Preparation method of optical-grade polymethyl methacrylate
By using a single-component rare earth complex catalyst, the problem of insufficient catalytic efficiency and selectivity of polymethyl methacrylate in the existing technology is solved, and polymethyl methacrylate with high transmittance and narrow molecular weight distribution is achieved, meeting the requirements meet the demand for high-end optical materials.
Patent Information
- Application Number
- CN202411118511.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-08-15
AI Technical Summary
Existing technology is difficult to catalyze polymethylmethacrylate efficiently and selectively, resulting in the generated polymer having low molecular weight, wide molecular weight distribution, and insufficient light transmittance, making it unable to meet the needs of high-end optical materials.
A single-component rare earth complex is used as a catalyst, including a rare earth metal compound with a large sterically hindered ligand, to achieve efficient and highly selective polymerization of methyl methacrylate through specific reaction steps and conditions, including mixing with CaH2 at room temperature. , evaporate under low temperature and reduced pressure, catalyze in an anhydrous and oxygen-free environment, use rare earth metals such as scandium, yttrium and lanthanide elements, and the ligands are hydrocarbon groups, benzylamino or aryl groups, etc., control the reaction time and molar ratio, and screen out Catalyst with high yield and high transmittance.
It achieves the high light transmittance of polymethyl methacrylate, narrow molecular weight distribution, high stereoselectivity, and light transmittance of up to 93%-94%. It is suitable for high-end optical materials, simplifies the process flow, and improves yield and Selectivity.
Smart Images

Figure CN118772318A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polar olefin polymerization, and particularly relates to a method for preparing optical-grade polymethyl methacrylate. Background Art
[0002] In recent years, the integration of polymer science and organometallic chemistry has achieved amazing success. Some progress has also been made in the polymerization of polar monomers such as methyl methacrylate using electron-deficient, highly active metallocenes and related single-site metal catalysts. Fifty years ago, conventional Ziegler-Natta type catalysts including TiCl4 / AlR3 and Cp2TiCl2 / AlEt3 had been used for the specific polymerization of methyl methacrylate (MMA), although the active species, polymerization mechanism and degree of polymerization control were not clear. In 1972, Ballard and Van Lienden reported the polymerization of MMA in toluene by coordinating anions using metal tetrabenzyl complexes such as Zr(CH2Ph)4. In 1988, Farnham and Hertler reported in a U.S. patent the polymerization of discrete chloro-metallocene enol esters, Cp2MCl[OC(OMe)=CMe2] (Cp is η 5 -cyclopentadiene, M is Ti, Zr, Hf), catalyzes the polymerization of MMA, however, the activity and polymerization yield of the system are very low, in THF, the polymerization at room temperature for 18 hours, only 20% yield ([MMA] / [Zr] = 20). The resulting polymethyl methacrylate (PMMA) has a low molecular weight (MW) and a wide molecular weight distribution (PDI>2). In 1992, Yasuda and his co-workers published the use of discrete metallocene complexes including neutral, single-component lanthanide metallocene complexes, such as dimer [Cp2SmH]2, which pioneered the study of controlled / living polymerization of acrylic monomers.
[0003] Optical-grade PMMA, that is, a high-molecular polymer with extremely high stereoregularity and high purity in its molecular structure, has a higher light transmittance than ordinary-grade PMMA. The light transmittance of ordinary optical-grade PMMA is 92%, and the current highest-grade optical-grade PMMA has a light transmittance of 96%. In addition, optical-grade PMMA has better electrical insulation, chemical resistance, solvent resistance, and heat and cold resistance. After post-processing, it can be applied to high-end equipment such as liquid crystal light guide plate films, LED lamps, optical fiber materials, and optical products. With the rapid development of markets such as liquid crystal displays, LED displays, and automobiles, the demand for high-grade optical-grade PMMA is also increasing rapidly. Based on the current research status of optical-grade polymethyl methacrylate materials, the core problem and difficulty is the development of efficient and highly selective catalytic systems. Summary of the invention
[0004] The purpose of the invention is to provide a method for producing optical grade polymethyl methacrylate (PMMA) with high efficiency and selectivity.
[0005] The present invention first provides a catalyst for producing optical grade polymethyl methacrylate, which is a single-component rare earth complex (containing a rare earth metal compound with a large steric hindrance ligand), and its structure is shown in the following formula 1:
[0006]
[0007] The ligand R group can be a hydrocarbon group ((CH2) n(n=2~6) ), dibenzylamino ((C6H5CH2)2N), aryl (such as phenyl, substituted phenyl, etc.), rare earth metal (Ln) is scandium (Sc), yttrium (Y) and all lanthanide elements (such as lanthanum (La), neodymium (Nd), samarium (Sm), lutetium (Lu), etc.).
[0008] Preferably, the rare earth metal is Lu or Sc; the ligand substituent is R=(C6H5CH2)2N or R=p-OMe-Ph.
[0009] The method for producing optical grade polymethyl methacrylate provided by the present invention uses the above-mentioned single-component rare earth complex as a catalyst, and the specific steps of production are as follows:
[0010] (1) Drying monomers and solvents:
[0011] Methyl methacrylate is mixed with CaH2 at room temperature, stirred for 16-24 hours, evaporated under reduced pressure, degassed three times to remove oxygen; then stored at low temperature (-35°C) under anhydrous and oxygen-free conditions; after the solvent is purified, soaked in sodium tablets and placed in a glove box for later use;
[0012] (2) Solution polymerization of methyl methacrylate:
[0013] Under room temperature, in an anhydrous and oxygen-free environment (in a glove box), take 0.01-10 mmol of the catalyst, put it into an eggplant-shaped bottle, add 1-1000 mL of solvent to dissolve it, and then weigh 0.2-1000 g of methyl methacrylate and add it; react for 1-12 hours; then inject 1-20 mL of ethanol containing a small amount of concentrated hydrochloric acid into the system to quench the reaction; after 5-20 minutes, slowly add 5-5000 mL of ethanol until the solid is completely precipitated; the obtained solid is placed in a vacuum drying oven and dried at 40-70° C. to constant weight;
[0014] (3) Purification of polymethyl methacrylate:
[0015] Take 2-20 g of polymethyl methacrylate after constant weight and dissolve it in 5-50 mL of THF, then add 20-200 mL of ethanol to precipitate it, repeat several times, and place it in a vacuum drying oven to dry to constant weight.
[0016] The polymerization solvent is selected from toluene and chlorobenzene.
[0017] Polymethyl methacrylate light transmittance test:
[0018] Weigh 2-10g of purified polymethyl methacrylate, add 5-50ml of THF and stir to dissolve, place in an ultrasonic cleaner for 10-30min to drive away the bubbles in the solution, then pour the solution into a grooved glass container, place in a fume hood for 2-4 days, and dry naturally. Cut a suitable shape and place it in a cuvette. Before the transmittance test, place two sets of blank cuvettes for a blank test. Then place the PMMA sample film in a cuvette for a transmittance test.
[0019] The molecular weight of the polymer was determined by gel permeation chromatography (GPC, Waters 410 1515_2707_2414 system). The meso-tactic, isotactic and atactic stereoselectivities of the polymer were calculated from the nuclear magnetic resonance spectrum.
[0020] The results show that the product stereoselectivity and syndiotactic selectivity content are between 40% and 90%, the product molecular weight is between 60000 and 120000, and the molecular weight distribution is between 1.4 and 1.7. After the polymethyl methacrylate is purified, the transmittance can reach 93%, and the transmittance in some wavelength ranges can reach 94%.
[0021] Furthermore, the present invention screens out a catalyst with high polymethyl methacrylate yield and optimal light transmittance from catalysts of various structures of single-component rare earth complexes by controlling the reaction time and the molar ratio of the monomer to the catalyst.
[0022] The results show that when the rare earth metal is Lu or Sc and the ligand substituent is R = (C6H5CH2)2N or R = p-OMe-Ph, the yield of the prepared polymethyl methacrylate is the highest and the transmittance is the best, as shown in Table 1 below:
[0023] Table 1, yield, stereostructure information and activity results of polymethyl methacrylate obtained using different catalysts:
[0024]
[0025] in:
[0026] 1-Sc catalyst, the R group on the ligand is phenyl and the central metal is Sc;
[0027] 2-Sc catalyst, the R group on the ligand is p-methoxyphenyl, and the central metal is Sc;
[0028] 3-Lu catalyst, the R group on the ligand is dibenzylamino, and the central metal is Lu;
[0029] 3-Sc catalyst, the R group on the ligand is dibenzylamino, and the central metal is Sc.
[0030] As can be seen from Table 1, the catalysts with the highest catalytic activity and better polymethyl methacrylate stereomicrostructure are 1-Sc, 2-Sc, 3-Lu, and 3-Sc.
[0031] The present invention uses a rare earth metal compound containing a large sterically hindered ligand as a catalyst for efficiently and highly selectively producing optical-grade PMMA. The present invention uses only one catalyst precursor and does not require the addition of an additional catalyst promoter. Polymethyl methacrylate can be obtained efficiently and highly selectively at room temperature. Optical-grade PMMA can be obtained after purification. In the laboratory, 100 grams of optical-grade PMMA can be obtained, which has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is the GPC spectrum of the product described in Example 1.
[0033] Figure 2 The UV-visible spectra of the products obtained after different times of purification of the product described in Example 1 are shown.
[0034] Figure 3 This is the GPC spectrum of the product described in Example 2.
[0035] Figure 4 This is the GPC spectrum of the product described in Example 3. DETAILED DESCRIPTION
[0036] The present invention is further described below through specific embodiments.
[0037] Example 1: Weigh 0.0078g (0.01mmol) of complex 2-Sc in a 25mL reaction tube, dissolve it with 2mL toluene, and then weigh 0.200g (2.0mmol) of methyl methacrylate and add it, start stirring, and react for 12 hours. After the reaction is completed, slowly add ethanol under stirring until the solid is completely precipitated. Pour off the liquid, and the obtained polymethyl methacrylate is a white solid. Dry to constant weight at 60°C in a vacuum drying oven, and the net yield of the blend is about 200mg, and the conversion rate is about 100%. After dissolving the blend by gel chromatography, a single peak can be obtained, and its molecular weight is: 85,000, and the molecular weight distribution is: 1.74. Using nuclear magnetic resonance hydrogen spectrum analysis, the content of the syndiotactic component is 81.0%. After the sample is purified six times, the transmittance is measured to be more than 93%, and some bands reach 94%.
[0038] Example 2, weigh 0.0084g (0.01mmol) of complex 3-Lu in a 25mL reaction tube, dissolve it with 2mL of toluene, weigh 0.200g (2.0mmol) of methyl methacrylate and add it, and start stirring. React for 12 hours. After the reaction is completed, slowly add ethanol dropwise with stirring until the solid is completely precipitated. Pour off the liquid, and the obtained polymethyl methacrylate is a white solid. Dry to constant weight at 60°C in a vacuum drying oven, and the net yield of the blend is about 200mg, and the conversion rate is about 100%. Using gel chromatography to dissolve the blend and test it, a single peak can be obtained, and its molecular weight is: 103,000, and the molecular weight distribution is: 1.42. Using nuclear magnetic resonance hydrogen spectrum analysis, the content of the syndiotactic component is 80.0%.
[0039] Example 3, weigh 0.0160g (0.02mmol) of complex 3-Sc in a 25mL schelank bottle, dissolve it with 6mL toluene, place it in -78 degree ice ethanol, and after 15min, add 2.000g (20.0mmol) of methyl methacrylate, and start stirring. React for 12 hours. After the reaction is completed, slowly add ethanol dropwise under stirring until the solid is completely precipitated. Pour off the liquid, and the obtained polymethyl methacrylate is a white solid. Dry to constant weight at 60℃ in a vacuum drying oven, and the net yield of the blend is about 2g, and the conversion rate is about 100%. Use gel chromatography to dissolve the blend and test it, and a single peak can be obtained, and its molecular weight is: 644,000, and the molecular weight distribution is: 1.27. Using nuclear magnetic resonance hydrogen spectrum analysis, the content of the syndiotactic component is 71.0%.
Claims
1. A method for producing optical grade polymethyl methacrylate, characterized in that: A single-component rare earth complex is used as a catalyst, and the structure of the single-component rare earth complex is shown in Formula 1 below: Among them, the ligand R group is a hydrocarbon group (CH2) n(n=2~6) , dibenzylamino (C6H5CH2)2N, one of the aromatic groups; rare earth metal Ln is one of scandium (Sc), yttrium (Y) and all lanthanide elements; The specific steps of manufacturing are as follows: (1) Drying monomers and solvents: Methyl methacrylate is mixed with CaH2 at room temperature, stirred for 16-24 hours, evaporated under reduced pressure, degassed three times to remove oxygen; then stored at low temperature under anhydrous and oxygen-free conditions; after the solvent is purified, soaked in sodium tablets and placed in a glove box for later use; (2) Solution polymerization of methyl methacrylate: At room temperature, in an anhydrous and oxygen-free environment, take 0.01-10 mmol of the catalyst, put it into an eggplant-shaped bottle, add 1-1000 mL of solvent to dissolve it, and then weigh 0.2-1000 g of methyl methacrylate and add it; react for 1-12 hours; then inject 1-20 mL of ethanol containing a small amount of concentrated hydrochloric acid into the system to quench the reaction; after 5-20 minutes, slowly add 5-5000 mL of ethanol until the solid is completely precipitated; the obtained solid is placed in a vacuum drying oven and dried at 40-70°C to constant weight; (3) Purification of polymethyl methacrylate: Take 2-20 g of polymethyl methacrylate after constant weight and dissolve it in 5-50 mL of THF, then add 20-200 mL of ethanol to precipitate it, repeat several times, and place it in a vacuum drying oven to dry to constant weight.
2. The manufacturing method according to claim 1, characterized in that: In the single-component rare earth complex, the rare earth metal is Lu or Sc; the ligand substituent is R=(C6H5CH2)2N or R=p-OMe-Ph.
3. The manufacturing method according to claim 2, characterized in that: The single-component rare earth complex is one of the following: The R group on the ligand is phenyl, and the central metal is Sc; it is denoted as 1-Sc catalyst; The R group on the ligand is p-methoxyphenyl, and the central metal is Sc; it is denoted as 2-Sc catalyst; The R group on the ligand is dibenzylamino, and the central metal is Sc; it is denoted as 3-Sc catalyst; The R group on the ligand is dibenzylamino, and the central metal is Lu; it is denoted as 3-Lu catalyst.
4. The manufacturing method according to claim 1, characterized in that: The polymerization solvent is selected from toluene and chlorobenzene.
5. A catalyst for the production of optical grade polymethyl methacrylate, characterized in that: It is a single-component rare earth complex, and the structure of the single-component rare earth complex is shown in the following formula 1: Among them, the ligand R group is a hydrocarbon group (CH2) n(n=2~6) , dibenzylamino (C6H5CH2)2N, one of the aromatic groups; the rare earth metal Ln is one of scandium (Sc), yttrium (Y) and all lanthanide elements.
6. The catalyst according to claim 5, characterized in that: The R group on the ligand is phenyl, and the central metal is Sc; it is denoted as 1-Sc catalyst; The R group on the ligand is p-methoxyphenyl, and the central metal is Sc; it is denoted as 2-Sc catalyst; The R group on the ligand is dibenzylamino, and the central metal is Sc; it is denoted as 3-Sc catalyst; The R group on the ligand is dibenzylamino, and the central metal is Lu; it is denoted as 3-Lu catalyst.
Citation Information
Patent Citations
Alpha-diimine rare-earth metal catalyst and preparation method and application thereof
CN101792498A
Catalyst for ternary polymerization of norbornene, acrylate and cyclohexene and preparation method thereof and ternary polymerization method
CN102153701A
Rare earth metal catalyst for catalysis of polar vinyl monomer polymerization
CN105237659A
Synthesis and application of rare-earth metal frustrated Lewis pair containing tridentate NNP ligand
CN106478717A
Coordination chain transfer polyisoprene system based on amidino rare earth alkyl compound
CN111087508A