Manganese zinc ferrite material as well as preparation method and application thereof

By adding specific additives to the manganese-zinc ferrite material and optimizing the preparation process, a high-resistivity grain structure is formed, which solves the problem of high power consumption of the manganese-zinc ferrite material under high temperature conditions and achieves a temperature range of 100 to 160 Low loss performance within the ℃ range meets the high efficiency requirements of electric vehicle fast charging and new energy vehicle platforms.

CN118771874AActive Publication Date: 2024-10-15HENGDIAN GRP DMEGC MAGNETICS CO LTD +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410839446.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-15
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

Existing manganese-zinc ferrite materials have high power consumption under high temperature conditions and are difficult to meet the high efficiency requirements of electric vehicle fast charging and new energy vehicle platforms operating at high voltages.

Method used

Using Fe2O3, ZnO, MnO as the main materials, SnO2, SiO2, CaO, Nb2O5, ZrO2, Co2O3 as additives, through pre-sintering and sintering process optimization, a high resistivity grain structure is formed, which reduces eddy current and hysteresis losses and realizes manganese Zinc ferrite material has low loss performance in the temperature range of 100~160℃.

Benefits of technology

Under the conditions of 100kHz and 200mT, the overall power consumption of manganese-zinc ferrite materials is reduced to 360kW/m3, and the power consumption is ≤320kW/m3 at 140℃, which significantly improves the energy conversion efficiency of electronic devices under ultra-high temperature and high current conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004914012620000141
    Figure BDA0004914012620000141
  • Figure BDA0004914012620000151
    Figure BDA0004914012620000151
  • Figure BDA0004914012620000161
    Figure BDA0004914012620000161
Patent Text Reader

Abstract

The invention provides a manganese zinc ferrite material and a preparation method and application thereof, the manganese zinc ferrite material comprises main materials and additives, the main materials comprise Fe2O3, ZnO and MnO, and the additives comprise SnO2, SiO2, CaO, Nb2O5, ZrO2 and Co2O3. The manganese-zinc ferrite material disclosed by the invention is relatively low in overall loss in a temperature range of 100-160 DEG C, and the energy conversion efficiency of an electronic device under ultrahigh-temperature and large-current conditions can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of magnetic materials and relates to a manganese-zinc ferrite material and a preparation method and application thereof. Background Art

[0002] As a functional material, soft ferrite has played an important role in promoting the development of the national economy and has been widely used in various fields. With the rapid development of digital technology, automotive electronics, network communications, energy, biotechnology and national defense technology, higher requirements have been put forward for electronic devices, and the miniaturization, intelligence, high efficiency and integration of electronic devices have also led to the continuous development of transformers.

[0003] Power-type manganese-zinc ferrite is mainly used in switching power supplies of various electronic devices such as computers and flat-screen TVs, as well as on-board chargers (OBCs). The lightweight, miniaturization, and planarization development of these devices have put forward higher requirements for reducing the size of the devices.

[0004] With the popularity of electric vehicles, onboard chargers (OBC) and charging piles are widely used. With the demand for fast charging of electric vehicles, the power requirements for OBC and charging piles will inevitably increase significantly. As the new energy vehicle platform operates at high voltage, the temperature of OBC and charging piles must be maintained at least above 100°C during operation. In order to fully realize the high-efficiency conversion of energy, higher requirements are placed on the power consumption of power-type manganese-zinc ferrite at high temperatures.

[0005] CN101169996A discloses a low-power Mn-Zn ferrite magnetic material for use in ultra-high temperature conditions and its preparation method. The main ingredients of the ferrite magnetic material include: Fe2O3: 52-56 mol%, ZnO: 2-10 mol%, MnO: 38-42 mol%, and additives include: CaCO3: 400-800 ppm, Nb2O5: 100-400 ppm, ZrO2: 100-800 ppm, Co2O3: 1000-5000 ppm or a combination thereof. The unit volume loss Pcv is less than or equal to 350 kW / m at 140°C, 100 kHz, and 200 mT. 3 , its loss is relatively high, and it only focuses on the temperature point of 140℃, so its application range is not wide.

[0006] CN102219486A discloses a high-temperature, low-loss manganese-zinc ferrite material. The high-temperature, low-loss manganese-zinc ferrite material includes the main ingredients: Fe2O3: 52-53.5mol%, ZnO: 6-9mol%, MnO: 37.5-42mol%, and the additive component is selected from at least one of SiO2, CaCO3, Nb2O5, V2O5, ZrO2, Co2O3, NiO, and Li2CO3. Although the unit volume loss P is within the temperature range of 120-150°C under the conditions of 100kHz and 200mT, the cv All less than 450kW / m 3 , but its loss is still high.

[0007] CN112125655A discloses a method for preparing a high-temperature, high-frequency, low-loss ferrite. The ferrite comprises the main ingredients of Fe2O3: 52-58 mol%, ZnO: 9-13 mol%, MnCO3: 31-38 mol%, NiO: 0.5-5 mol%, and additives of SnO2: 0.02-0.3 wt%, TiO2: 0.02-0.3 wt%, and V2O5: 0.02-0.3 wt%. Although the power loss is low at a high operating temperature of 120-180°C in a frequency range of 100-1000 kHz, the loss is still high.

[0008] In summary, it is of great significance to provide a high-temperature, low-loss manganese-zinc ferrite with low overall loss in the temperature range of 100 to 160°C and its preparation method and application, which are used to meet the high efficiency requirements of devices such as OBC and charging piles under ultra-high temperature and high current conditions. Summary of the invention

[0009] The object of the present invention is to provide a manganese-zinc ferrite material and a preparation method and application thereof. The manganese-zinc ferrite material of the present invention has a relatively low overall loss in the temperature range of 100 to 160° C., and can improve the energy conversion efficiency of electronic devices under ultra-high temperature and high current conditions.

[0010] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0011] In a first aspect, the present invention provides a manganese-zinc ferrite material, comprising a main ingredient and additives, wherein the main ingredient comprises Fe2O3, ZnO and MnO, and the additive comprises SnO2, SiO2, CaO, Nb2O5, ZrO2 and Co2O3.

[0012] The present invention adds SnO2, SiO2, CaO, Nb2O5, ZrO2 and Co2O3 as additives to the manganese-zinc ferrite material. The coordinated effect of various additives can not only reduce eddy current loss and hysteresis loss, but also have the effect of wide temperature range and loss reduction. The manganese-zinc power ferrite material achieves low loss (manganese-zinc ferrite power consumption P under the conditions of 100kHz and 200mT) in a wide high temperature range (100-160°C). cv ≤360kW / m 3 )performance.

[0013] Preferably, based on the total molar amount of the main material as 100%, the molar fraction of Fe2O3 is 52.4-52.8%, for example: 52.4%, 52.5%, 52.6%, 52.7% or 52.8%, etc., not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0014] In the prior art, the proportion of iron oxide in the main material of manganese-zinc ferrite is about 54%. The present invention improves the resistivity of the manganese-zinc ferrite material by appropriately reducing the content of Fe2O3, thereby reducing eddy current loss; but too low Fe2O3 content is not conducive to reducing hysteresis loss.

[0015] Preferably, based on the total molar amount of the main material as 100%, the molar fraction of ZnO is 7-10%, for example: 7%, 7.5%, 8%, 9% or 10%, etc., not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0016] Controlling the ZnO content within the above range is beneficial to controlling the valley point and BS. Specifically, a ZnO content lower than 7% is not conducive to reducing hysteresis loss; a ZnO content higher than 10% is not conducive to increasing Bs, and will also move the valley point toward low temperature, which is not conducive to reducing high temperature loss.

[0017] Preferably, based on the total molar amount of the main material as 100%, the molar fraction of MnO is 36-42%, for example, 36%, 37%, 37.2%, 38%, 39%, 40% or 42%, etc., not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] Preferably, the added amount of SnO2 is 0.12-0.18wt% of the total mass of the main material, for example: 0.12wt%, 0.13wt%, 0.14wt%, 0.16wt% or 0.18wt%, etc., not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, the added amount of SiO2 is 0.02-0.04wt% of the total mass of the main material, for example: 0.02wt%, 0.025wt%, 0.03wt%, 0.035wt% or 0.04wt%, etc., not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the added amount of CaO is 0.08-0.15wt% of the total mass of the main material, for example: 0.08wt%, 0.1wt%, 0.11wt%, 0.13wt% or 0.15wt%, etc., not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0021] Preferably, the added amount of Nb2O5 is 0.02-0.04wt% of the total mass of the main material, for example: 0.02wt%, 0.025wt%, 0.03wt%, 0.035wt% or 0.04wt%, etc., not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0022] Preferably, the added amount of ZrO2 is 0.02-0.04wt% of the total mass of the main material, for example: 0.02wt%, 0.025wt%, 0.03wt%, 0.035wt% or 0.04wt%, etc., not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0023] The combined addition of SiO2, CaCO3, Nb2O5 and ZrO2 forms a high resistance layer at the grain boundary to increase the grain boundary resistivity, while improving the uniformity of the grains and reducing pores, thereby reducing eddy current loss and hysteresis loss.

[0024] Preferably, the added amount of Co2O3 is 0.2-0.4wt% of the total mass of the main material, for example: 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt% or 0.4wt%, etc., not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0025] Co2O3 and Fe 2+ A synergistic effect is formed. Due to its positive K1 (magnetocrystalline anisotropy constant), it compensates for the negative K1 value of manganese-zinc ferrite, reduces hysteresis loss, and achieves the effect of wide temperature range and loss reduction.

[0026] In a second aspect, the present invention provides a method for preparing the manganese-zinc ferrite material as described in the first aspect, the preparation method comprising the following steps:

[0027] (1) mixing and grinding the main material and the first additive, and then pre-calcining to obtain a pre-calcined material;

[0028] (2) mixing and grinding the pre-sintered material and the second additive, and then granulating the material, and sintering the material obtained by the granulation to obtain the manganese-zinc ferrite material;

[0029] Wherein, the first additive includes SnO2, and the second additive includes SiO2, CaCO3, Nb2O5, ZrO2 and Co2O3.

[0030] The present invention pre-mixes SnO2 with the main material for pre-sintering, and SnO2 enters the grains to inhibit Fe 2+ with Fe 3+ The electron transition between them can increase the resistivity inside the grains, reduce the eddy current loss, and then the pre-sintered material is mixed with other additives and sintered. In addition, some SnO2 that has not entered the ferrite lattice is segregated in the grain boundary layer. Since the melting point of SnO2 (1127°C) is lower than the sintering temperature, a liquid phase will be formed during sintering, thereby promoting solid-phase reaction and accelerating ion diffusion. When the ion diffusion rate is too fast, some pores cannot be eliminated in time and thus remain inside the grains. Compared with adding SnO2 in step (2), the more beneficial effect of adding SnO2 in step (1) is that Sn 4+ It is easier to enter the lattice and enhance Fe 2+ with Fe 3+ It inhibits the electron transition between the two and increases the grain resistivity, reduces the segregation of SnO2 in the grain boundary layer, weakens the solid phase reaction, and reduces the porosity.

[0031] Preferably, the mixed grinding in step (1) includes sand grinding.

[0032] Preferably, the mixing and grinding time in step (1) is 2 to 4 hours, for example, 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours, etc., and is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0033] Preferably, the temperature of the pre-firing treatment in step (1) is 700-800°C, for example, 700°C, 720°C, 750°C, 780°C or 800°C, etc., and is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0034] Preferably, the pre-burning treatment time in step (1) is 2 to 4 hours, for example, 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours, etc., not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0035] Preferably, the atmosphere of the pre-firing treatment in step (1) comprises air and / or oxygen.

[0036] Preferably, the mixed grinding in step (2) includes sand grinding, which is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] Preferably, the mixing and grinding time in step (2) is 2 to 4 hours, for example: 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours.

[0038] Preferably, after the mixing and grinding in step (2), a drying treatment is performed before the granulation treatment. The numerical values ​​are not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0039] Preferably, the median particle size D50 of the powder obtained by the drying treatment is 0.9-1.2 μm, for example, 0.9 μm, 0.95 μm, 1 μm, 1.1 μm or 1.2 μm, etc., and is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] Preferably, the granulating agent in the granulation treatment in step (2) comprises PVA and / or PVB.

[0041] Preferably, the mass ratio of the granulating agent to the powder obtained by drying is 0.05 to 0.1:1, for example, 0.05:1, 0.06:1, 0.08:1, 0.09:1 or 0.1:1, etc., and is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] Preferably, the sintering treatment in step (2) includes heat preservation and cooling treatment.

[0043] Preferably, the insulation temperature is 1240-1280°C, for example, 1240°C, 1250°C, 1260°C, 1270°C or 1280°C, etc., and is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] Preferably, the insulation time is 150 to 250 minutes, for example, 150 minutes, 180 minutes, 200 minutes, 220 minutes or 250 minutes, etc., and is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0045] Preferably, the volume percentage of oxygen in the insulating atmosphere is 4-6%, for example, 4%, 4.5%, 5%, 5.5% or 6%, etc., not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] Preferably, the cooling treatment includes one-step cooling and two-step cooling.

[0047] Preferably, the terminal temperature of the one-step cooling is ≥ 1100°C.

[0048] Preferably, the volume percentage of oxygen in the one-step cooling atmosphere is 1.5-3.5%, for example, 1.5%, 2%, 2.5%, 3% or 3.5%, etc., not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0049] Preferably, the terminal temperature of the two-step cooling is 900-1100°C, for example, 900°C, 950°C, 1000°C, 1050°C or 1100°C, etc., not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0050] Preferably, the volume percentage of oxygen in the atmosphere of the second-step cooling is 0.3-0.8%, for example, 0.3%, 0.4%, 0.5%, 0.6% or 0.8%, etc., not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0051] In a third aspect, the present invention provides an electronic device, wherein the electronic device comprises the manganese-zinc ferrite material as described in the first aspect.

[0052] Compared with the prior art, the present invention has the following beneficial effects:

[0053] (1) The present invention adds SnO2, SiO2, CaO, Nb2O5, ZrO2 and Co2O3 as additives to the manganese-zinc ferrite material. The coordinated effect of various additives can not only reduce eddy current loss and hysteresis loss, but also have the effect of wide temperature range and loss reduction.

[0054] (2) The present invention adjusts the preparation process and the ratio of raw materials to make the manganese-zinc power ferrite material have a power consumption P of 100kHz, 200mT in the temperature range of 100-160°C. cv ≤360kW / m 3 , and at 140°C, at 100kHz, 200mT, the power consumption of Mn-Zn ferrite is P cv ≤320kW / m 3 . DETAILED DESCRIPTION

[0055] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0056] The material described in the embodiment of the present invention is a mixed material obtained by mixing the materials in each step. For example, the material described in step (1) of embodiment 1 is a mixture of the main material and SnO2, and the material described in step (2) is a mixture of the remaining additives and the pre-burned material.

[0057] Example 1

[0058] The present embodiment provides a manganese-zinc ferrite material, which consists of a main material and an additive. The main material is 52.4 mol% of Fe2O3 and 10 mol% of ZnO, and the rest is MnO; the additive is based on the total mass of the main material and includes 1500 ppm (i.e. 0.15%) of SnO2, 300 ppm (i.e. 0.03%) of SiO2, 1000 ppm (0.1%) of CaO, 300 ppm (i.e. 0.03%) of Nb2O5, 200 ppm (i.e. 0.02%) of ZrO2 and 3900 ppm (i.e. 0.39%) of Co2O3.

[0059] The preparation method of the manganese-zinc ferrite material is as follows:

[0060] (1) mixing the main material and SnO2, and performing a sand milling for 3 hours, during which the mass ratio of the material, zirconium balls and water is 1:6:1.5, and then pre-calcining at 750°C for 3 hours in an air atmosphere after drying to obtain a pre-calcined material;

[0061] (2) Mix the remaining additives and the obtained pre-burned material, and perform secondary sand grinding for 3 hours. During the process, the mass ratio of the material, zirconium balls and water is 1:6:1.5, and the median particle size D50 of the sand milled material is 1 μm. Then, 8 wt% of the PVA by mass of the dried powder after the secondary sand grinding is mixed for granulation and molding, and finally sintering. The sintering includes a 1260°C insulation section for 180 minutes and a cooling section. The oxygen content in the insulation section is 5 vol%, and the oxygen content in the cooling section to 1100°C is 1.5 vol%, and the oxygen content at 1100°C-900°C is 0.3 vol%, to obtain the manganese-zinc power ferrite material.

[0062] Example 2

[0063] The present embodiment provides a manganese-zinc ferrite material, which is composed of a main material and an additive. The main material is 52.8 mol% of Fe2O3 and 7 mol% of ZnO, and the rest is MnO; the additive is based on the total mass of the main material and includes 1200 ppm of SnO2, 200 ppm of SiO2, 1000 ppm of CaO, 400 ppm of Nb2O5, 300 ppm of ZrO2 and 2400 ppm of Co2O3. The preparation method of the manganese-zinc ferrite material is as follows:

[0064] (1) mixing the main material and SnO2, and performing a sand milling for 2 hours, during which the mass ratio of the material, zirconium balls and water is 1:5:2, and then pre-calcining at 700°C for 4 hours in an air atmosphere after drying to obtain a pre-calcined material;

[0065] (2) Mix the remaining additives and the obtained pre-burned material, and perform secondary sand grinding for 4 hours. During the process, the mass ratio of the material, zirconium balls and water is 1:5:2, and the median particle size D50 of the sand milled material is 0.9 μm. Then, mix the dried powder after the secondary sand grinding with 5 wt% of PVA for granulation and molding, and finally sintering. The sintering includes a 1240°C insulation section for 180 minutes and a cooling section. The oxygen content in the insulation section is 5 vol%. The oxygen content in the process of cooling to 1100°C is 3.4 vol%, and the oxygen content at 1100°C-900°C is 0.6 vol%, to obtain the manganese-zinc power ferrite material.

[0066] Example 3

[0067] The present embodiment provides a manganese-zinc ferrite material, the manganese-zinc power ferrite material is composed of a main material and an additive, the main material is 52.5 mol% Fe2O3 and 9.5 mol% ZnO, and the rest is MnO; the additive is based on the total mass of the main material, including 1400 ppm SnO2, 200 ppm SiO2, 800 ppm CaO, 400 ppm Nb2O5, 400 ppm ZrO2 and 2400 ppm Co2O3, the preparation method of the manganese-zinc ferrite material is as follows:

[0068] (1) mixing the main material and SnO2, and performing a sand milling for 4 hours, during which the mass ratio of the material, zirconium balls and water is 1:7:1, and then pre-calcining at 800°C for 2 hours in an air atmosphere to obtain a pre-calcined material;

[0069] (2) Mixing the remaining additives and the obtained pre-burned material, and performing secondary sand grinding for 2 hours, during which the mass ratio of the material, zirconium balls and water is 1:7:1, and the median particle size D50 of the sand milled material is 1.2 μm, and then mixing with PVA with a mass 10 wt% of the dried powder after the secondary sand grinding for granulation and molding, and finally sintering, the sintering includes a 1280°C insulation section for 150 minutes and a cooling section, the oxygen content in the insulation section is 5 vol%, and the oxygen content in the process of cooling to 1100°C is 1.6 vol%, and the oxygen content at 1100°C-900°C is 0.5 vol%, to obtain the manganese-zinc power ferrite material.

[0070] Example 4

[0071] The present embodiment provides a manganese-zinc ferrite material, the manganese-zinc power ferrite material is composed of a main material and an additive, the main material is 52.6 mol% Fe2O3 and 9 mol% ZnO, and the rest is MnO; the additive is 1600 ppm SnO2, 300 ppm SiO2, 1300 ppm CaO, 200 ppm Nb2O5, 400 ppm ZrO2 and 2800 ppm Co2O3 based on the total mass of the main material, and the preparation method of the manganese-zinc ferrite material is as follows:

[0072] (1) mixing the main material and SnO2, and performing a sand milling for 3 hours, during which the mass ratio of the material, zirconium balls and water is 1:6:1.5, and then pre-calcining at 750°C for 3 hours in an air atmosphere to obtain a pre-calcined material;

[0073] (2) Mix the remaining additives and the obtained pre-sintered material, and perform secondary sand grinding for 3 hours. During the process, the mass ratio of the material, zirconium balls and water is 1:6:1.5, and the median particle size D50 of the sand mill is 1 μm. Then 8 wt% of PVA is mixed for granulation and molding, and finally sintering is performed. The sintering includes a 1270°C insulation section for 200 minutes and a cooling section. The oxygen content in the insulation section is 5 vol%. In the process of cooling to 1100°C, the oxygen content is 1.8 vol%. The oxygen content at 1100°C-900°C is 0.6 vol%, and the manganese-zinc power ferrite material is obtained.

[0074] Example 5

[0075] The only difference between this embodiment and embodiment 1 is that the amount of Fe2O3 is 52 mol% (the total amount is adjusted by MnO), and the other conditions and parameters are exactly the same as those in embodiment 1.

[0076] Example 6

[0077] The only difference between this embodiment and embodiment 1 is that the amount of Fe2O3 is 53 mol% (the total amount is adjusted by MnO), and the other conditions and parameters are exactly the same as those in embodiment 1.

[0078] Example 7

[0079] The only difference between this embodiment and embodiment 1 is that the amount of ZnO is 11 mol% (the total amount is adjusted by MnO), and the other conditions and parameters are exactly the same as those in embodiment 1.

[0080] Example 8

[0081] The only difference between this embodiment and embodiment 1 is that the amount of ZnO is 6 mol% (the total amount is adjusted by MnO), and the other conditions and parameters are exactly the same as those in embodiment 1.

[0082] Example 9

[0083] The only difference between this embodiment and embodiment 1 is that the mass of SnO2 is 800ppm of the total mass of the main material, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0084] Example 10

[0085] The only difference between this embodiment and embodiment 1 is that the mass of SnO2 is 2000ppm of the total mass of the main material, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0086] Embodiment 11

[0087] The only difference between this embodiment and embodiment 1 is that the mass of SiO2 is 500ppm of the total mass of the main material, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0088] Example 12

[0089] The only difference between this embodiment and embodiment 1 is that the mass of SiO2 is 100 ppm of the total mass of the main material, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0090] Embodiment 13

[0091] The only difference between this embodiment and embodiment 1 is that the mass of CaO is 400 ppm of the total mass of the main material, and other conditions and parameters are exactly the same as those in embodiment 1.

[0092] Embodiment 14

[0093] The only difference between this embodiment and embodiment 1 is that the mass of CaO is 2000 ppm of the total mass of the main material, and other conditions and parameters are exactly the same as those in embodiment 1.

[0094] Embodiment 15

[0095] The only difference between this embodiment and embodiment 1 is that the mass of Nb2O5 is 100 ppm of the total mass of the main material, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0096] Example 16

[0097] The only difference between this embodiment and embodiment 1 is that the mass of Nb2O5 is 500ppm of the total mass of the main material, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0098] Embodiment 17

[0099] The only difference between this embodiment and embodiment 1 is that the mass of ZrO2 is 500ppm of the total mass of the main material, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0100] Embodiment 18

[0101] The only difference between this embodiment and embodiment 1 is that the mass of ZrO2 is 100 ppm of the total mass of the main material, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0102] Embodiment 19

[0103] The only difference between this embodiment and embodiment 1 is that the mass of Co2O3 is 1500ppm of the total mass of the main material, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0104] Embodiment 20

[0105] The only difference between this embodiment and embodiment 1 is that the mass of Co2O3 is 4500ppm of the total mass of the main material, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0106] Embodiment 21

[0107] The only difference between this embodiment and embodiment 1 is that the mass of Co2O3 is 4500ppm of the total mass of the main material, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0108] The only difference between this embodiment and embodiment 1 is that the oxygen content in the cooling section in step (2) is controlled at 4 vol% when the temperature drops to 1100°C, and the oxygen content in the temperature range of 1100-900°C is controlled at 1 vol%. Other conditions and parameters are exactly the same as those in embodiment 1.

[0109] Embodiment 22

[0110] The only difference between this embodiment and embodiment 1 is that the oxygen content in the cooling section in step (2) is controlled at 1 vol% when the temperature drops to 1100°C, and the oxygen content in the temperature range of 1100-900°C is controlled at 0.2 vol%. Other conditions and parameters are exactly the same as those in embodiment 1.

[0111] Comparative Example 1

[0112] The only difference between this comparative example and Example 1 is that SnO2 is not added, and the other conditions and parameters are exactly the same as those in Example 1.

[0113] Comparative Example 2

[0114] The only difference between this comparative example and Example 1 is that SnO2 is added together with other additives in step (2), and the other conditions and parameters are exactly the same as those in Example 1.

[0115] Comparative Example 3

[0116] The only difference between this comparative example and Example 1 is that no CaCO3 is added, and the other conditions and parameters are exactly the same as those in Example 1.

[0117] Comparative Example 4

[0118] The only difference between this comparative example and Example 1 is that Nb2O5 is not added, and the other conditions and parameters are exactly the same as those in Example 1.

[0119] Comparative Example 5

[0120] The only difference between this comparative example and Example 1 is that ZrO2 is not added, and the other conditions and parameters are exactly the same as those in Example 1.

[0121] Comparative Example 6

[0122] The only difference between this comparative example and Example 1 is that Co2O3 is not added, and the other conditions and parameters are exactly the same as those in Example 1.

[0123] Comparative Example 7

[0124] The only difference between this comparative example and Example 1 is that SiO2 is not added, and the other conditions and parameters are exactly the same as those in Example 1.

[0125] Performance Testing:

[0126] The manganese-zinc power ferrite materials obtained in the above examples and comparative examples were placed on a SY8219 test device, and their losses were tested under the conditions of 100kHz, 200mT, T=100°C / 120°C / 140°C / 160°C. The test results are shown in Table 1:

[0127] Table 1

[0128]

[0129]

[0130]

[0131] As can be seen from Table 1, from Examples 1-4, the loss of the manganese-zinc ferrite material prepared by the method of the present invention at 100°C, 100kHz, and 200mT can reach 345kW / m 3 Below, 120℃, 100kHz, 200mT, the loss can reach 320kW / m 3 Below, 140℃, 100kHz, 200mT loss can reach 320kW / m 3 Below, 160℃, 100kHz, 200mT, the loss can reach 355kW / m 3 the following.

[0132] By comparing Example 1 with Examples 5-6, it can be seen that during the preparation process of the manganese-zinc ferrite material of the present invention, the molar proportion of Fe2O3 in the main material will affect its performance. When the molar proportion of Fe2O3 in the main material is controlled at 52.4-52.8%, the performance of the manganese-zinc ferrite obtained is better. If the molar proportion of Fe2O3 in the main material is too high, the high-temperature performance of the material decreases faster. If the molar proportion of Fe2O3 in the main material is too low, the overall performance of the material decreases.

[0133] By comparing Example 1 with Examples 7-8, it can be seen that during the preparation process of the manganese-zinc ferrite material of the present invention, the molar proportion of ZnO in the main material will affect its performance. When the molar proportion of ZnO in the main material is controlled at 7-10%, the performance of the manganese-zinc ferrite obtained is better. If the molar proportion of ZnO in the main material is too high, the high-temperature performance of the material decreases faster. If the molar proportion of ZnO in the main material is too low, the overall performance of the material decreases.

[0134] By comparing Example 1 with Examples 9-10, it can be seen that during the preparation process of the manganese-zinc ferrite material of the present invention, the amount of SnO2 added will affect its performance. By controlling the mass of SnO2 to 0.12-0.18% of the total mass of the main material, the performance of the manganese-zinc ferrite obtained is better. If the amount of SnO2 added is too high or too low, the performance of the material will decrease to varying degrees.

[0135] By comparing Example 1 with Examples 11-20, it can be seen that in the preparation process of the manganese-zinc ferrite material of the present invention, the addition amount of other additives will also affect its performance. The performance of the material is better when the mass of SiO2 is controlled at 0.02-0.04% of the total mass of the main material, the mass of CaCO3 is controlled at 0.08-0.15% of the total mass of the main material, the mass of Nb2O5 is controlled at 0.02-0.04% of the total mass of the main material, the mass of ZrO2 is controlled at 0.02-0.04% of the total mass of the main material, and the mass of Co2O3 is controlled at 0.2-0.4% of the total mass of the main material. If the above range is exceeded, the performance of the material will decrease to varying degrees.

[0136] By comparing Example 1 with Examples 21-22, it can be seen that during the preparation process of the manganese-zinc ferrite material of the present invention, the oxygen content in the atmosphere during the cooling process will also affect its performance. During the cooling process with an end temperature of ≥1100°C, the volume proportion of oxygen in the atmosphere is controlled at 1.5-3.5%. During the cooling process with an end temperature of 900-1100°C, the volume proportion of oxygen in the atmosphere is controlled at 0.3-0.8%. The performance of the manganese-zinc ferrite material is better. If it exceeds the above range, the performance of the material will decrease to varying degrees.

[0137] By comparing Example 1 with Comparative Example 1, it can be seen that the present invention adds SnO2 as an additive to the manganese-zinc ferrite, and SnO2 enters the grains to inhibit Fe 2+ with Fe 3+ The electron transition between them can increase the resistivity inside the grains and reduce the eddy current loss.

[0138] From the comparison between Example 1 and Comparative Example 2, it can be seen that the addition of SnO2 in step (1) is beneficial to the overall performance of the material.

[0139] From the comparison between Example 1 and Comparative Examples 3-7, it can be seen that the combined addition of SiO2, CaCO3, Nb2O5 and ZrO2 forms a high resistance layer at the grain boundary to increase the grain boundary resistivity, while improving the uniformity of the grains and reducing pores, thereby reducing eddy current loss and hysteresis loss. 2+ A synergistic effect is formed. Due to its positive K1 (magnetocrystalline anisotropy constant), it compensates for the negative K1 value of manganese-zinc ferrite, reduces hysteresis loss, and achieves the effect of wide temperature range and loss reduction.

[0140] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A manganese-zinc ferrite material, characterized in that: The manganese-zinc ferrite material comprises a main material and additives, wherein the main material comprises Fe2O3, ZnO and MnO, and the additives comprise SnO2, SiO2, CaO, Nb2O5, ZrO2 and Co2O3.

2. The manganese-zinc ferrite material according to claim 1, characterized in that: Taking the total molar amount of the main material as 100%, the molar fraction of Fe2O3 is 52.4-52.8%; Preferably, based on the total molar amount of the main material being 100%, the molar fraction of ZnO is 7 to 10%; Preferably, based on the total molar amount of the main material being 100%, the molar fraction of MnO is 36-42%.

3. The manganese-zinc ferrite material according to claim 1 or 2, characterized in that: The amount of SnO2 added is 0.12-0.18wt% of the total mass of the main material; Preferably, the amount of SiO2 added is 0.02-0.04wt% of the total mass of the main material; Preferably, the amount of CaO added is 0.08-0.15wt% of the total mass of the main material; Preferably, the addition amount of Nb2O5 is 0.02-0.04wt% of the total mass of the main material; Preferably, the amount of ZrO2 added is 0.02-0.04wt% of the total mass of the main material; Preferably, the added amount of Co2O3 is 0.2-0.4wt% of the total mass of the main material.

4. The method for preparing the manganese-zinc ferrite material according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) mixing and grinding the main material and the first additive, and then pre-calcining to obtain a pre-calcined material; (2) mixing and grinding the pre-sintered material and the second additive, and then granulating the material, and sintering the material obtained by the granulation to obtain the manganese-zinc ferrite material; Among them, the first additive is SnO2, and the second additive includes SiO2, CaCO3, Nb2O5, ZrO2 and Co2O3.

5. The preparation method according to claim 4, characterized in that: The mixed grinding in step (1) includes sand grinding; Preferably, the mixing and grinding time in step (1) is 2 to 4 hours; Preferably, the temperature of the pre-sintering treatment in step (1) is 700-800°C; Preferably, the pre-burning treatment time in step (1) is 2 to 4 hours; Preferably, the atmosphere of the pre-firing treatment in step (1) comprises an oxygen-containing atmosphere; Preferably, the oxygen-containing atmosphere comprises oxygen and / or air.

6. The preparation method according to claim 4 or 5, characterized in that: The mixed grinding in step (2) includes sand grinding; Preferably, the mixing and grinding time in step (2) is 2 to 4 hours; Preferably, after the mixing and grinding in step (2), drying is performed before granulation; Preferably, the median particle size D50 of the powder obtained by the drying process is 0.9 to 1.2 μm.

7. The preparation method according to claim 6, characterized in that: The granulating agent for the granulation process comprises PVA and / or PVB; Preferably, the mass ratio of the granulating agent to the powder obtained by drying is 0.05 to 0.1:

1.

8. The preparation method according to any one of claims 4 to 7, characterized in that: The sintering treatment in step (2) includes heat preservation and cooling treatment; Preferably, the insulation temperature is 1240-1280°C; Preferably, the insulation time is 150 to 250 minutes; Preferably, the volume proportion of oxygen in the heat-insulating atmosphere is 4-6%.

9. The preparation method according to claim 8, characterized in that: The cooling process includes one-step cooling and two-step cooling; Preferably, the terminal temperature of the one-step cooling is ≥1100°C; Preferably, the volume percentage of oxygen in the one-step cooling atmosphere is 1.5-3.5%; Preferably, the terminal temperature of the two-step cooling is 900-1100°C; Preferably, the volume proportion of oxygen in the atmosphere of the second step cooling is 0.3-0.8%.

10. An electronic device, characterized in that: The electronic device comprises the manganese-zinc ferrite material according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Ferrite material

    CN102442820A

  • MnZn ferrite material with relatively high magnetic permeability, wide temperature range and low loss, and preparation method thereof

    CN102745981A

  • Manganese-zinc ferrite with high negative-temperature magnetic conductivity and low high-temperature loss, and preparation method thereof

    CN111362685A

  • Manganese-zinc ferrite material as well as preparation method and application thereof

    CN112592170A

  • Wide-temperature ultralow-loss manganese zinc ferrite material and preparation method thereof

    CN113024239A