) makes it possible to apply electrodes to wastewater treatment in the electrochemical field. However, the CVD method for producing BDD has limitations such as small active area and slow mass transfer rate, resulting in low efficiency and high energy consumption in the electrochemical oxidation and degradation of organic wastewater, thus restricting its industrialization. Therefore, it has remained in the research stage and has not yet been industrialized. Compared with the CVD method, the HPHT method for synthesizing BDD has advantages such as short synthesis cycle and low cost. However, the BDD prepared by the HPHT method currently exhibits low conductivity due to the low boron doping concentration, which affects its electrochemical performance. Summary of the Invention
[0004] The purpose of this invention is to provide a method for preparing boron-doped diamond. The method uses graphene, nano-boron nitride, and o-carborane as raw materials, and employs sol-coagulation technology to prepare metal catalysts in situ. Highly active graphite columns are prepared by electric field-assisted sintering, and boron-doped diamond with high boron doping content is synthesized from the above graphite columns using a six-sided press.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0006] A method for preparing boron-doped diamond includes the following steps:
[0007] S1. Dissolve o-carborane in cyclohexane and mix evenly, then add graphene and nano boron nitride in sequence and treat in an ultrasonic device for 2 hours until the mixture is evenly mixed;
[0008] S2. Place the solution after ultrasonic treatment in step S1 in an oven and keep it at 40-60℃ for 8-12 hours to remove cyclohexane. Dissolve o-carborane in cyclohexane, and then the cyclohexane will evaporate, and o-carborane will become a coating on the graphene surface.
[0009] S3. Dissolve N,N'-methylenebisacrylamide, acrylamide, cobalt nitrate hexahydrate, ferric nitrate nonahydrate, nickel nitrate hexahydrate, and citric acid in 80-100 ml of distilled water and stir until homogeneous. To ensure uniform dispersion of graphene and nano-boron nitride, add the graphene treated in step S2 to the solution and treat it in an ultrasonic mechanical stirrer for 2 hours until homogeneous. Then, add ammonium persulfate solution and tetramethylethylenediamine solution and stir to form a gel. Ammonium persulfate acts as an initiator, enabling N,N'-methylenebisacrylamide and acrylamide to undergo a cross-linking reaction. Tetramethylethylenediamine acts as a catalyst, accelerating the above reaction. This reaction solidifies the entire solution into a gel, forming a co-precipitate, which can be called polymer network gel technology. Citric acid acts as a complexing agent, forming a metal ion complex, which can also be understood as a co-precipitation of iron, cobalt, and nickel. The iron, cobalt, and nickel alloy is grown in situ on the graphite surface through hydrogen reduction.
[0010] S4. Place the gel in a 120℃ oven for 10-15 hours, crush the dry gel into powder with a fineness of less than 325# using a ball mill, reduce it in a hydrogen atmosphere furnace at 600-800℃ for 3-5 hours, press it into graphite columns, and then treat it under an electric field of 800-3000V for 3-5 hours.
[0011] S5. The graphite column after step S4 is treated with a six-sided press at a pressure of 3.5-4.5 GPa and a temperature of 1300-1500℃ for 5-20 min to synthesize boron-doped diamond.
[0012] Furthermore, in step S1, both graphene and boron nitride nanoparticles have single-layer or multi-layer structures, and the mass ratio of ortho-carborane, graphene, and boron nitride nanoparticles is 1-6:20-60:1-10.
[0013] Furthermore, in steps S2 and S3, the ultrasonic treatment is performed with an ultrasonic power of 1000-3000W and a mechanical stirring speed of 10-40rpm.
[0014] Furthermore, in step S3, the mass ratio of N,N'-methylenebisacrylamide, acrylamide, cobalt nitrate hexahydrate, ferric nitrate nonahydrate, nickel nitrate hexahydrate, and citric acid is 0.2–0.4:3–7:10–20:20–30:13–20:2–6, and the mass ratio of ammonium persulfate solution to tetramethylethylenediamine solution is 0.2–0.5:0.1–0.3.
[0015] The mechanism of this invention is as follows: graphene containing o-carborane and single / multilayer boron nitride on its surface is converted into boron-containing diamond with high boron content under high temperature and pressure in the presence of a catalyst (iron, cobalt, nickel). The boron source has two origins: 1. o-carborane, and 2. nano-sized boron nitride. The catalyst is an iron-cobalt-nickel catalyst prepared on the surface of graphene and other raw materials using polymer network gelation and hydrogen reduction technology.
[0016] The advantages of this invention are: compared with the prior art, the diamond synthesized by using graphene, nano boron nitride, ortho-carborane and other raw materials to prepare metal catalysts in situ using sol-coagulation technology and preparing highly active graphite columns by electric field-assisted sintering has high thermal shock strength, high wear resistance, high chemical inertness and electrical conductivity. Attached Figure Description
[0017] Figure 1 This is the XRD pattern of boron-doped diamond prepared by the method in Example 1 of this invention.
[0018] Figure 2 This is a SEM image of boron-doped diamond prepared by the method in Example 1 of this invention. Detailed Implementation
[0019] Example 1
[0020] like Figure 1-2 As shown, a method for preparing boron-doped diamond includes the following steps:
[0021] 1. Weigh 10g of o-carborane and dissolve it in 500g of cyclohexane;
[0022] 2. Weigh 200g of single-layer or multi-layer graphene and 30g of single-layer or multi-layer nano boron nitride and add them to the above solution. Treat the mixture in an ultrasonic mechanical stirrer for 2 hours, where the ultrasonic power is 2000W and the mechanical stirring speed is 40rpm to mix them evenly.
[0023] 3. Place the above solution in an oven and keep it at 60°C for 12 hours to allow the cyclohexane to evaporate and be removed.
[0024] 4. Weigh 0.4g of N,N'-methylenebisacrylamide, 5g of acrylamide, 15g of cobalt nitrate hexahydrate, 23g of ferric nitrate nonahydrate, 18g of nickel nitrate hexahydrate, and 4g of citric acid, dissolve them in 100ml of distilled water, and stir well. Add the above-treated graphene to the solution and treat it in an ultrasonic mechanical stirrer for 2 hours, where the ultrasonic power is 2000W and the mechanical stirring speed is 40rpm to mix it evenly.
[0025] 5. Take 0.3g of 10% ammonium persulfate solution and 0.2g of 2% tetramethylethylenediamine solution and add them to the above solution. Stir for 3 hours to form a gel.
[0026] 6. Place the above gel in an oven at 120°C for 12 hours, and then use a ball mill to break the dry gel into fine powder of 325#.
[0027] 7. Reduce the above powder in a furnace under a hydrogen atmosphere at 700°C for 4 hours.
[0028] 8. Press the above powder into a Φ30mm graphite column and treat it under an electric field of 2000V for 4 hours.
[0029] 9. Using a six-sided press, the above-treated graphite columns were treated at a pressure of 3.5 GPa and a temperature of 1400℃ for 20 min to synthesize diamond.
[0030] Example 2
[0031] The difference between Example 2 and Example 1 is that the graphene is a single-layer structure.
[0032] Example 3
[0033] The difference between Example 3 and Example 1 is that o-carborane was not used.
[0034] Example 4
[0035] The difference between Example 4 and Example 1 is that the step of treating the graphite column under an electric field of 2000V for 4 hours was not included.
[0036] Performance testing
[0037] The hardness, impact toughness, boron content, and average electrical conductivity of the boron-doped diamonds prepared in Examples 1-4 were tested according to national standards. The specific test results are shown in Table 1, and the test process is as follows:
[0038] Diamond TTI test method: Take 100g of agglomerated diamond particles and steel balls and put them into the test tube. Heat to 900℃ and oscillate and impact at a frequency of 2000r / min. Calculate the breakage rate after impact. The impact toughness of the sample is characterized by the number of impacts when the non-breakage rate is 50%.
[0039] Boron element measurement method: Inductively coupled plasma atomic emission spectrometry (ICP-AES) was used to test the boron element.
[0040] Electrical conductivity measurement equipment: The prepared diamond was measured using a HADFM100H powder resistivity tester.
[0041] Table 1
[0042] Sample source Diamond hardness (GPa) Impact toughness Boron content (mg / L) Average conductivity mS / cm Example 1 21.8 810 10.57 10.3317 Example 2 17.1 625 6.31 3.2668 Example 3 12.3 560 5.52 4.7433 Example 4 4.9 379 3.18 1.0941
Claims
1. A method for preparing boron-doped diamond, characterized in that, Includes the following steps: S1. Dissolve o-carborane in cyclohexane and mix evenly, then add graphene and nano-boron nitride in sequence and treat in an ultrasonic device for 2 hours until evenly mixed; both graphene and nano-boron nitride are single-layer or multi-layer structures, and the mass ratio of o-carborane, graphene and nano-boron nitride is 1~6:20~60:1~10. S2. Place the solution after ultrasonic treatment in step S1 in an oven and keep it at 40~60℃ for 8~12 h to remove cyclohexane; S3. Dissolve N,N'-methylenebisacrylamide, acrylamide, cobalt nitrate hexahydrate, ferric nitrate nonahydrate, nickel nitrate hexahydrate, and citric acid in 80-100 ml of distilled water and stir until homogeneous. Add the graphene treated in step S2 to the solution and treat it in an ultrasonic mechanical stirrer for 2 hours until it is homogeneous. Then add ammonium persulfate solution and tetramethylethylenediamine solution and stir to form a gel. S4. Place the gel in a 120℃ oven for 10~15 h, crush the dry gel into powder with a fineness of less than 325# using a ball mill, reduce it in a furnace under a hydrogen atmosphere at 600~800℃ for 3~5 h, press it into graphite columns, and then treat it under an electric field of 800~3000 V for 3~5 h. S5. The graphite column after step S4 is treated with a six-sided press at a pressure of 3.5~4.5 GPa and a temperature of 1300~1500℃ for 5~20 min to synthesize boron-doped diamond.
2. The method for preparing boron-doped diamond as described in claim 1, characterized in that: In steps S2 and S3, the ultrasonic treatment is performed with an ultrasonic power of 1000~3000W and a mechanical stirring speed of 10~40 rpm.
3. The method for preparing boron-doped diamond as described in claim 2, characterized in that: In step S3, the mass ratio of N,N'-methylenebisacrylamide, acrylamide, cobalt nitrate hexahydrate, ferric nitrate nonahydrate, nickel nitrate hexahydrate, and citric acid is 0.2~0.4:3~7:10~20:20~30:13~20:2~6, and the mass ratio of ammonium persulfate solution to tetramethylethylenediamine solution is 0.2~0.5:0.1~0.3.
Citation Information
Patent Citations
Method for manufacturing boron nitride toughened polycrystalline diamond
CN103883257A
Synthesis method and synthesis device of monocrystalline diamond
CN114029002A
Preparation method of uniform boron-doped diamond single crystal
CN117026372A