HfCxNy-SiC modified C / C composite material and preparation method thereof
By depositing the HfCxNy-SiC layer on the surface of the C/C composite material, the problem of insufficient interface bonding force is solved, and its ablation resistance in high-temperature environments is significantly improved, making it suitable for high-speed aircraft applications.
Patent Information
- Application Number
- CN202410795611.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-19
AI Technical Summary
The existing C/C composite materials have poor interfacial bonding force, which causes the coating to easily peel off in high-temperature and long-term ablation environments, limiting its ablation resistance in high-temperature applications.
HfSi2 and Si3N4 powders are mixed as the infiltration agent, and a HfCxNy-SiC layer is deposited on the surface of the C/C composite material through a reactive infiltration process to enhance the interface bonding force and improve the ablation resistance.
It improves the ablation resistance of C/C composite materials in high-temperature oxygen-containing environments, extends the flight time of high-speed aircraft, has higher hardness and toughness, and is suitable for extreme aerodynamic heat and high-speed particle erosion environments.
Smart Images

Figure CN118771889A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of C / C composite material modification and relates to a HfC x N y -SiC modified C / C composite material and preparation method thereof. Background Art
[0002] Since its discovery in 1958, carbon / carbon composites have been widely used in hot-end components in the aerospace field, such as solid rocket engine nozzles, aircraft nose cones and leading edges, and turbine engine blades, due to their low density, high thermal conductivity, high specific strength, high specific modulus, low thermal expansion coefficient, and mechanical strength that increases instead of decreases with increasing temperature. However, carbon / carbon composites have high oxidation activity, and oxidation weight loss significantly reduces the strength of the material. Poor ablation resistance in high-enthalpy combustion environments and weak oxidation stability under oxygen-containing heat flows have greatly limited the application of carbon / carbon composites.
[0003] Ultra-high temperature ceramics (UHTCs) have a melting point of over 3000°C and a melting point of their oxides of over 1800°C. They are a type of thermal protection material that can maintain relatively stable physical and chemical properties in high temperature environments (>2000°C) and plasma reaction atmospheres and can be reused at temperatures above 1650°C. They are considered to be an ideal introduction material for improving the performance of C / C composites. x N y ) Ultra-high temperature ceramics have a higher melting point than HfC (3890℃), better hardness, toughness and ductility, and can better meet the material performance requirements of the new generation of hypersonic aircraft service environment. x N y There are few studies on HfC. Existing reports mainly focus on some theoretical calculations and x N y Few scholars have considered HfC x N y As a matrix modification component, its influence on the properties of C / C composites was studied.
[0004] Reference "Zhang, J. et al. Ablation behavior of a novel carbonitridesHfC 0.68 N 0.32coating for C / C composites in laser and oxyacetyleneenvironment.Journal of the European Ceramic Society 44,3049-3057." Using HfCl 4 -CH 4 -N 2 -H 2 -Ar system, HfC was deposited on the prefabricated SiC coating on the surface of C / C composite by CVD process. 0.68 N 0.32 The coating material shows good anti-ablation performance in laser and oxyacetylene atmosphere. However, the coating prepared by CVD has poor bonding with the substrate, and the coating is prone to peeling off during high temperature and long-term ablation. Summary of the invention
[0005] The object of the present invention is to provide a HfC x N y -SiC modified C / C composite material and its preparation method solve the problem of poor interface bonding strength in the prior art.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A HfC x N y -A method for preparing a SiC-modified C / C composite material, comprising:
[0008] Pre-treating the C / C composite material to obtain a C / C preform for melt infiltration;
[0009] HfSi 2 With Si 3 N 4 The powders are mixed and dried to obtain powder for infiltration;
[0010] The C / C preform for infiltration is placed parallel to the upper layer of the infiltration powder, and the infiltration powder is continued to be added until the C / C preform for infiltration is completely covered and higher than the upper surface of the C / C preform for infiltration. After sealing, it is modified by a reaction infiltration process at high temperature to obtain C / C-HfC x N y -SiC composites;
[0011] For C / C-HfC x N y -SiC composite material is polished, cleaned and dried to obtain HfC x N y -SiC modified C / C composites.
[0012] Furthermore, the pretreatment includes grinding, cleaning, boiling and drying.
[0013] Furthermore, the boiling treatment temperature is 100 to 350° C., and the treatment time is 1 to 6 hours.
[0014] Furthermore, the drying treatment temperature is 70° C. and the treatment time is 6 to 10 hours.
[0015] Furthermore, the HfSi 2 With Si 3 N 4 The molar ratio of the powder is 1-4:1-4.
[0016] Furthermore, the HfSi 2 With Si 3 N 4 The powders are mixed by ball milling. During the ball milling process, the ball-to-material ratio is 2:1, the rotation speed is 200-500 rpm, and the ball milling time is 4-6 hours.
[0017] Furthermore, the drying temperature of the infiltration powder is 60-100° C., and the drying time is 8-12 hours.
[0018] Furthermore, the modification treatment conditions are: in the presence of Ar or N 2 In an inert atmosphere protection environment or a vacuum environment with a vacuum degree of 1 to 100 Pa, the temperature is 1600 to 2100°C, the heating rate is 4 to 10°C / min, and the insulation time is 0.5 to 3h.
[0019] Furthermore, the HfC x N y -The drying temperature of SiC modified C / C composite material is 60-100°C and the drying time is 6-12h.
[0020] HfC prepared by the preparation method x N y -SiC modified C / C composites.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention provides a HfC x N y -SiC modified C / C composite material preparation method, HfSi 2 and Si 3 N 4 The mixed powder is used as a melting agent to infiltrate HfC with ultra-high melting point, high hardness, certain toughness and ductility. x N yUsed for modification of C / C composite materials, where Si 3 N 4 Provide nitrogen source, the composite material prepared by reactive infiltration process has strong interface bonding. In addition, the introduction of SiC makes Hf(C, N) based composite materials attractive for different high temperature applications. 2 and Si 3 N 4 Molar ratio to control HfC x N y The relative content of components and SiC makes the tissue composition easy to control. The process of the present invention is simple and has low requirements on equipment. Compared with hafnium carbide, hafnium carbonitride has a higher melting point. Hafnium carbonitride ceramic-based composite materials have excellent anti-ablation properties in high-temperature oxygen-containing environments. And hafnium carbonitride has higher hardness, certain toughness and ductility. Compared with other ultra-high temperature ceramic matrices, it has strong anti-erosion properties in extreme aerodynamic heat and high-speed particle erosion environments. It can better improve the service life of materials in high heat flux density, high-pressure airflow and high-speed particle erosion environments, and extend the flight time of high-speed aircraft, which has great space strategic significance. At the same time, based on the present invention, HfC can also be designed more widely. x N y The preparation and performance improvement scheme of modified carbon / carbon composite materials, therefore, the development prospect of the present invention is very considerable, and the economic and social benefits are very outstanding. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0024] Figure 1 The HfC of the present invention x N y -Process flow chart of the preparation method of SiC modified C / C composite material.
[0025] Figure 2 HfC prepared in Example 1 of the present invention x N y -XRD pattern of SiC modified C / C composites.
[0026] Figure 3 HfC prepared in Example 1 of the present invention x N y -SEM image of SiC modified C / C composite. DETAILED DESCRIPTION
[0027] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0028] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0029] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0030] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0031] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0032] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0033] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0034] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0035] See also Figure 1 The present invention provides a HfC x N y -A method for preparing a SiC-modified C / C composite material comprises the following steps:
[0036] Step 1: Select 2.5DC / C composite material, process it into a block sample of 10mm×10mm×10mm, and polish it with 50 mesh, 800 mesh and 3000 mesh silicon carbide sandpaper in turn to ensure that the sample has no obvious defects during the reaction melt infiltration and the surface is regular and smooth. Use deionized water to ultrasonically clean the polished sample for 3 to 5 times, and each cleaning time is 30 to 60 minutes. Then, boil the block sample at 100 to 350°C for 1 to 6 hours until no bubbles emerge on the surface of the sample to ensure that the openings in the sample are fully opened. Then place the sample in an electric blast drying oven at a temperature of 70°C and dry it for 6 to 10 hours to obtain a C / C preform for melt infiltration.
[0037] Step 2: HfSi 2 With Si 3 N 4 The powders are mixed in a molar ratio of 1-4:1-4, and the powder mixture and zirconium oxide grinding balls are placed in a corundum ball mill with a ball-to-material ratio of 2:1. The corundum ball mill is then sealed and ball milled with a planetary ball mill at a rotation speed of 200-500 rpm. After ball milling for 4-6 hours, the powder is taken out and then placed in an electric heated blast drying oven at a temperature of 60-100°C for drying for 8-12 hours to obtain a uniformly mixed powder for infiltration.
[0038] Step 3: The C / C composite material is modified by a reactive infiltration process, 3 to 5 layers of graphite paper are laid on the inner wall of the graphite crucible, 4 to 10 mm thick infiltration powder is laid on the bottom of the crucible, and the C / C preform for infiltration is placed parallel to the upper layer of the infiltration powder, and the infiltration powder is continued to be added until the C / C preform for infiltration is completely covered and is 5 to 10 mm higher than the upper surface of the C / C preform for infiltration. During the addition of the infiltration powder, the infiltration powder is ensured to be in a loose state. After the addition of the infiltration powder is completed, it is sealed with graphite paper and carbon felt in turn, and then the crucible is sealed.
[0039] Step 4: Place the sealed crucible in a graphite furnace for high temperature treatment. The high temperature heat treatment conditions are: temperature of 1600-2100°C, vacuum degree of 1-100 Pa in the furnace, or in Ar or N 2 In an inert atmosphere, the heating rate is 4-10℃ / min, the holding time is 0.5-3h, and then the power is turned off to cool down. When the sample cools down to room temperature, it is taken out to obtain C / C-HfCx N y -SiC composite materials.
[0040] Step 5: C / C-HfC obtained after reaction infiltration x N y -SiC composite materials were polished with 50 mesh, 800 mesh and 3000 mesh diamond grinding discs in turn to ensure that there were no obvious protrusions on the surface. The samples were then ultrasonically cleaned with deionized water for 3 to 5 times, each time for 30 to 60 minutes, and then placed in an electric hot air drying oven for drying at 60 to 100 ° C for 6 to 12 hours to obtain HfC x N y -SiC modified C / C composites.
[0041] The present invention is further described in detail below in conjunction with specific embodiments:
[0042] Embodiment 1:
[0043] Step 1: Select a density of 1.1 g / cm 3 The 2.5DC / C composite material was processed into a block sample of 10mm×10mm×10mm, and then polished with 50 mesh, 800 mesh and 3000 mesh silicon carbide sandpaper in turn to ensure that the sample had no obvious defects during the reaction melt infiltration and the surface was regular and smooth. The polished sample was ultrasonically cleaned with deionized water for 5 times, each cleaning time was 30 minutes, and then the block sample was boiled at 300℃ for 3h until no bubbles emerged on the surface of the sample to ensure that the openings in the sample were fully opened, and then the sample was placed in an electric blast drying oven at a temperature of 70℃ for 8h for standby use.
[0044] Step 2: HfSi 2 With Si 3 N 4 The powders were mixed in a molar ratio of 4:1, and the powder mixture and zirconium oxide grinding balls were placed in a corundum ball mill with a ball-to-material ratio of 2:1. The corundum ball mill was then sealed and milled for 6 hours using a planetary ball mill at a rotation speed of 400 rpm. The mixture was sieved and then placed in an electric heated blast drying oven at a temperature of 70°C for drying for 8 hours to obtain a uniformly mixed powder mixture, which was used as powder for infiltration.
[0045] Step 3: The C / C composite material is modified by the reactive infiltration process. Five layers of graphite paper are laid on the inner wall of the graphite crucible, and 10 mm thick infiltration powder is laid on the bottom of the crucible. The porous C / C composite material is placed parallel to the upper layer of the infiltration powder. Powder is continued to be added until the sample is completely covered and 10 mm higher than the upper surface of the sample. During the powder addition process, the powder is ensured to be loose. After the powder is added, it is sealed with graphite paper and carbon felt in turn, and then the crucible is sealed.
[0046] Step 4: Place the sealed crucible in a graphite furnace for high temperature treatment. The high temperature heat treatment conditions are: temperature of 1700°C, pressure in the furnace of 10Pa, heating rate of 5°C / min, insulation time of 3h, followed by power off and cooling. Take out the sample after it cools to room temperature with the furnace.
[0047] Step 5: The composite material obtained after the reaction infiltration was polished with 50 mesh, 800 mesh and 3000 mesh diamond grinding discs in turn to ensure that there was no obvious protrusion on the sample surface. The sample was then ultrasonically cleaned with deionized water for 5 times, each cleaning time was 60 minutes, and then placed in an electric heating blast drying oven at 80°C for 10 hours to obtain HfC x N y -SiC modified C / C composites.
[0048] The prepared composite material was subjected to X-ray diffraction analysis, such as Figure 2 As shown in the figure, it is shown that high melting point hafnium carbonitride is generated during the infiltration process. The SEM image of the prepared composite material is analyzed, as shown in the figure. Figure 3 As shown, from Figure 3 It can be seen that a white HfC x N y phase and the gray SiC phase. Therefore, it can be judged that the HfC x N y -SiC modified C / C composites.
[0049] Embodiment 2:
[0050] Step 1: Select a density of 1.7 g / cm 3The C / C composite material was processed into a cubic block sample with a size of 10 mm, and then polished with 50 mesh, 800 mesh and 3000 mesh silicon carbide sandpaper in turn to ensure that the sample had no obvious defects during the reaction melt infiltration and the surface was regular and smooth. The polished sample was ultrasonically cleaned with deionized water for 3 times, each cleaning time was 60 minutes, and then the block sample was boiled at 350°C for 3 hours until no bubbles emerged on the surface of the sample to ensure that the openings in the sample were fully opened, and then the sample was placed in an electric blast drying oven at a temperature of 70°C for 6 hours for use.
[0051] Step 2: HfSi 2 With Si 3 N 4 The powders were mixed in a molar ratio of 4:1, and the powder mixture and zirconium oxide grinding balls were placed in a corundum ball mill with a ball-to-material ratio of 2:1. The corundum ball mill was then sealed and milled for 6 hours using a planetary ball mill at a rotation speed of 400 rpm. The mixture was sieved and then placed in an electric heated blast drying oven at a temperature of 70°C for drying for 8 hours to obtain a uniformly mixed powder mixture, which was used as powder for infiltration.
[0052] Step 3: When modifying the C / C composite material by the reactive infiltration process, lay 4 layers of graphite paper on the inner wall of the graphite crucible, lay 10 mm thick infiltration powder on the bottom of the crucible, and place the porous C / C composite material parallel to the upper layer of the infiltration powder. Continue to add powder until the sample is completely covered and 10 mm higher than the upper surface of the sample. During the powder addition process, ensure that the powder is in a loose state. After the powder is added, seal it with graphite paper and carbon felt in turn, and then seal the crucible.
[0053] Step 4: Place the sealed crucible in a graphite furnace for high-temperature treatment. The high-temperature heat treatment conditions are as follows: temperature of 1700°C, pressure in the furnace of 10Pa, heating rate of 5°C / min, and insulation time of 3h. Subsequently, the power is turned off and the temperature is lowered. After the sample cools to room temperature with the furnace, it is taken out to obtain a modified carbon-carbon composite material.
[0054] Step 5: The composite material obtained after the reaction infiltration was polished with 50 mesh, 800 mesh and 3000 mesh diamond grinding discs in turn to ensure that there was no obvious protrusion on the sample surface. The sample was then ultrasonically cleaned with deionized water for 5 times, each cleaning time was 30 minutes, and then placed in an electric heating blast drying oven at 80°C for 12 hours to obtain HfC x N y -SiC modified C / C composites.
[0055] Embodiment three:
[0056] Step 1: Select a density of 1.2 g / cm 3 The 2.5DC / C composite material was processed into a block sample of 10mm×10mm×10mm, and then polished with 50 mesh, 800 mesh and 3000 mesh silicon carbide sandpaper in turn to ensure that the sample had no obvious defects during the reaction melt infiltration and the surface was regular and smooth. The polished sample was ultrasonically cleaned with deionized water for 3 times, each cleaning time was 60 minutes, and then the block sample was boiled at 200℃ for 4 hours until no bubbles emerged on the surface of the sample to ensure that the openings in the sample were fully opened, and then the sample was placed in an electric blast drying oven at a temperature of 70℃ for 6 hours for use.
[0057] Step 2: HfSi 2 With Si 3 N 4 The powders were mixed in a molar ratio of 4:1, and the powder mixture and zirconium oxide grinding balls were placed in a corundum ball mill with a ball-to-material ratio of 2:1. The corundum ball mill was then sealed and milled for 4 hours using a planetary ball mill at a rotation speed of 400 rpm. The mixture was sieved and then placed in an electric heated blast drying oven at a temperature of 70°C for drying for 8 hours to obtain a uniformly mixed powder mixture, which was used as powder for infiltration.
[0058] Step 3: Use the reactive infiltration process to modify the matrix of the C / C composite material. Lay 5 layers of graphite paper on the inner wall of the graphite crucible, lay 6 mm thick infiltration powder on the bottom of the crucible, and place the porous C / C composite material parallel to the upper layer of the infiltration powder. Continue to add powder until the sample is completely covered and 8 mm higher than the upper surface of the sample. During the powder addition process, ensure that the powder is in a loose state. After the powder is added, seal it with graphite paper and carbon felt in turn, and then seal the crucible.
[0059] Step 4: Place the sealed crucible in a graphite furnace for high temperature treatment. The high temperature heat treatment conditions are as follows: temperature of 1900°C, Ar gas atmosphere in the furnace, heating rate of 10°C / min, holding time of 2h, followed by power off and cooling. The sample is taken out after cooling to room temperature with the furnace.
[0060] Step 5: The composite material obtained after the reaction infiltration was polished with 50 mesh, 800 mesh and 3000 mesh diamond grinding discs in turn to ensure that there was no obvious protrusion on the sample surface. The sample was then ultrasonically cleaned with deionized water for 5 times, each cleaning time was 30 minutes, and then placed in an electric heating blast drying oven at 80°C for 12 hours to obtain HfC x N y -SiC modified C / C composites.
[0061] Embodiment 4:
[0062] Step 1: Select a density of 1.7 g / cm 3 The 2.5DC / C composite material was processed into a block sample of 10mm×10mm×10mm, and then polished with 50 mesh, 800 mesh and 3000 mesh silicon carbide sandpaper to ensure that the sample had no obvious defects during the reaction melt infiltration and the surface was regular and smooth. The polished sample was ultrasonically cleaned with deionized water for 3 times, each time for 30 minutes. Subsequently, the block sample was boiled at 350℃ for 3h until no bubbles emerged on the surface of the sample to ensure that the openings in the sample were fully opened. Then the sample was placed in an electric blast drying oven at 70℃ for 8h for standby use.
[0063] Step 2: HfSi 2 With Si 3 N 4 The powders were mixed in a molar ratio of 4:1, and the powder mixture and zirconium oxide grinding balls were placed in a corundum ball mill with a ball-to-material ratio of 2:1. The corundum ball mill was then sealed and milled for 4 hours using a planetary ball mill at a rotation speed of 300 rpm. The mixture was sieved and then placed in an electric heated blast drying oven at a temperature of 70°C for drying for 10 hours to obtain a uniformly mixed powder mixture, which was used as powder for infiltration.
[0064] Step 3: Use the reactive infiltration process to modify the matrix of the C / C composite material. Spread 5 layers of graphite paper on the inner wall of the graphite crucible, spread 6 mm thick infiltration powder on the bottom of the crucible, and place the porous C / C composite material parallel to the upper layer of the infiltration powder. Continue to add powder until the sample is completely covered and 8 mm higher than the upper surface of the sample. During the powder addition process, ensure that the powder is in a loose state. After the powder is added, seal it with graphite paper and carbon powder in turn, and then seal the crucible.
[0065] Step 4: Place the sealed crucible in a graphite furnace for high-temperature treatment. The high-temperature heat treatment conditions are as follows: temperature of 1900°C, Ar gas atmosphere in the furnace, atmospheric pressure, heating rate of 4°C / min, holding time of 1h, followed by power off and cooling. The sample is taken out after cooling to room temperature with the furnace.
[0066] Step 5: The composite material obtained after the reaction infiltration was polished with 50 mesh, 800 mesh and 3000 mesh diamond grinding discs in turn to ensure that there was no obvious protrusion on the sample surface. The sample was then ultrasonically cleaned with deionized water for 5 times, each cleaning time was 40 minutes, and then placed in an electric heating blast drying oven at 80°C for 12 hours to obtain HfC x N y -SiC modified C / C composites.
[0067] Embodiment five:
[0068] Step 1: Select a density of 1.1 g / cm 3 The 2.5DC / C composite material was processed into a block sample of 10mm×10mm×10mm, and then polished with 50 mesh, 800 mesh and 3000 mesh silicon carbide sandpaper in turn to ensure that the sample had no obvious defects during the reaction melt infiltration and the surface was regular and smooth. The polished sample was ultrasonically cleaned with deionized water for 5 times, each time for 30 minutes. Subsequently, the block sample was boiled at 350℃ for 3h until no bubbles emerged on the surface of the sample to ensure that the openings in the sample were fully opened. Then the sample was placed in an electric blast drying oven at 80℃ for 8h for standby use.
[0069] Step 2: HfSi 2 With Si 3 N 4 The powders were mixed in a molar ratio of 4:1, and the powder mixture and zirconium oxide grinding balls were placed in a corundum ball mill with a ball-to-material ratio of 2:1. The corundum ball mill was then sealed and milled for 6 hours using a planetary ball mill at a rotation speed of 300 rpm. The mixture was sieved and then placed in an electric heated blast drying oven at a temperature of 70°C for drying for 10 hours to obtain a uniformly mixed powder mixture, which was used as powder for infiltration.
[0070] Step 3: Use the reactive infiltration process to modify the matrix of the C / C composite material. Lay 5 layers of graphite paper on the inner wall of the graphite crucible, lay 6 mm thick infiltration powder on the bottom of the crucible, and place the porous C / C composite material parallel to the upper layer of the infiltration powder. Continue to add powder until the sample is completely covered and 8 mm higher than the upper surface of the sample. During the powder addition process, ensure that the powder is in a loose state. After the powder is added, seal it with graphite paper and carbon felt in turn, and then seal the crucible.
[0071] Step 4: Place the sealed crucible in a graphite furnace for high temperature treatment. The high temperature heat treatment conditions are as follows: temperature of 2100°C, Ar gas atmosphere in the furnace, heating rate of 5°C / min, holding time of 1h, followed by power off and cooling. Wait for the sample to cool to room temperature before taking it out.
[0072] Step 5: The composite material obtained after the reaction infiltration was polished with 50 mesh, 800 mesh and 3000 mesh diamond grinding discs in turn to ensure that there was no obvious protrusion on the sample surface. The sample was then ultrasonically cleaned with deionized water for 5 times, each cleaning time was 30 minutes, and then placed in an electric heating blast drying oven at 80°C for 12 hours to obtain HfC x N y-SiC modified C / C composites.
[0073] Embodiment six:
[0074] Step 1: Select a density of 1.7 g / cm 3 The 2.5DC / C composite material was processed into a block sample of 10mm×10mm×10mm, and then polished with 50 mesh, 800 mesh and 3000 mesh silicon carbide sandpaper to ensure that the sample had no obvious defects during the reaction melt infiltration and the surface was regular and smooth. The polished sample was ultrasonically cleaned with deionized water for 3 times, each time for 60 minutes. Subsequently, the block sample was boiled at 300℃ for 3 hours until no bubbles emerged on the surface of the sample to ensure that the openings in the sample were fully opened. Then the sample was placed in an electric blast drying oven at 80℃ and dried for 8 hours for use.
[0075] Step 2: HfSi 2 With Si 3 N 4 The powders were mixed in a molar ratio of 1:1, and the powder mixture and zirconium oxide grinding balls were placed in a corundum ball mill with a ball-to-material ratio of 2:1. The corundum ball mill was then sealed and milled for 4 hours using a planetary ball mill at a rotation speed of 400 rpm. The mixture was sieved and then placed in an electric heated blast drying oven at a temperature of 70°C for drying for 10 hours to obtain a uniformly mixed powder mixture, which was used as powder for infiltration.
[0076] Step 3: Use the reactive infiltration process to modify the matrix of the C / C composite material. Lay 5 layers of graphite paper on the inner wall of the graphite crucible, lay 4 mm thick infiltration powder on the bottom of the crucible, and place the porous C / C composite material parallel to the upper layer of the infiltration powder. Continue to add powder until the sample is completely covered and 8 mm higher than the upper surface of the sample. During the powder addition process, ensure that the powder is in a loose state. After the powder is added, seal it with graphite paper and carbon felt in turn, and then seal the crucible.
[0077] Step 4: Place the sealed crucible in a graphite furnace for high temperature treatment. The high temperature heat treatment conditions are as follows: temperature of 2100°C, Ar gas atmosphere in the furnace, heating rate of 5°C / min, holding time of 1h, followed by power off and cooling. Wait for the sample to cool to room temperature before taking it out.
[0078] Step 5: The composite material obtained after the reaction infiltration was polished with 50 mesh, 800 mesh and 3000 mesh diamond grinding discs in turn to ensure that there was no obvious protrusion on the sample surface. The sample was then ultrasonically cleaned with deionized water for 3 times, each cleaning time was 60 minutes, and then placed in an electric heating blast drying oven at 80°C for 12 hours to obtain HfC xN y -SiC modified C / C composites.
[0079] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A HfC x N y - Preparation method of SiC modified C / C composite material, It is characterized in that include: Pre-treating the C / C composite material to obtain a C / C preform for melt infiltration; HfSi 2 With Si 3 N 4 The powders are mixed and dried to obtain powder for infiltration; The C / C preform for infiltration is placed parallel to the upper layer of the infiltration powder, and the infiltration powder is continued to be added until the C / C preform for infiltration is completely covered and higher than the upper surface of the C / C preform for infiltration. After sealing, it is modified by a reaction infiltration process at high temperature to obtain C / C-HfC x N y -SiC composites; For C / C-HfC x N y -SiC composite material is polished, cleaned and dried to obtain HfC x N y -SiC modified C / C composites.
2. A HfC according to claim 1 x N y - Preparation method of SiC modified C / C composite material, It is characterized in that The pretreatment includes grinding, cleaning, boiling and drying.
3. A HfC according to claim 2 x N y - Preparation method of SiC modified C / C composite material, It is characterized in that The boiling treatment temperature is 100-350° C., and the treatment time is 1-6 hours.
4. A HfC according to claim 2 x N y - Preparation method of SiC modified C / C composite material, It is characterized in that The drying treatment temperature is 70° C. and the treatment time is 6 to 10 hours.
5. A HfC according to claim 1 x N y - Preparation method of SiC modified C / C composite material, It is characterized in that The HfSi 2 With Si 3 N 4 The molar ratio of the powder is (1-4):(1-4).
6. A HfC according to claim 1 x N y - Preparation method of SiC modified C / C composite material, It is characterized in that The HfSi 2 With Si 3 N 4 The powders are mixed by ball milling. During the ball milling process, the ball-to-material ratio is 2:1, the rotation speed is 200-500 rpm, and the ball milling time is 4-6 hours.
7. A HfC according to claim 1 x N y - Preparation method of SiC modified C / C composite material, It is characterized in that The drying temperature of the powder for infiltration is 60-100° C., and the drying time is 8-12 hours.
8. A HfC according to claim 1 x N y - Preparation method of SiC modified C / C composite material, It is characterized in that The modification treatment conditions are: in the presence of Ar or N 2 In an inert atmosphere protection environment or a vacuum environment with a vacuum degree of 1 to 100 Pa, the temperature is 1600 to 2100°C, the heating rate is 4 to 10°C / min, and the insulation time is 0.5 to 3h.
9. A HfC according to claim 1 x N y - Preparation method of SiC modified C / C composite material, It is characterized in that The HfC x N y -The drying temperature of SiC modified C / C composite material is 60-100°C and the drying time is 6-12h.
10. HfC prepared by the preparation method according to any one of claims 1 to 9 x N y -SiC modified C / C composites.
Citation Information
Patent Citations
Continuous fiber reinforced ceramic matrix composite material and preparation method thereof
CN117567165A
Ultrahigh-temperature ceramic material based on reactive melt infiltration and preparation method thereof
CN117756534A
Application of chopped carbon fiber gradient toughened ultrahigh-melting-point ceramic matrix composite material
CN118005407A
Manufacturing method for pork cutlet sauce and pork cutlet sauce manufactured by the same
KR102302950B1
Substrate holding device