Alumina fiber reinforced quartz ceramic-based composite material and preparation method thereof

Through the surface modification of alumina fibers and the 2.5D warp and weft lining structural braid, combined with the gradient concentration impregnation and pressure curing process, the high-temperature strength and mechanical properties of quartz ceramic-based composite materials have been improved, and the problem of quartz ceramic-based composite materials at high temperatures has been solved. The problem of insufficient temperature resistance and mechanical properties in the environment meets the needs of wave-transparent radome/window materials for new generation aircraft.

CN118771900APending Publication Date: 2024-10-15THE RES INST FOR SPECIAL STRUCTURES OF AERONAUTICAL COMPOSITE AVIC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410935277.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Quartz ceramic matrix composite materials have insufficient temperature resistance and mechanical properties in high-temperature environments and cannot meet the requirements of 1200°C high temperature, high strength, and reusability, especially in the application of wave-transparent radome/window materials for new-generation hypersonic aircraft. .

Method used

The high-temperature self-healing ability of the composite material is enhanced by surface modification of alumina fiber. The 2.5D warp-insertion and weft-inlay structural braid and the gradient concentration vacuum impregnation and pressure curing process are used to improve the high-temperature strength and mechanical properties of the composite material and solve the thermal problem of the material. Stress matching and densification issues.

Benefits of technology

The high-temperature strength retention rate of alumina fiber-reinforced quartz ceramic matrix composites is ≥90%, the room temperature bending and tensile strength are significantly improved, and the dielectric properties are optimized to meet the high-temperature, high-strength, and reusable wave transmission requirements of 1200°C. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771900A_ABST
    Figure CN118771900A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of composite materials, and particularly relates to an alumina fiber reinforced quartz ceramic-based composite material and a preparation method thereof. Dipping alumina fibers into the aluminum-silicon-oxygen sol, and carrying out heat treatment to obtain an aluminum-silicon-oxygen coating; the alumina fibers are woven into a 2.5 D warp insertion and weft insertion structure woven body, the volume fraction of reinforcement fibers is 35-55%, and the thickness of the woven body is 3-20 mm; after the alumina fiber woven body is heated, silica sol is injected into a container to be fully impregnated into the 2.5 D warp insertion weft insertion structure alumina woven body with the transition interface layer, the silica sol is cured and dried, silica sol particles rapidly construct a gel three-dimensional network, and the alumina fiber woven body with the 2.5 D warp insertion weft insertion structure is obtained. After moisture is fully volatilized, obtaining an unsintered 2.5 D warp insertion weft insertion structure alumina fiber reinforced quartz ceramic-based composite material green body; then sintering in vacuum at the temperature of 800-1000 DEG C, and keeping the temperature for 30-120 minutes to obtain a semi-finished product of the alumina fiber reinforced quartz ceramic-based composite material with the 2.5 D warp insertion and weft insertion structure; and repeating the steps for 1-3 times, and when the weight increment of the composite material is less than or equal to 4%, obtaining a finished product of the alumina fiber reinforced quartz ceramic-based composite material with the 2.5 D warp insertion and weft insertion structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of composite materials, and in particular relates to a preparation process for a high-strength, high-temperature-resistant, heat-oxidation-resistant, reusable ceramic composite material suitable for wave-transmitting antenna cover / window materials. Background Art

[0002] The wave-transmitting radome / window materials mainly include fiber-reinforced resin-based composite materials, single-phase / complex-phase ceramic materials such as quartz ceramics, alumina ceramics, microcrystalline glass, nitride ceramics, and fiber-reinforced ceramic-based composite materials. Fiber-reinforced resin-based composite materials have been widely used in low Mach number (<4Ma) missile radomes, but their heat resistance is poor and they are easily cracked to form free carbon (>500℃) at high temperatures, which can no longer meet the heat protection and wave transmission requirements of high Mach number missiles during flight. Quartz ceramics have excellent dielectric properties (dielectric constant ≈3.4 at room temperature, dielectric loss ≈4×10 -4 ), good high temperature dielectric stability (from room temperature to 1473K, dielectric constant change rate ≤ 2%), and excellent thermal shock resistance (thermal expansion coefficient ≈ 5.4×10 -7 / k), has been widely used in aircraft with Mach number (Ma) ≤ 5. With the further increase in aircraft flight speed and flight time, single-phase or multi-phase ceramic materials are still brittle materials in nature, with insufficient bearing capacity, and have disadvantages such as difficulty in forming large-size components and poor machinability, which limits their further application. Continuous fiber reinforced ceramic matrix composites, while maintaining the advantages of single-phase / multi-phase ceramics such as high temperature resistance, low dielectric constant, and corrosion resistance, overcome the disadvantage of insufficient toughness of ceramic materials, have high application reliability, and have become the main choice for antenna cover materials under high thermal conditions. In recent years, due to the limited source of alumina fibers, domestic research on continuous fiber reinforced ceramic matrix composites has mainly focused on quartz fiber reinforced quartz ceramic matrix composite systems.

[0003] Quartz fiber reinforced quartz ceramic matrix composites use silica sol to impregnate fiber preforms, prepare the matrix through drying, sintering and other processes, and then perform multiple impregnation-drying-sintering to finally obtain a dense composite material. Silica sol is widely available and relatively low in cost; silica sol has low drying and sintering temperatures, and causes less thermal damage to oxide fibers; at the same time, the sol-gel process can be used to prepare components of complex shapes and achieve near-size molding. However, quartz fiber will undergo obvious crystallization when heat treated above 1150°C, and the glass phase will transform into the quartz phase. The volume effect produced by the precipitation of the new phase causes the fiber strength to decrease rapidly; in addition, quartz fiber has high activity and low modulus. It is easy to diffuse with the ceramic matrix under high temperature conditions to form a strong interface bond, resulting in matrix cracks penetrating the fiber, and the fiber cannot play a toughening and reinforcing role, and the mechanical properties of the composite material are poor. Therefore, quartz fiber reinforced quartz ceramic-based composite materials are difficult to use for a long time or repeatedly at temperatures above 1000°C, and cannot meet the requirements of the new generation of hypersonic aircraft for high-temperature resistance of 1200°C, high strength, reusability, and heat-oxidation-resistant and wave-transparent antenna cover / window materials. Summary of the invention

[0004] Purpose of the invention: In view of the current situation that the temperature resistance and mechanical properties of quartz ceramic-based composite materials are insufficient and cannot meet the needs of long-term and reusable use in a high-temperature oxidation environment of 1200°C, (1) the present invention improves the high-temperature self-healing ability of alumina fibers through surface modification of alumina fibers, improves the thermal stress matching between the reinforcement and the matrix, and improves the high-temperature strength retention rate of the composite material, thereby solving the current situation of insufficient temperature resistance of quartz ceramic-based composite materials; (2) by increasing the consistency of the mechanical properties of the warp and weft directions of the braided body, the tensile strength and compressive strength of the composite material are effectively improved, thereby solving the current situation of insufficient mechanical properties of quartz ceramic-based composite materials; (3) by gradient concentration and pressurized impregnation curing, the short-cycle rapid densification of the silicon oxide matrix is ​​achieved, thereby solving the current situation of long cycle and high cost of the sol-gel process of quartz ceramic composite materials. It is used to meet the requirements of the new generation of aircraft for the use of 1200°C high-temperature resistant, high-strength, reusable, heat-resistant oxidation-resistant wave-transparent antenna cover / window materials.

[0005] Technical solution: In order to overcome the deficiencies of existing technologies and materials, the present invention provides a high-strength alumina fiber reinforced quartz ceramic matrix composite material and a preparation method thereof.

[0006] The present invention is achieved through the following technical solutions:

[0007] A preparation method of a high-strength alumina fiber reinforced quartz ceramic matrix composite material mainly includes fiber transition interface coating impregnation, drying, heat treatment, fiber weaving, sol impregnation, pressurized curing, sintering and the like.

[0008] (1) preparing a fiber transition interface coating: dipping alumina fiber into an aluminum-silicon-oxygen sol, drying at 60°C to 120°C, winding into a roll, and heat treating at 600°C to 1000°C to obtain an aluminum-silicon-oxygen coating;

[0009] (2) Preparation of alumina fiber braid: alumina fiber is treated with a sizing agent and woven into a 2.5D warp-lined and weft-lined braid, the volume fraction of the reinforcement fiber is 35% to 55%, and the braid thickness is 3 mm to 20 mm;

[0010] (3) Sol impregnation and pressurized curing: After the alumina fiber braid is heat treated at 500°C for 30 min to 60 min, vacuum is drawn for 10 min to 30 min, and silica sol is injected into a container and fully impregnated into the 2.5D warp and weft lining structure alumina braid with a transition interface layer. The silica sol is cured and dried, and the silica sol particles quickly construct a gel three-dimensional network. After the water is fully volatilized, an unsintered 2.5D warp and weft lining structure alumina fiber reinforced quartz ceramic matrix composite material blank is obtained;

[0011] (4) Sintering: The alumina fiber reinforced quartz ceramic matrix composite material green body is placed in a sintering furnace and sintered at 800°C to 1000°C under vacuum for 30 min to 120 min to obtain a 2.5D warp and weft lining structure alumina fiber reinforced quartz ceramic matrix composite material semi-finished product;

[0012] (5) Impregnation, curing and sintering process cycle weight gain: repeat steps (3) and (4) for 1 to 3 times. When the weight gain of the composite material is ≤4%, a 2.5D warp and weft lined alumina fiber reinforced quartz ceramic matrix composite product is obtained.

[0013] Furthermore, in the step (1), the concentration of the aluminum-silicon-oxygen sol is 10% to 30%, the fiber dipping time is 1 min to 5 min, the dipping times are 1 to 3 times, and too much transition interface coating is not conducive to the subsequent preparation of the fiber braid.

[0014] Furthermore, in step (2), the fineness of the warp yarn, weft yarn, lining warp yarn and lining weft yarn of the 2.5D warp-lined and weft-lined alumina fiber braided body is between 200tex×1 and 200tex×3, and the density of the warp yarn, weft yarn, lining warp yarn and lining weft yarn is between 2.5 yarns / cm and 6.5 yarns / cm.

[0015] Furthermore, in step (3), the silica sol is cured by vacuum impregnation under pressure at a gradient concentration of 20% to 40%, and the gel-curing system is 90°C for 120 min to 600 min, 120°C for 60 min to 180 min, and 200°C for 30 min to 120 min.

[0016] Furthermore, in step (4), the sintering furnace is a muffle furnace or a vacuum molybdenum wire sintering furnace, and the sintering atmosphere is a vacuum environment or an air atmosphere.

[0017] Furthermore, the alumina fiber braid adopts a 2.5D warp and weft structure, the fineness of the warp, weft, warp and weft yarns of the braid is between 200tex×1 and 200tex×3, the density of the warp, weft, warp and weft yarns is between 2.5 and 6.5 strands / cm, and the volume fraction of the reinforcement fiber is 35% to 55%. It can achieve consistent mechanical properties in the warp and weft directions, and the strength is significantly higher than that of the ordinary 2.5D structure.

[0018] Furthermore, the fiber-matrix transition interface coating is an aluminum-silicon-oxygen coating, the aluminum-silicon-oxygen sol concentration is 10% to 30%, the fiber immersion time is 1min to 5min, and the immersion times are 1 to 3 times, which can significantly improve the high temperature mechanical properties.

[0019] Furthermore, the quartz substrate is vacuum impregnated and pressurized to solidify with silica sol gradient concentration, the silica sol concentration is 20% to 40%, the gel-curing system is 90°C curing for 120min to 600min, 120°C curing for 60min to 180min, and 200°C curing for 30min to 120min.

[0020] Beneficial technical effects: The present invention uses several key technologies such as new high-performance domestic alumina fiber prepared through transition interface coating, new 2.5D warp and weft structure weaving, gradient concentration vacuum impregnation, pressurized curing and sintering. The preparation process cycle is only 1 to 3 times, the preparation process is simple, the cycle is short, and the equipment requirements are low. The density of the prepared 2.5D warp and weft structure alumina fiber reinforced quartz ceramic matrix composite material is 1.7g / cm 3 ~2.5g / cm 3 , room temperature bending strength is 170MPa-260MPa, room temperature tensile strength is 120MPa-170MPa, 1200℃ strength retention rate is ≥90%, room temperature dielectric constant is between 3.0 and 3.8, and dielectric loss is ≤0.007. The present invention is used to meet the requirements of a new generation of aircraft for 1200℃ high temperature resistance, high strength, reusability, heat-resistant oxidation-resistant wave-transparent antenna cover / window materials, and has extremely high application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Preparation flow chart of alumina fiber reinforced quartz-based ceramic composites;

[0022] Figure 2 Schematic diagram of 2.5D warp and weft structured alumina fiber braided body. DETAILED DESCRIPTION

[0023] The present invention is further described below in conjunction with implementation cases, which are only some implementation cases or certain specific implementation forms of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0024] See attached Figure 1 , 2 The present invention specifically proposes a method for preparing an alumina fiber reinforced quartz ceramic matrix composite material, comprising the following steps:

[0025] The first step is to prepare the fiber transition interface coating: the alumina fiber is immersed in aluminum-silicon-oxygen sol, dried in an oven at 60°C to 120°C, wound into a roll, and heat treated at 600°C to 1000°C in a muffle furnace to obtain an aluminum-silicon-oxygen coating.

[0026] The second step is to prepare an alumina fiber braid: the alumina fiber is treated with a sizing agent and woven into a 2.5D warp and weft structure braid, the volume fraction of the reinforcement fiber is 35% to 55%, and the braid thickness is 3mm to 20mm.

[0027] The third step is sol impregnation and pressurized curing: the alumina fiber braid is heat treated at 500°C in a muffle furnace for 30min to 60min, and then placed in a vacuum container and evacuated for 10min to 30min. The silica sol is injected into the container and fully impregnated into the 2.5D warp and weft lined alumina braid with a transition interface layer. The silica sol is cured and dried, and the silica sol particles quickly construct a gel three-dimensional network. After the water is fully evaporated, an unsintered 2.5D warp and weft lined alumina fiber reinforced quartz ceramic-based composite material blank is obtained.

[0028] The fourth step is sintering: the alumina fiber reinforced quartz ceramic matrix composite material green body is placed in a sintering furnace and sintered at 800°C to 1000°C in vacuum for 30min to 120min to obtain a 2.5D warp and weft lining structure alumina fiber reinforced quartz ceramic matrix composite material semi-finished product.

[0029] The fifth step is to increase weight through the impregnation, curing and sintering process cycle: repeat the third and fourth steps 1 to 3 times, at which time the weight gain of the composite material is ≤4%, and a 2.5D warp and weft lining structure alumina fiber reinforced quartz ceramic matrix composite product is obtained.

[0030] Example 1

[0031] Aluminum-silicon-oxygen sol with a concentration of 25% was selected to prepare the fiber transition interface coating. The fiber was impregnated for 3 minutes, impregnated twice, and then wound into a roll after drying. The aluminum-silicon-oxygen coating was obtained by heat treatment at 600°C in a muffle furnace. The alumina fiber was treated with a sizing agent and woven into a 2.5D warp-lined and weft-lined structure braid. The density of the braided warp, weft, warp-lined and weft-lined yarns was 6.5 strands / cm, the volume fraction of the reinforcement fiber was 55%, and the braid thickness was 6mm. The alumina fiber braid was heat treated in a muffle furnace to remove the impregnant and then placed in a vacuum container for 30 minutes. 40% silica sol was injected into the container and fully impregnated into the 2.5D warp-lined and weft-lined alumina braid with a transition interface layer. The silica sol gel-curing system was 90°C for 300 minutes, 120°C for 90 minutes, and 200°C for 60 minutes. The alumina fiber reinforced quartz ceramic matrix composite body was placed in a vacuum molybdenum wire sintering furnace and kept at 900℃ for 90 minutes. The impregnation curing and sintering process was repeated once, and a 30% concentration of silica sol was used for the second impregnation to obtain a 2.5D warp and weft structure alumina fiber reinforced quartz ceramic matrix composite material. The density of the composite flat sample is 2.3g / cm 3 ~2.5g / cm 3 The room temperature flexural strength is 185MPa~220MPa, the room temperature tensile strength is 150MPa~170MPa, the 1200℃ strength retention rate is ≥90%, the room temperature dielectric constant is 3.5~3.7, and the dielectric loss is ≤0.007.

[0032] Example 2

[0033] Aluminum-silicon-oxygen sol with a concentration of 15% was selected to prepare the fiber transition interface coating. The fiber was impregnated for 5 minutes, impregnated 3 times, and then wound into a roll after drying. The aluminum-silicon-oxygen coating was obtained by heat treatment at 800℃ in a muffle furnace. The alumina fiber was treated with a sizing agent and woven into a 2.5D warp-lined and weft-lined structure braid. The density of the braided warp, weft, warp-lined and weft-lined yarns was 5.5 pieces / cm, the volume fraction of the reinforcement fiber was 45%, and the braid thickness was 15mm. The alumina fiber braid was heat treated in a muffle furnace to remove the impregnant and then placed in a vacuum container for 30 minutes. 35% silica sol was injected into the container and fully impregnated into the 2.5D warp-lined and weft-lined alumina braid with a transition interface layer. The silica sol gel-curing system was 90℃ for 480 minutes, 120℃ for 120 minutes, and 200℃ for 90 minutes. The alumina fiber reinforced quartz ceramic matrix composite body was placed in a vacuum molybdenum wire sintering furnace and kept at 1000℃ for 60min. The impregnation curing and sintering process was repeated twice. The second process used 30% silica sol concentration, and the third process used 30% silica sol concentration to obtain a 2.5D warp and weft structure alumina fiber reinforced quartz ceramic matrix composite material. The density of the composite flat sample is 2.1g / cm3 ~2.3g / cm 3 The room temperature flexural strength is 210MPa~240MPa, the room temperature tensile strength is 130MPa~155MPa, the 1200℃ strength retention rate is ≥90%, the room temperature dielectric constant is 3.3~3.5, and the dielectric loss is ≤0.007.

[0034] (1) The present invention uses high-temperature resistant and oxidation-resistant alumina fiber as a reinforcing material, and prepares a transition interface layer on the surface of the alumina fiber through an impregnation-coating-sintering process to repair the surface microcracks of the alumina fiber generated in a high-temperature environment, while improving the thermal stress matching problem between the fiber and the matrix, thereby improving the high-temperature strength retention rate of the quartz-based composite material.

[0035] (2) Alumina fiber braids are prepared as reinforcements for composite materials using a 2.5D warp and weft weaving process. The 2.5D warp and weft braids are formed by interweaving the warp yarns at a certain angle along the thickness direction. They have good resistance to delamination and interlaminar fracture toughness and are suitable for curved components such as antenna covers. By increasing the consistency of the warp and weft mechanical properties of the braid in the warp and weft directions, the tensile strength, bending strength, and compressive strength of quartz-based composite materials can be effectively improved.

[0036] (3) The sol-gel process is used to achieve short-term rapid densification of the quartz matrix through gradient concentration and pressure impregnation curing, thereby obtaining a low-cost, high-strength quartz matrix.

[0037] Those skilled in the art will appreciate that, unless otherwise specifically defined, all technical terms used above have the same meanings as those generally understood by ordinary technicians in the field to which the present invention belongs; all the above specific implementation methods and specific cases further illustrate the purpose, technical solutions and beneficial technical effects of the present invention in detail. It should also be understood that the above description is only some specific implementation methods and cases of the present invention, and is not intended to limit the present invention. On the contrary, any other modifications, equivalent substitutions, improvements, etc. made within the design ideas and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a high-strength alumina fiber reinforced quartz ceramic matrix composite material, characterized in that: The following steps are involved: (1) preparing a fiber transition interface coating: dipping alumina fiber into an aluminum-silicon-oxygen sol, drying at 60°C to 120°C, winding into a roll, and heat treating at 600°C to 1000°C to obtain an aluminum-silicon-oxygen coating; (2) Preparation of alumina fiber braid: alumina fiber is treated with a sizing agent and woven into a 2.5D warp-lined and weft-lined braid, the volume fraction of the reinforcement fiber is 35% to 55%, and the braid thickness is 3 mm to 20 mm; (3) Sol impregnation and pressurized curing: After the alumina fiber braid is heat treated at 500°C for 30 min to 60 min, vacuum is drawn for 10 min to 30 min, and silica sol is injected into a container and fully impregnated into the 2.5D warp and weft lining structure alumina braid with a transition interface layer. The silica sol is cured and dried, and the silica sol particles quickly construct a gel three-dimensional network. After the water is fully volatilized, an unsintered 2.5D warp and weft lining structure alumina fiber reinforced quartz ceramic matrix composite material blank is obtained; (4) Sintering: The alumina fiber reinforced quartz ceramic matrix composite material green body is placed in a sintering furnace and sintered at 800°C to 1000°C under vacuum for 30 min to 120 min to obtain a 2.5D warp and weft lining structure alumina fiber reinforced quartz ceramic matrix composite material semi-finished product; (5) Impregnation, curing and sintering process cycle weight gain: repeat steps (3) and (4) for 1 to 3 times. When the weight gain of the composite material is ≤4%, a 2.5D warp and weft lined alumina fiber reinforced quartz ceramic matrix composite product is obtained.

2. The method for preparing a high-strength alumina fiber reinforced quartz ceramic matrix composite material according to claim 1, characterized in that: In the step (1), the concentration of the aluminum-silicon-oxygen sol is 10% to 30%, the fiber dipping time is 1 min to 5 min, and the dipping times are 1 to 3 times. Too much transition interface coating is not conducive to the subsequent preparation of the fiber braid.

3. The method for preparing a high-strength alumina fiber reinforced quartz ceramic matrix composite material according to claim 1, characterized in that: In step (2), the fineness of the warp yarn, weft yarn, lining warp yarn and lining weft yarn of the 2.5D warp-lined and weft-lined alumina fiber braided body is between 200tex×1 and 200tex×3, and the density of the warp yarn, weft yarn, lining warp yarn and lining weft yarn is between 2.5 yarns / cm and 6.5 yarns / cm.

4. The method for preparing a high-strength alumina fiber reinforced quartz ceramic matrix composite material according to claim 1, characterized in that: In step (3), the silica sol is cured by vacuum impregnation under pressure at a gradient concentration of 20% to 40%, and the gel-curing system is 90°C for 120min to 600min, 120°C for 60min to 180min, and 200°C for 30min to 120min.

5. The method for preparing a high-strength alumina fiber reinforced quartz ceramic matrix composite material according to claim 1, characterized in that: In step (4), the sintering furnace is a muffle furnace or a vacuum molybdenum wire sintering furnace, and the sintering atmosphere is a vacuum environment or an air atmosphere.

6. The method for preparing a high-strength alumina fiber reinforced quartz ceramic matrix composite material according to claim 1, characterized in that: The alumina fiber braid adopts 2.5D warp and weft structure, the fineness of the warp, weft, warp and weft yarns of the braid is between 200tex×1 and 200tex×3, the density of the warp, weft, warp and weft yarns is between 2.5 and 6.5 strands / cm, and the volume fraction of the reinforcement fiber is 35% to 55%. It can achieve consistent mechanical properties in the warp and weft directions, and the strength is significantly higher than that of the ordinary 2.5D structure.

7. The method for preparing a high-strength alumina fiber reinforced quartz ceramic matrix composite material according to claim 1, characterized in that: The fiber-matrix transition interface coating uses aluminum-silicon-oxygen coating, the aluminum-silicon-oxygen sol concentration is 10% to 30%, the fiber dipping time is 1min to 5min, and the dipping times are 1 to 3 times.

8. The method for preparing a high-strength alumina fiber reinforced quartz ceramic matrix composite material according to claim 1, characterized in that: The quartz matrix is ​​vacuum impregnated with silica sol gradient concentration and pressurized solidified. The silica sol concentration is 20% to 40%. The gel-solidification system is 90° C. solidified for 120 min to 600 min, 120° C. solidified for 60 min to 180 min, and 200° C. solidified for 30 min to 120 min.

Citation Information

Patent Citations

  • Silicon nitride fiber reinforced ceramic matrix composite material and preparation method thereof

    CN113698219A

  • High-density fiber-reinforced quartz ceramic composite material and preparation method thereof

    CN113896554A

  • Preparation method of high-performance alumina fiber ceramic-based composite material

    CN113956058A

  • Carbon fiber warp-inserted weft-inserted weft-knitted tubular fabric

    CN213739902U