Production process and equipment for dry-type composite furnace lining material of intermediate frequency furnace

Through the intermediate frequency furnace dry composite furnace lining production process, specific material proportions and process flows are used to solve the problems of insufficient strength of the intermediate frequency furnace lining and insufficient mixing of raw materials, achieving efficient construction and trimming, and improving production efficiency and material performance. .

CN118771864AInactive Publication Date: 2024-10-15JINAN HENGJIN REFRACTORY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411009823.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The lining of the existing medium frequency induction furnace has insufficient strength, resulting in abrasion or damage. The construction and repair steps are complicated, which affects production efficiency. In addition, the raw materials of the composite furnace lining are not fully mixed, which affects the use effect.

Method used

The intermediate frequency furnace dry composite furnace lining production process is adopted, including the proportional mixing of dense fused corundum, quartz sand, quartz powder, ceramic fiber, silicon carbide ultrafine powder, sodium tripolyphosphate and boric acid, through stirring and dry pounding processes. Combining natural drying and heated baking to improve the strength and mixing uniformity of the lining material.

Benefits of technology

It improves the strength and trimming efficiency of the intermediate frequency furnace lining material, shortens the construction time, improves production efficiency, and ensures full mixing of raw materials, suitable for overall and partial trimming.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771864A_ABST
    Figure CN118771864A_ABST
Patent Text Reader

Abstract

The invention discloses a production process and equipment for a dry-type composite furnace lining of an intermediate frequency furnace, and relates to the technical field of composite furnace lining production, and the dry-type composite furnace lining comprises the following materials in parts by mass: 45 parts of dense fused corundum; 15 parts of quartz sand; 15 parts of quartz powder; 5 parts of ceramic fiber; 3 parts of silicon carbide superfine powder; 1 part of sodium tripolyphosphate; and 1 part of boric acid. By improving the production process of the dry-type composite furnace lining material of the intermediate frequency furnace and adjusting the component proportion and process parameters, the prepared lining material is not only suitable for overall construction operation, but also suitable for local finishing of a target area. The constructed lining material is high in strength, the construction time can be shortened by 30%-50% compared with the prior art, the finishing efficiency is effectively improved, and the situation that normal production operation of the intermediate frequency furnace and the dry type composite furnace is affected due to overlong-time shutdown overhaul is avoided; by arranging the stirring mechanism, raw materials can be stirred, the stirring effect on the raw materials is improved, and the raw materials can be fully mixed conveniently.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite furnace lining production, in particular to a production process and equipment for dry composite furnace lining of a medium frequency furnace. Background Art

[0002] The working frequency of the medium frequency induction furnace (hereinafter referred to as the medium frequency furnace) is between 50-2000 Hz. It is widely used in the smelting of non-ferrous metals and ferrous metals. Compared with other casting equipment, the medium frequency induction furnace has the advantages of high thermal efficiency, short smelting time, less alloy element burnout, wide smelting material, low environmental pollution, and accurate control of the temperature and composition of the molten metal. However, when the existing medium frequency induction furnace is in use, the lining strength does not meet the use requirements, and it is easy to cause abrasion or damage in the target area, resulting in the equipment being unable to operate normally. The construction and repair steps for the lining of the medium frequency induction furnace are relatively complicated, especially the repair operation, which requires a long shutdown to wait for the hydration reaction of the lining to be completed so that it can obtain the preset use strength, which is time-consuming and labor-intensive and affects production efficiency.

[0003] In addition, when producing composite furnace linings, multiple raw materials need to be mixed. If the raw materials are not fully mixed, it is easy to affect the subsequent use of the lining.

[0004] In order to improve the use intensity and maintenance efficiency of medium frequency furnace dry composite furnace linings, and to facilitate the full mixing of raw materials for producing linings, production processes and equipment for medium frequency furnace dry composite furnace linings are provided. Summary of the invention

[0005] The purpose of the present invention is to provide a production process and equipment for dry composite furnace lining of a medium frequency furnace in order to solve the technical problems in the background technology.

[0006] To achieve the above object, the present invention provides the following technical solution: a production process of dry composite furnace lining of medium frequency furnace, comprising the following materials by mass fraction: Dense fused corundum, 45-50 parts; Quartz sand, 15-20 parts; Quartz powder, 15-20 parts; Ceramic fiber, 5-10 parts; Silicon carbide ultrafine powder, 3-8 parts; Sodium tripolyphosphate, 1-5 parts; Boric acid, 1-5 parts; The specific steps are as follows: Step 1: Use a mixing device to weigh dense fused corundum, quartz sand, quartz powder, ceramic fiber, and silicon carbide ultrafine particles in proportion and mix them evenly; Step 2: Add the raw materials mixed in step 1 into a forced mixer and stir them. After stirring evenly, add sodium tripolyphosphate and boric acid and stir evenly. Then, use a dry ramming method to ram the furnace lining to the bottom and surrounding of the medium frequency furnace groove. Step 3: After the overall construction in the furnace is implemented, it is naturally dried for 24 hours to complete the hydration reaction process; If it is a local repair work inside the furnace, dry it naturally for 5-10 hours; Finally, the construction area is evenly heated and baked with a heating device for 24-48 hours, and the maximum heating temperature does not exceed 300°C.

[0007] The production equipment of the production process of medium frequency furnace dry composite furnace lining includes the mixing equipment used in step one, the mixing equipment includes a mounting seat, a stirring barrel is fixedly mounted on the outer wall of the mounting seat, a feeding port is arranged at the top of the stirring barrel, a connecting pipe is arranged at the bottom end of the stirring barrel, a discharge pipe is fixedly connected to the bottom end of the connecting pipe, a first motor is mounted at the end of the discharge pipe away from the opening, a conveying shaft is connected to the output end of the first motor, the material in the stirring barrel is stirred by a stirring mechanism, and the raw materials in the stirring barrel are discharged by the discharge mechanism.

[0008] As a further solution of the present invention: the stirring mechanism includes a second motor, the second motor is installed at the top of the stirring barrel, the output end of the second motor is connected to a stirring shaft, the outer wall of the stirring shaft is fixedly connected to a stirring rod, the outer wall of the stirring shaft is located inside the stirring barrel and is fixedly connected to a first spur gear, the inside of the stirring barrel is located on the outer wall of the first spur gear and is rotatably connected to a second spur gear, the inner cavity of the stirring barrel is rotatably connected to a rotating frame, the second spur gear is in contact with the rotating frame, the inner cavity of the rotating frame is symmetrically provided with stirring plates, one end of the stirring plate is fixedly connected to a connecting shaft The gear train is configured to be coupled to the first gear and to have a contact plate disposed inside the gear train, wherein the contact plate is located on a line connecting the first gear and the contact plate of the first gear.

[0009] As a further scheme of the present invention: the discharging mechanism includes an active groove, the active groove is opened in the interior of the mounting seat, the support plate is slidably connected to the inner wall of the active groove, the outer wall of the mounting seat is rotatably connected to a rotating block, one end of the rotating block is fixedly connected to a screw rod, the screw rod extends to the interior of the supporting plate, and the interior of the mounting seat is slidably connected to a pushing frame extending to the inner cavity of the active groove, the interior of the mounting seat is located at a displacement block that is slidably connected to the bottom of the pushing frame, the displacement block and the mounting seat are connected with a spring, one end of the displacement block is located at the outer wall of the mounting seat and is fixedly connected to a baffle, the baffle is used to close the opening of the discharging pipe, the outer wall of the mounting seat is provided with a fixed groove, the top of the mounting seat is located at one side of the rotating block and is fixedly connected to a fixed seat, the inner wall of the fixed seat is rotatably connected to a fixing rod, the inner wall of the fixed seat is slidably connected to a positioning block extending to the inner wall of the fixed seat, the outer wall of the fixed seat is rotatably connected to a rotating column, and one end of the rotating column is fixedly connected to a threaded rod, and the threaded rod extends into the interior of the positioning block.

[0010] As a further solution of the present invention: the first spur gear is meshed with the second spur gear, the outer wall of the rotating frame is in contact with the inner wall of the mixing barrel, the inner ring of the rotating frame is provided with gear teeth, and the gear teeth are meshed with the second spur gear.

[0011] As a further solution of the present invention: an annular tooth groove is formed on the inner wall of the mixing barrel, the third spur gear is meshed with the annular tooth groove, and the first bevel gear is meshed with the second bevel gear.

[0012] As a further solution of the present invention: the outer wall of the support plate is fitted with the inner wall of the movable groove, and a first threaded hole is formed on the outer wall of the support plate, and the first threaded hole matches the screw rod.

[0013] As a further solution of the present invention: the pushing frame is in a Y-shape, and a first inclined surface is provided at one end of the pushing frame located in the inner cavity of the movable groove.

[0014] As a further solution of the present invention: a second inclined surface is provided at one end of the displacement block, and the bottom end of the pushing frame is in contact with the second inclined surface.

[0015] As a further solution of the present invention: the outer wall of the fixing rod is fitted with the inner wall of the fixing groove, and the outer wall of the positioning block is provided with a second threaded hole, and the second threaded hole matches the threaded rod.

[0016] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention improves the production process of medium frequency furnace dry composite furnace lining materials, adjusts the component ratio and process parameters, so that the prepared lining material is not only suitable for overall construction operations, but also suitable for local repair of the target area. The lining material after construction has high strength and the construction time can be shortened by 30%-50% compared with the existing technology, effectively improving the repair efficiency and avoiding long-term shutdown and maintenance to affect the normal production operation of the medium frequency furnace dry composite furnace.

[0017] 2. By setting up a stirring mechanism, the second motor drives the stirring shaft to rotate, the rotation of the stirring shaft drives the stirring rod to move in a circle, and at the same time, the rotation of the stirring shaft drives the rotating frame to rotate, the rotation of the rotating frame drives the stirring plate to move in a circle, the stirring plate and the stirring rod move in opposite circles, so as to stir the raw materials, and at the same time, the rotation of the rotating frame drives the stirring plate to rotate, so that the stirring plate automatically rotates during the circular displacement process, thereby improving the stirring effect on the raw materials and facilitating the full mixing of the raw materials.

[0018] 3. By setting up a discharging mechanism, the baffle blocks the opening of the discharging pipe to prevent impurities from entering the discharging pipe through the opening; when discharging, the rotating block is rotated to drive the supporting plate to move, and the supporting plate moves in the movable groove and contacts with the pushing frame, pushing the pushing frame to move, and the movement of the pushing frame drives the displacement block to move, and the movement of the displacement block drives the baffle to move, and the opening of the discharging pipe is automatically opened, which is convenient for discharging the mixed raw materials in the mixing barrel, and when discharging, the opening of the discharging pipe is automatically opened. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a structural schematic diagram of the present invention; Figure 2 is a cross-sectional view of a mixing barrel of the present invention; Figure 3 is a cross-sectional view of a rotating frame of the present invention; Figure 4 It is a structural schematic diagram of the stirring plate of the present invention; Figure 5 is a cross-sectional view of the mounting seat of the present invention; Figure 6 It is a structural schematic diagram of the push frame of the present invention; Figure 7 is a cross-sectional view of a fixing seat of the present invention; Figure 8 It is a schematic diagram of the installation of the positioning block of the present invention.

[0020] In the figure: 1, mounting seat; 2, mixing barrel; 3, connecting pipe; 4, discharging pipe; 5, first motor; 6, conveying shaft; 7, feeding port; 8, stirring mechanism; 801, second motor; 802, stirring shaft; 803, stirring rod; 804, first spur gear; 805, second spur gear; 806, rotating frame; 807, stirring plate; 808, connecting shaft; 809, first bevel gear; 810, second bevel gear; 811, mounting shaft; 812, third spur gear; 813, supporting plate; 9, discharging mechanism; 901, movable groove; 902, screw rod; 903, rotating block; 904, pushing frame; 905, displacement block; 906, spring; 907, baffle; 908, fixed groove; 909, fixed seat; 910, fixed rod; 911, positioning block; 912, threaded rod; 913, rotating column; 10, annular tooth groove. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance. In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", and "set" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal connection of two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances. The following is an explanation of an embodiment of the present invention based on the overall structure of the present invention. Example 1

[0023] See also Figures 1 to 8 In the embodiment of the present invention, the production process of the medium frequency furnace dry composite furnace lining includes the following materials by mass fraction: Dense fused corundum, 45 parts; Quartz sand, 15 parts; Quartz powder, 15 parts; Ceramic fiber, 5 parts; Silicon carbide ultrafine powder, 3 parts; Sodium tripolyphosphate, 1 part; Boric acid, 1 part; The specific steps are as follows: Step 1: Use a mixing device to weigh dense fused corundum, quartz sand, quartz powder, ceramic fiber, and silicon carbide ultrafine particles in proportion and mix them evenly; Step 2: Add the raw materials mixed in step 1 into a forced mixer and stir them. After stirring evenly, add sodium tripolyphosphate and boric acid and stir evenly. Then, use a dry ramming method to ram the furnace lining to the bottom and surrounding of the medium frequency furnace groove. Step 3: After the overall construction in the furnace is implemented, it is naturally dried for 24 hours to complete the hydration reaction process; If it is a local repair work inside the furnace, dry it naturally for 5 hours; Finally, the construction area is evenly heated and baked with a heating device for 24 hours, with the highest heating temperature reaching 280°C.

[0024] The production equipment of dry composite furnace lining of medium frequency furnace, the mixing equipment used in step one, the mixing equipment includes a mounting seat 1, a stirring barrel 2 is fixedly mounted on the outer wall of the mounting seat 1, a feeding port 7 is arranged on the top of the stirring barrel 2, a connecting pipe 3 is arranged on the bottom end of the stirring barrel 2, a discharging pipe 4 is fixedly connected to the bottom end of the connecting pipe 3, a first motor 5 is mounted on the end of the discharging pipe 4 away from the opening, a conveying shaft 6 is connected to the output end of the first motor 5, the material in the stirring barrel 2 is stirred by a stirring mechanism 8, and the raw materials in the stirring barrel 2 are discharged by a discharging mechanism 9, the stirring mechanism 8 includes a second motor 801, the second motor 801 is mounted on the top of the stirring barrel 2, a stirring shaft 802 is connected to the output end of the second motor 801, when the outer wall of the stirring shaft 802 is fixedly connected to the stirring rod 803, the outer wall of the stirring shaft 802 is located inside the stirring barrel 2 and is fixedly connected to the first spur gear 804, the inner part of the stirring barrel 2 is located at the outer wall of the first spur gear 804 and is rotatably connected The inner cavity of the mixing barrel 2 is rotatably connected with a rotating frame 806, the second spur gear 805 is in contact with the rotating frame 806, and the inner cavity of the rotating frame 806 is symmetrically provided with stirring plates 807, one end of the stirring plate 807 is fixedly connected with a connecting shaft 808, the connecting shaft 808 is rotatably connected with the rotating frame 806 and extends to the inside of the rotating frame 806, and one end of the connecting shaft 808 located inside the rotating frame 806 is fixedly connected with a first bevel gear 809, and the rotating frame 806 The inner part of the first bevel gear 809 is rotatably connected to the outer wall of the first bevel gear 809, the inner wall of the second bevel gear 810 is fixedly connected to the mounting shaft 811, the bottom end of the mounting shaft 811 is fixedly connected to the third spur gear 812, the third spur gear 812 extends to the outer wall of the rotating frame 806 and contacts the inner wall of the mixing barrel 2, the mounting seat 1 and the mixing barrel 2 are slidably connected to the inner part of the supporting plate 813, the supporting plate 813 extends to the inner cavity of the mixing barrel 2 and is located at the bottom end of the rotating frame 806.

[0025] In this embodiment: the raw materials are poured into the mixing barrel 2 through the feed port 7, and the raw materials are accumulated on the top of the support plate 813. At this time, the second motor 801 is started, and the second motor 801 drives the mixing shaft 802 to rotate, and the mixing shaft 802 drives the mixing rod 803 to move in a circle. At the same time, the mixing shaft 802 drives the first spur gear 804 to rotate, and the first spur gear 804 drives the second spur gear 805 to rotate, and the second spur gear 805 drives the rotating frame 806 to rotate, and the rotating frame 806 drives the mixing plate 807 to move in a circle, and the mixing plate 807 and the mixing rod 803 move in opposite circles, so as to stir the raw materials. At the same time, the rotating frame 806 drives The third spur gear 812 moves in a circle, and the third spur gear 812 rotates during the movement. The rotation of the third spur gear 812 drives the installation shaft 811 to rotate. The rotation of the installation shaft 811 drives the second bevel gear 810 to rotate. The rotation of the second bevel gear 810 drives the first bevel gear 809 to rotate. The rotation of the first bevel gear 809 drives the connecting shaft 808 to rotate. The rotation of the connecting shaft 808 drives the stirring plate 807 to rotate, so that the stirring plate 807 automatically rotates during the circular displacement, thereby improving the stirring effect of the raw materials. The support plate 813 is used to limit the raw materials to prevent the raw materials from falling directly to the connecting pipe 3 and affecting the mixing and stirring effect, so as to facilitate the full stirring of the raw materials.

[0026] Please refer to Figures 5 and 6 The discharging mechanism 9 includes a movable groove 901, which is opened inside the mounting seat 1, and the support plate 813 is slidably connected to the inner wall of the movable groove 901. The outer wall of the mounting seat 1 is rotatably connected with a rotating block 903, and one end of the rotating block 903 is fixedly connected with a screw rod 902. The screw rod 902 extends to the inside of the support plate 813. The inside of the mounting seat 1 is slidably connected with a pushing frame 904 extending to the inner cavity of the movable groove 901. The inside of the mounting seat 1 is located at the bottom end of the pushing frame 904 and is slidably connected with a displacement block 905. A spring 906 is connected between the displacement block 905 and the mounting seat 1, and one end of the displacement block 905 is located at the mounting seat 1. The outer wall of the mounting seat 1 is fixedly connected with a baffle 907, and the baffle 907 is used to close the opening of the discharge pipe 4. The outer wall of the rotating block 903 is provided with a fixing groove 908. The top of the mounting seat 1 is located on one side of the rotating block 903 and is fixedly connected with a fixing seat 909. The inner wall of the fixing seat 909 is rotatably connected with a fixing rod 910. The interior of the fixing seat 909 is slidably connected with a positioning block 911 extending to the inner wall of the fixing seat 909. The outer wall of the fixing seat 909 is rotatably connected with a rotating column 913, and one end of the rotating column 913 is fixedly connected with a threaded rod 912. The threaded rod 912 extends into the interior of the positioning block 911.

[0027] In this embodiment: when the material is not discharged, the baffle 907 blocks the opening of the discharge pipe 4 to prevent impurities from entering the discharge pipe 4 through the opening, causing the impurities to mix with the raw materials during subsequent discharge; When discharging, the rotating block 903 is rotated, and the rotating block 903 rotates to drive the screw rod 902 to rotate, and the screw rod 902 rotates to drive the supporting plate 813 to move, and the supporting plate 813 moves so that the raw materials on the top of the supporting plate 813 fall into the discharging pipe 4 through the connecting pipe 3 for discharging, and at the same time, the supporting plate 813 moves in the movable groove 901 and contacts with the pushing frame 904, pushing the pushing frame 904 to move, and the pushing frame 904 moves to drive the displacement block 905 to move, and the displacement block 905 moves to drive the baffle 907 to move, and the opening of the discharging pipe 4 is automatically opened, so as to facilitate the discharging of the mixed raw materials in the mixing barrel 2, and when discharging, the opening of the discharging pipe 4 is automatically opened; When the support plate 813 closes the bottom of the mixing barrel 2, the rotating fixing rod 910 enters the fixing groove 908 to fix the rotating block 903, thereby fixing the position of the support plate 813, and at the same time, the rotating column 913 is rotated. The rotating column 913 rotates to drive the threaded rod 912 to rotate, and the rotating threaded rod 912 rotates to drive the positioning block 911 to move. The positioning block 911 contacts the top of the fixing rod 910, so that the fixing rod 910 cannot move out of the fixing groove 908, thereby reinforcing the support plate 813.

[0028] Please refer to Figures 2 to 4 The first spur gear 804 meshes with the second spur gear 805 , the outer wall of the rotating frame 806 fits with the inner wall of the mixing barrel 2 , the inner ring of the rotating frame 806 is provided with gear teeth, and the gear teeth mesh with the second spur gear 805 .

[0029] In this embodiment: the operation of the second motor 801 drives the stirring shaft 802 to rotate, the rotation of the stirring shaft 802 drives the stirring rod 803 to move in a circle, and at the same time, the rotation of the stirring shaft 802 drives the first spur gear 804 to rotate, the rotation of the first spur gear 804 drives the second spur gear 805 to rotate, the rotation of the second spur gear 805 drives the rotating frame 806 to rotate, the rotation of the rotating frame 806 drives the stirring plate 807 to move in a circle, the stirring plate 807 and the stirring rod 803 move in opposite circles, thereby stirring the raw materials.

[0030] Please refer to Figures 2 to 4 The inner wall of the mixing barrel 2 is provided with an annular tooth groove 10 , the third spur gear 812 is meshed with the annular tooth groove 10 , and the first bevel gear 809 is meshed with the second bevel gear 810 .

[0031] In this embodiment: the rotating frame 806 rotates to drive the third spur gear 812 to move in a circular motion, the third spur gear 812 rotates during the movement, the third spur gear 812 rotates to drive the mounting shaft 811 to rotate, the mounting shaft 811 rotates to drive the second bevel gear 810 to rotate, the second bevel gear 810 rotates to drive the first bevel gear 809 to rotate, the first bevel gear 809 rotates to drive the connecting shaft 808 to rotate, the connecting shaft 808 rotates to drive the stirring plate 807 to rotate, so that the stirring plate 807 automatically rotates during the circular displacement.

[0032] Please refer to Figures 5 and 6 The outer wall of the support plate 813 fits with the inner wall of the movable groove 901 , and a first threaded hole is formed on the outer wall of the support plate 813 , which matches with the screw rod 902 .

[0033] In this embodiment: the rotating block 903 is rotated, the rotating block 903 rotates to drive the screw rod 902 to rotate, the screw rod 902 rotates to drive the support plate 813 to move, and the movement of the support plate 813 causes the raw materials on the top of the support plate 813 to fall into the discharge pipe 4 through the connecting pipe 3 for discharge.

[0034] Please refer to Figures 5 and 6 The push frame 904 is in a Y-shape, and a first inclined surface is provided at one end of the push frame 904 located in the inner cavity of the movable groove 901, and a second inclined surface is provided at one end of the displacement block 905, and the bottom end of the push frame 904 contacts the second inclined surface.

[0035] In this embodiment: the support plate 813 moves in the movable groove 901 and contacts the pushing frame 904, pushing the pushing frame 904 to move, the pushing frame 904 moves to push the displacement block 905 to move, the displacement block 905 moves to drive the baffle 907 to move, and the opening of the discharge pipe 4 is automatically opened.

[0036] Please refer to Figures 7 and 8 The outer wall of the fixing rod 910 fits with the inner wall of the fixing groove 908 , and the outer wall of the positioning block 911 is provided with a second threaded hole, which matches the threaded rod 912 .

[0037] In this embodiment: the fixing rod 910 is rotated to enter the fixing groove 908 to fix the rotating block 903, and then the position of the support plate 813 is fixed, and at the same time, the rotating column 913 is rotated, and the rotation of the rotating column 913 drives the threaded rod 912 to rotate, and the rotation of the threaded rod 912 drives the positioning block 911 to move, and the positioning block 911 contacts the top end of the fixing rod 910, so that the fixing rod 910 cannot move out of the fixing groove 908. Example 2

[0038] The production process of dry composite furnace lining for medium frequency furnace includes the following materials by mass fraction: Dense fused corundum, 48 parts; Quartz sand, 18 parts; Quartz powder, 18 parts; Ceramic fiber, 7 parts; Silicon carbide ultrafine powder, 5 parts; Sodium tripolyphosphate, 3 parts; Boric acid, 3 parts; The specific steps are as follows: Step 1: Use a mixing device to weigh dense fused corundum, quartz sand, quartz powder, ceramic fiber, and silicon carbide ultrafine particles in proportion and mix them evenly; Step 2: Add the raw materials mixed in step 1 into a forced mixer and stir them. After stirring evenly, add sodium tripolyphosphate and boric acid and stir evenly. Then, use a dry ramming method to ram the furnace lining to the bottom and surrounding of the medium frequency furnace groove. Step 3: After the overall construction in the furnace is implemented, it is naturally dried for 24 hours to complete the hydration reaction process; If it is a local repair work inside the furnace, dry it naturally for 8 hours; Finally, the construction area was evenly heated and baked with a heating device for 36 hours, with the highest heating temperature reaching 260°C.

[0039] The other structures and implementation methods of this embodiment are the same as those of the first embodiment and will not be described in detail. Example 3

[0040] The production process of dry composite furnace lining for medium frequency furnace includes the following materials by mass fraction: Dense fused corundum, 50 parts; Quartz sand, 20 parts; Quartz powder, 20 parts; Ceramic fiber, 10 parts; Silicon carbide ultrafine powder, 8 parts; Sodium tripolyphosphate, 5 parts; Boric acid, 5 parts; The specific steps are as follows: Step 1: Use a mixing device to weigh dense fused corundum, quartz sand, quartz powder, ceramic fiber, and silicon carbide ultrafine particles in proportion and mix them evenly; Step 2: Add the raw materials mixed in step 1 into a forced mixer and stir them. After stirring evenly, add sodium tripolyphosphate and boric acid and stir evenly. Then, use a dry ramming method to ram the furnace lining to the bottom and surrounding of the medium frequency furnace groove. Step 3: After the overall construction in the furnace is implemented, it is naturally dried for 24 hours to complete the hydration reaction process; If it is a local repair work inside the furnace, dry it naturally for 10 hours; Finally, the construction area is evenly heated and baked with a heating device for 48 hours, with the highest heating temperature reaching 300°C.

[0041] The other structures and implementation methods of this embodiment are the same as those of the first embodiment and will not be described in detail.

[0042] What is described above is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. The production process of dry composite furnace lining for medium frequency furnace is characterized by: The following materials are included: Dense fused corundum, 45-50 parts; Quartz sand, 15-20 parts; Quartz powder, 15-20 parts; Ceramic fiber, 5-10 parts; Silicon carbide ultrafine powder, 3-8 parts; Sodium tripolyphosphate, 1-5 parts; Boric acid, 1-5 parts; The specific steps are as follows: Step 1: Use a mixing device to weigh dense fused corundum, quartz sand, quartz powder, ceramic fiber, and silicon carbide ultrafine particles in proportion and mix them evenly; Step 2: Add the raw materials mixed in step 1 into a forced mixer and stir them. After stirring evenly, add sodium tripolyphosphate and boric acid and stir evenly. Then, use a dry ramming method to ram the furnace lining to the bottom and surrounding of the medium frequency furnace groove. Step 3: After the overall construction in the furnace is implemented, it is naturally dried for 24 hours to complete the hydration reaction process; If it is a local repair work inside the furnace, dry it naturally for 5-10 hours; Finally, the construction area is evenly heated and baked with a heating device for 24-48 hours, and the maximum heating temperature does not exceed 300°C.

2. The production equipment of the production process of the medium frequency furnace dry composite furnace lining according to claim 1 is characterized in that: The invention comprises a mixing device used in step 1, wherein the mixing device comprises a mounting seat (1), a stirring barrel (2) is fixedly mounted on the outer wall of the mounting seat (1), a feeding port (7) is arranged at the top end of the stirring barrel (2), a connecting pipe (3) is arranged at the bottom end of the stirring barrel (2), a discharge pipe (4) is fixedly connected to the bottom end of the connecting pipe (3), a first motor (5) is mounted at the end of the discharge pipe (4) away from the opening, a conveying shaft (6) is connected to the output end of the first motor (5), the material in the stirring barrel (2) is stirred by a stirring mechanism (8), and the raw material in the stirring barrel (2) is discharged by a discharge mechanism (9).

3. The production equipment of the production process of the medium frequency furnace dry composite furnace lining according to claim 2 is characterized in that: The stirring mechanism (8) comprises a second motor (801), the second motor (801) being mounted on the top of the stirring barrel (2), the output end of the second motor (801) being connected to a stirring shaft (802), the outer wall of the stirring shaft (802) being fixedly connected to a stirring rod (803), the outer wall of the stirring shaft (802) being located inside the stirring barrel (2) and being fixedly connected to a first spur gear (804), the inner wall of the stirring barrel (2) being located on the outer wall of the first spur gear (804) being rotatably connected to a second spur gear (805), the inner cavity of the stirring barrel (2) being rotatably connected to a rotating frame (806), the second spur gear (805) being in contact with the rotating frame (806), the inner cavity of the rotating frame (806) being symmetrically provided with stirring plates (807), one end of the stirring plate (807) being fixedly connected to a connecting shaft (808), the connecting shaft (808) 808) is rotatably connected to the rotating frame (806) and extends to the interior of the rotating frame (806); one end of the connecting shaft (808) located inside the rotating frame (806) is fixedly connected to a first bevel gear (809); the interior of the rotating frame (806) is located on the outer wall of the first bevel gear (809) and is rotatably connected to a second bevel gear (810); the inner wall of the second bevel gear (810) is fixedly connected to a mounting shaft (811); the bottom end of the mounting shaft (811) is fixedly connected to a third spur gear (812); the third spur gear (812) extends to the outer wall of the rotating frame (806) and contacts the inner wall of the mixing barrel (2); a support plate (813) is slidably connected to the interior of the mounting seat (1) and the mixing barrel (2); the support plate (813) extends to the inner cavity of the mixing barrel (2) and is located at the bottom end of the rotating frame (806).

4. The production equipment of the production process of the medium frequency furnace dry composite furnace lining according to claim 3 is characterized in that: The discharging mechanism (9) comprises a movable groove (901), wherein the movable groove (901) is provided inside the mounting seat (1), the support plate (813) is slidably connected to the inner wall of the movable groove (901), the outer wall of the mounting seat (1) is rotatably connected to a rotating block (903), one end of the rotating block (903) is fixedly connected to a screw rod (902), the screw rod (902) extends to the inside of the support plate (813), the inside of the mounting seat (1) is slidably connected to a pushing frame (904) extending to the inner cavity of the movable groove (901), the inside of the mounting seat (1) is slidably connected to a displacement block (905) located at the bottom end of the pushing frame (904), the displacement block (905) is connected to the mounting seat (1) with a spring (906), the displacement block (905) is A baffle (907) is fixedly connected to the outer wall of the mounting seat (1) at one end, and the baffle (907) is used to close the opening of the discharge pipe (4). A fixing groove (908) is provided on the outer wall of the rotating block (903). The top of the mounting seat (1) is fixedly connected to a fixing seat (909) at one side of the rotating block (903). A fixing rod (910) is rotatably connected to the inner wall of the fixing seat (909). A positioning block (911) extending to the inner wall of the fixing seat (909) is slidably connected inside the fixing seat (909). A rotating column (913) is rotatably connected to the outer wall of the fixing seat (909). A threaded rod (912) is fixedly connected to one end of the rotating column (913). The threaded rod (912) extends into the interior of the positioning block (911).

5. The production equipment of the production process of the medium frequency furnace dry composite furnace lining according to claim 3 is characterized in that: The first spur gear (804) meshes with the second spur gear (805), the outer wall of the rotating frame (806) fits with the inner wall of the mixing barrel (2), and the inner ring of the rotating frame (806) is provided with gear teeth, which mesh with the second spur gear (805).

6. The production equipment of the production process of the medium frequency furnace dry composite furnace lining according to claim 3 is characterized in that: An annular tooth groove (10) is provided on the inner wall of the mixing barrel (2), the third spur gear (812) meshes with the annular tooth groove (10), and the first bevel gear (809) meshes with the second bevel gear (810).

7. The production equipment of the production process of the medium frequency furnace dry composite furnace lining according to claim 4 is characterized in that: The outer wall of the support plate (813) fits the inner wall of the movable groove (901), and a first threaded hole is formed on the outer wall of the support plate (813), and the first threaded hole matches the screw rod (902).

8. The production equipment of the production process of the medium frequency furnace dry composite furnace lining according to claim 4 is characterized in that: The pushing frame (904) is in a Y-shape, and a first inclined surface is provided at one end of the pushing frame (904) located in the inner cavity of the movable groove (901).

9. The production equipment of the production process of the medium frequency furnace dry composite furnace lining according to claim 4 is characterized in that: One end of the displacement block (905) is provided with a second inclined surface, and the bottom end of the pushing frame (904) is in contact with the second inclined surface.

10. The production equipment of the production process of the medium frequency furnace dry composite furnace lining according to claim 4, characterized in that: The outer wall of the fixing rod (910) fits with the inner wall of the fixing groove (908), and the outer wall of the positioning block (911) is provided with a second threaded hole, and the second threaded hole matches the threaded rod (912).