Phosphorus-containing intrinsic flame-retardant epoxy resin as well as preparation method and application thereof
By introducing phosphoric acid, pyrophosphoric acid or tripolyphosphoric acid into epoxy resin, the problems of harsh chain extension reaction conditions and difficult adjustment of phosphorus content are solved, and a flame-retardant epoxy resin with high phosphorus content and range control is achieved, showing excellent performance flame retardant and smoke suppression properties.
Patent Information
- Application Number
- CN202410842102.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-27
AI Technical Summary
In the existing technology, the reaction conditions of flame-retardant epoxy resins using phosphaphenanthrene groups introduced by the chain extension reaction are harsh and the phosphorus content is difficult to adjust, making it difficult to achieve high phosphorus content and range control.
By introducing phosphoric acid, pyrophosphoric acid or tripolyphosphoric acid into the molecular structure of epoxy resin, using mild reaction conditions (55-70°C) and simple process flow, controllable phosphorus content and high phosphorus content can be achieved. Using epoxy Phosphate esters, epoxy pyrophosphate or epoxy tripolyphosphate serve as key components.
It achieves controllability of phosphorus content and higher regulation of phosphorus content. The reaction conditions are simple and it shows excellent flame retardant and smoke suppression properties at only 1/20 or 1/40 of the epoxy resin.
Smart Images

Figure CN118772372A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of flame-retardant epoxy resin compositions, and in particular relates to a phosphorus-containing intrinsic flame-retardant epoxy resin and a preparation method and application thereof. Background Art
[0002] Epoxy resin (EP), as an important thermosetting material, has excellent physical, mechanical and electrical insulation properties, bonding properties with various materials, and flexible use processes. It is widely used in the fields of electronics, coatings, adhesives, fiber-reinforced composite materials, etc. However, the limiting oxygen index (LOI) of pure epoxy resin is about 23%, and it can burn in the air, while releasing a large amount of heat and harmful gases, accompanied by high-temperature molten droplets dripping, which poses a huge hidden danger to human life and property, and greatly limits the application of epoxy resin. Therefore, it is very important to give epoxy resin flame retardant properties.
[0003] Generally speaking, the flame retardant methods of epoxy resin can be divided into two categories: additive and reactive. Additive flame retardant epoxy resin is to introduce flame retardants containing elements such as P, Si, N, C into epoxy resin through mechanical mixing, and there is no chemical reaction between the flame retardant additive and the epoxy resin. Common additive flame retardants for epoxy resin include red phosphorus, silica, ammonium polyphosphate, hydrotalcite, inorganic hydroxides and inorganic oxides. This method has obvious advantages such as simple process and low cost, but it also has disadvantages such as uneven dispersion of flame retardants, easy migration, and poor compatibility between the matrix and flame retardant.
[0004] Reactive flame retardant is also called intrinsic flame retardant. It is to introduce flame retardant monomers into the polymer structure through covalent bonds and other means, which overcomes the shortcomings of additive flame retardants such as poor dispersibility and compatibility, and easy migration. Intrinsic flame retardant epoxy resin refers to the introduction of flame retardant functional groups or elements (such as Cl, Br, N, P, Si, etc.) during the synthesis of resins containing epoxy groups or by chemical methods in the later stage, so that it has flame retardancy. However, although the introduction of halogens represented by Cl and Br can produce good flame retardant effects, highly toxic carcinogenic and highly corrosive harmful gases such as hydrogen halides, brominated furans, and dioxins will be produced during combustion, which will cause damage to the environment and human health and have been banned by the European Union and other countries. Therefore, the current method is mainly to introduce elements such as P, N and Si to prepare halogen-free intrinsic flame retardant epoxy resins. The advantages of this method are that the flame retardant elements are not easy to migrate out, the compatibility is good, the influence on the mechanical properties of the epoxy resin is small, and a small amount of flame retardant can achieve excellent flame retardant effects. The disadvantages are complex process and high cost.
[0005] Among the flame retardant elements or groups mentioned above, phosphorus flame retardants play a key role in halogen-free flame retardants due to their abundant resources, low smoke release, low toxicity, chemical versatility, multiple flame retardant mechanisms and high flame retardant efficiency. The use of phosphorus flame retardants can also be divided into two types: additive and reactive. Additive phosphorus flame retardants include inorganic phosphorus compounds such as phosphates, ammonium polyphosphate and red phosphorus, as well as organic phosphorus compounds such as alkyl (aryl) phosphates, phosphites, phosphazenes, and phosphorus-containing Schiff bases. Reactive phosphorus flame retardants are divided into two categories: phosphorus-containing curing agents and phosphorus-containing epoxy resins. The former is to add a curing agent containing a flame retardant structure to the epoxy resin matrix, and use it to cure the epoxy resin. The cured epoxy resin has good flame retardant properties. Instead, the latter is directly polymerized from monomers containing flame retardants. Among them, phosphaphenanthrene flame retardants represented by DOPO are the most typical. Usually, DOPO or its derivatives are introduced into the epoxy resin molecular chain by chain extension reaction. The process is relatively complicated and the reaction conditions are relatively harsh. In addition, it is difficult to adjust the phosphorus content in epoxy resin, and it is necessary to design reactions at the front end to construct DOPO derivatives with more complex structures.
[0006] In view of the problems that the reaction conditions of the intrinsic flame-retardant epoxy resins introduced with phosphaphenanthrene groups by chain extension reaction are harsh and the phosphorus content is difficult to adjust, it is urgent to propose a phosphorus-containing intrinsic flame-retardant epoxy resin with mild reaction conditions and which can achieve a higher phosphorus content and a wider range of phosphorus content regulation. Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a phosphorus-containing intrinsic flame-retardant epoxy resin with simple process, low cost and good flame-retardant effect, as well as a preparation method and application thereof.
[0008] To achieve the above object, the technical solution of the present invention is:
[0009] In a first aspect, the present invention provides a phosphorus-containing intrinsic flame-retardant epoxy resin, comprising epoxy phosphate, epoxy pyrophosphate, or epoxy tripolyphosphate, and corresponding cured products thereof.
[0010] In a second aspect, the present invention provides a method for preparing the phosphorus-containing intrinsic flame retardant epoxy resin as described above, comprising the following steps:
[0011] S1, adding a certain amount of bisphenol A epoxy resin into a solvent, heating and stirring to dissolve it, to obtain solution A;
[0012] S2, weighing a corresponding amount of inorganic phosphoric acid, dissolving it in the same solvent to obtain solution B;
[0013] S3, mixing solution A and solution B in a reaction container, and continuously stirring and refluxing to react to obtain solution C;
[0014] S4. Remove the solvent from solution C to obtain product D.
[0015] Further, in step S1, the solvent is a mixture of one or more of acetone, ketone, ethyl ketone, cyclohexanone, ethyl acetate, toluene, xylene, anhydrous ethanol, and ethylene glycol;
[0016] Preferably, when the solvent is acetone, the ratio of epoxy resin to acetone is 1 g:2.5 mL.
[0017] Furthermore, in step S2:
[0018] The inorganic phosphoric acid is phosphoric acid (PI), pyrophosphoric acid (PPI) or tripolyphosphoric acid (PPA);
[0019] The corresponding reaction equations are shown below:
[0020]
[0021] Preferably, the molar ratio of the epoxy resin to the inorganic phosphoric acid is 5 to 70:1.
[0022] Furthermore, in step S3, the reaction temperature is 55-70° C., and the reaction time is 2.5-4.5 h.
[0023] Further, in step S3, solution B is slowly added to solution A under continuous stirring.
[0024] In a third aspect, the present invention provides an application of the phosphorus-containing intrinsic flame retardant epoxy resin as described above, comprising the following steps:
[0025] S01. Place the flame retardant epoxy resin in a dry container, and heat and stir until it is completely melted;
[0026] S02. Add curing agent to the melt and stir vigorously until the curing agent is evenly mixed;
[0027] S03, placing the above mixture in a vacuum drying oven and evacuating the air to remove bubbles;
[0028] S04. After degassing, pour the mixture into a preheated mold to prepare a specimen, and place it in a vacuum drying oven for curing;
[0029] S05, after the curing is completed, cooling and demoulding are performed to obtain a cured product.
[0030] Furthermore, in step S02:
[0031] The curing agent is 4,4'-diaminodiphenylmethane (DDM);
[0032] The curing agent was added in batches within 5 minutes.
[0033] Furthermore, in step S03:
[0034] The vacuum drying temperature is 100-130°C;
[0035] The vacuum drying time shall not exceed 5 minutes.
[0036] Furthermore, in step S04, the curing process is: baking at 120° C. for 2 hours, then heating to 150° C. and baking for another 2 hours.
[0037] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:
[0038] (1) The present invention introduces phosphoric acid, pyrophosphoric acid and tripolyphosphoric acid into the molecular structure of epoxy resin to realize intrinsic flame retardant epoxy resin with controllable phosphorus content. The reaction conditions are mild and the reaction temperature is only 55-70°C, which is simpler than the chain extension reaction at about 160°C and requiring a catalyst.
[0039] (2) The phosphorus-containing epoxy resin prepared by the present invention can achieve a higher phosphorus content and a wider range of phosphorus content control;
[0040] (3) The phosphorus-containing intrinsic flame-retardant epoxy resin of the present invention exhibits excellent flame retardancy and smoke suppression properties when only 1 / 20 or 1 / 40 of the epoxy resin reacts. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The accompanying drawings are part of the present invention and are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention, but do not constitute an improper limitation of the present invention. Obviously, the drawings described below are only some embodiments. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In the drawings:
[0042] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of Preparation Example 1.
[0043] Figure 2 This is the hydrogen nuclear magnetic resonance spectrum of Preparation Example 2.
[0044] Figure 3 This is the hydrogen nuclear magnetic resonance spectrum of Preparation Example 3.
[0045] Figure 4 It is the HRR curve of pure EP and phosphorus-containing epoxy resin cured product.
[0046] Figure 5 This is the THR curve of pure EP and phosphorus-containing epoxy resin cured product.
[0047] Figure 6 It is the SPR curve of pure EP and phosphorus-containing epoxy resin cured product.
[0048] Figure 7 These are the TSP curves of pure EP and phosphorus-containing epoxy resin cured products.
[0049] It should be noted that these drawings and textual descriptions are not intended to limit the conceptual scope of the present invention in any way, but are intended to illustrate the concept of the present invention for those skilled in the art by referring to specific embodiments. DETAILED DESCRIPTION
[0050] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The following embodiments are used to illustrate the present invention but are not used to limit the scope of the present invention.
[0051] It should be noted that the bisphenol A epoxy resin described in the present invention includes various types, such as E-44, E-42, E-51, E-55, etc., and this specification takes E44 as an example for explanation; the solvent of the reaction system includes but is not limited to a mixture of one or more of acetone, ketone, ethyl ketone, cyclohexanone, ethyl acetate, toluene, xylene, anhydrous ethanol, and ethylene glycol, and this specification takes acetone as an example.
[0052] Preparation Example 1
[0053] Weigh 80.00g of bisphenol A epoxy resin E44, add 200mL of acetone, heat to 65°C and stir to dissolve, to obtain an epoxy resin-acetone solution; weigh 40.60g of phosphoric acid solution, add 80mL of acetone and stir to obtain a phosphoric acid-acetone solution; under continuous stirring, slowly add the phosphoric acid-acetone solution to the epoxy resin-acetone solution, reflux at 65°C for 4.5h; remove the acetone solvent by rotary evaporation to obtain a sample labeled EP-PI; the epoxy group conversion rate of the sample is measured by the national standard GB / T-1677 to be 99.2%, and the nuclear magnetic hydrogen spectrum is as follows Figure 1 shown.
[0054] Preparation Example 2
[0055] Weigh 80.00g of bisphenol A epoxy resin E44, add 200mL of acetone, heat to 55°C and stir to dissolve, to obtain an epoxy resin-acetone solution; weigh 62.73g of pyrophosphoric acid, add 100mL of acetone and stir to obtain a pyrophosphoric acid-acetone solution; under continuous stirring, slowly add the pyrophosphoric acid-acetone solution to the epoxy resin-acetone solution, and reflux at 55°C for 3h; remove the acetone solvent by rotary evaporation to obtain a sample labeled EP-PPI; the epoxy group conversion rate of the sample is measured by the national standard GB / T-1677 to be 97.5%, and the nuclear magnetic hydrogen spectrum is as follows Figure 2 shown.
[0056] Preparation Example 3
[0057] Weigh 80.00g of bisphenol A epoxy resin E44, add 200mL of acetone, heat to 70°C and stir to dissolve, to obtain an epoxy resin-acetone solution; weigh 119.12g of tripolyphosphoric acid, add 120mL of acetone and stir to obtain a tripolyphosphoric acid-acetone solution; under continuous stirring, slowly add the tripolyphosphoric acid-acetone solution to the epoxy resin-acetone solution, and reflux at 70°C for 2.5h; remove the acetone solvent by rotary evaporation to obtain a sample labeled EP-PPA; the epoxy group conversion rate of the sample is measured by the national standard GB / T-1677 to be 95.6%, and the nuclear magnetic hydrogen spectrum is as follows Figure 3 shown.
[0058] Preparation Example 4
[0059] Weigh 80.00g of bisphenol A epoxy resin E44, add 200mL of acetone, heat to 65°C and stir to dissolve it to obtain an epoxy resin-acetone solution; then weigh 1.02g of phosphoric acid solution, add 10mL of acetone and stir to obtain a phosphoric acid-acetone solution; under continuous stirring, slowly add the phosphoric acid-acetone solution to the epoxy resin-acetone solution, reflux at 65°C for 4.5h; remove the acetone solvent by rotary evaporation to obtain a sample labeled EP-PI (20:1).
[0060] Preparation Example 5
[0061] Weigh 80.00g of bisphenol A epoxy resin E44, add 200mL of acetone, heat to 55°C and stir to dissolve it to obtain an epoxy resin-acetone solution; then weigh 1.57g of pyrophosphoric acid, add 10mL of acetone and stir to obtain a pyrophosphoric acid-acetone solution; under continuous stirring, slowly add the pyrophosphoric acid-acetone solution to the epoxy resin-acetone solution, and reflux at 55°C for 3h; remove the acetone solvent by rotary evaporation to obtain a sample labeled EP-PPI (20:1).
[0062] Preparation Example 6
[0063] Weigh 80.00g of bisphenol A epoxy resin E44, add 200mL of acetone, heat to 70°C and stir to dissolve it to obtain an epoxy resin-acetone solution; then weigh 2.98g of tripolyphosphoric acid, add 10mL of acetone and stir to obtain a tripolyphosphoric acid-acetone solution; under continuous stirring, slowly add the tripolyphosphoric acid-acetone solution to the epoxy resin-acetone solution, reflux at 70°C for 2.5h; remove the acetone solvent by rotary evaporation to obtain a sample labeled EP-PPA (20:1).
[0064] Preparation Example 7
[0065] Weigh 80.00g of bisphenol A epoxy resin E44, add 200mL of acetone, heat to 65°C and stir to dissolve it to obtain an epoxy resin-acetone solution; then weigh 0.51g of phosphoric acid solution, add 5mL of acetone and stir to obtain a phosphoric acid-acetone solution; under continuous stirring, slowly add the phosphoric acid-acetone solution to the epoxy resin-acetone solution, reflux at 65°C for 4.5h; remove the acetone solvent by rotary evaporation to obtain a sample labeled EP-PI (40:1).
[0066] Preparation Example 8
[0067] Weigh 80.00g of bisphenol A epoxy resin E44, add 200mL of acetone, heat to 55°C and stir to dissolve it to obtain an epoxy resin-acetone solution; then weigh 0.78g of pyrophosphoric acid, add 5mL of acetone and stir to obtain a pyrophosphoric acid-acetone solution; under continuous stirring, slowly add the pyrophosphoric acid-acetone solution to the epoxy resin-acetone solution, reflux at 55°C for 3h; remove the acetone solvent by rotary evaporation to obtain a sample labeled EP-PPI (40:1).
[0068] Preparation Example 9
[0069] Weigh 80.00g of bisphenol A epoxy resin E44, add 200mL of acetone, heat to 70°C and stir to dissolve it to obtain an epoxy resin-acetone solution; then weigh 1.49g of tripolyphosphoric acid, add 5mL of acetone and stir to obtain a tripolyphosphoric acid-acetone solution; under continuous stirring, slowly add the tripolyphosphoric acid-acetone solution to the epoxy resin-acetone solution, reflux at 70°C for 2.5h; remove the acetone solvent by rotary evaporation to obtain a sample labeled EP-PPA (40:1).
[0070] Example 1
[0071] Weigh 80g of EP-PI (20:1), EP-PPI (20:1), and EP-PPA (20:1) respectively and add them to a dry beaker, place it at 90°C and stir until it is completely melted; add 16.57g of curing agent 4,4'-diaminodiphenylmethane (DDM) to the melt, add it in batches within 5 minutes, and stir vigorously until the curing agent is completely mixed; place the above mixture in a 120°C vacuum drying oven to evacuate (no more than 5 minutes) to complete the defoaming work; then pour the mixed slurry into a preheated mold to prepare a specimen, and place it in a vacuum drying oven for curing: bake at 120°C for 2h, then heat to 150°C and bake for another 2h; after curing, cool it slightly and demold it to obtain EP-PI (20:1), EP-PPI (20:1), and EP-PPA (20:1) cured products.
[0072] The EP-PI (20:1), EP-PPI (20:1), and EP-PPA (20:1) were prepared by Preparation Examples 4, 6, and 8, respectively.
[0073] Example 2
[0074] Weigh 80g of EP-PI (40:1), EP-PPI (40:1), and EP-PPA (40:1) respectively and add them to a dry beaker, place it at 90°C and stir until it is completely melted; add 17.01g of curing agent DDM to the melt, add it in batches within 5 minutes, and stir vigorously until the curing agent is completely mixed; place the above mixture in a 120°C vacuum drying oven to evacuate (no more than 5 minutes) to complete the degassing work; then pour the mixed slurry into a preheated mold to prepare a specimen, and place it in a vacuum drying oven for curing: bake at 120°C for 2h, then heat to 150°C and bake for another 2h; after curing, cool it slightly and demold it to obtain EP-PI (40:1), EP-PPI (40:1), and EP-PPA (40:1) cured products.
[0075] The EP-PI (40:1), EP-PPI (40:1), and EP-PPA (40:1) were prepared by Preparation Examples 5, 7, and 9, respectively.
[0076] Comparative Example 1
[0077] Weigh 80g of bisphenol A epoxy resin E44 and add it to a dry beaker, place it at 90℃ and stir until it is completely melted; add 17.45g of curing agent DDM to the melt, add it in batches within 5 minutes, and stir vigorously until the curing agent is completely mixed; place the above mixture in a 120℃ vacuum drying oven to evacuate (no more than 5 minutes) to complete the defoaming work; then pour the mixed slurry into a preheated mold to prepare a specimen, and place it in a vacuum drying oven for curing: bake at 120℃ for 2h, then heat to 150℃ and bake for another 2h; after curing is completed, cool it slightly and demold it to obtain the EP cured product.
[0078] Test Example 1: Determination of flame retardant properties of soft PVC / MHEPE composite materials
[0079] (1) Test method:
[0080] The 7 kinds of cured products prepared in Examples 1-2 and Comparative Example 1 were taken to measure their LOI value, heat release rate (HRR), total heat release (THR), smoke production rate (SPR) and total smoke production (TSP), and the measuring methods were as follows: LOI value was tested according to the test conditions and steps specified in GB / T2406.2-2009 "Determination of Combustion Behavior of Plastics by Oxygen Index Method", and the sample size was 80mm×10mm×4mm. The remaining parameters were tested according to the test conditions and steps specified in GB / T16172-2007 "Test Method for Heat Release Rate of Building Materials", and the sample size was 100mm×100mm×3mm, and the irradiation intensity was 35kW / m2.
[0081] (2) Test results:
[0082] The LOI values of the above 7 kinds of cured products are shown in Table 1; the comparison of HRR and THR curves is shown in Figure 4 and Figure 5 As shown; SPR and TSP curves are shown Figure 6 and Figure 7 shown.
[0083] It can be seen from Table 1 that the LOI values of the six cured products, EP-PI (20:1), EP-PI (40:1), EP-PPI (20:1), EP-PPI (40:1), EP-PPA (20:1), and EP-PPA (40:1), are all greater than that of pure EP. Figure 4 and Figure 5It can be seen that the HRR and THR of the above six cured products are all lower than those of pure EP. Taking EP-PPA (40:1) as an example, its LOI value, peak HRR and THR values are 32.33%, 462.99kW / m2 and 98.7MJ / m2, respectively, which are 31.96% higher, 46.54% lower and 13.05% lower than those of pure EP, respectively. That is, when only 1 / 40 of EP-PPA exists, excellent flame retardant effect can be achieved.
[0084]
[0085] Table 1
[0086] Depend on Figure 6 and Figure 7 It can be seen that the SPR and TSP values of the six cured products, EP-PI (20:1), EP-PI (40:1), EP-PPI (20:1), EP-PPI (40:1), EP-PPA (20:1), and EP-PPA (40:1), are all lower than those of pure EP. Taking EP-PPA (40:1) as an example, its peak SPR and TSP are 0.1114m2 / s and 22.8m2, respectively, which are 66.87% and 50.97% lower than those of pure EP, respectively, showing excellent smoke suppression performance.
[0087] The above description is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modifications to equivalent embodiments of equivalent changes by using the technical content suggested above without departing from the scope of the technical solution of the present invention. The implementation scheme in the above embodiment can also be further combined or replaced. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the solution of the present invention.
Claims
1. A phosphorus-containing intrinsic flame-retardant epoxy resin, characterized in that: It comprises epoxy phosphate, epoxy pyrophosphate, epoxy tripolyphosphate, and corresponding cured products.
2. A method for preparing the phosphorus-containing intrinsic flame-retardant epoxy resin as claimed in claim 1, characterized in that: The following steps are involved: S1, adding a certain amount of bisphenol A epoxy resin into a solvent, heating and stirring to dissolve it, to obtain solution A; S2, weighing a corresponding amount of inorganic phosphoric acid, dissolving it in the same solvent to obtain solution B; S3, mixing solution A and solution B in a reaction container, and continuously stirring and refluxing to react to obtain solution C; S4. Remove the solvent from solution C to obtain product D.
3. The method for preparing the phosphorus-containing intrinsic flame-retardant epoxy resin according to claim 2, characterized in that: In step S1: The solvent is a mixture of one or more of acetone, ketone, ethyl ketone, cyclohexanone, ethyl acetate, toluene, xylene, anhydrous ethanol, and ethylene glycol; Preferably, when the solvent is acetone, the ratio of epoxy resin to acetone is 1 g:2.5 mL.
4. The method for preparing the phosphorus-containing intrinsic flame-retardant epoxy resin according to claim 2, characterized in that: In step S2: The inorganic phosphoric acid is phosphoric acid, pyrophosphoric acid or tripolyphosphoric acid; Preferably, the molar ratio of the epoxy resin to the inorganic phosphoric acid is 5 to 70:
1.
5. The method for preparing the phosphorus-containing intrinsic flame-retardant epoxy resin according to claim 2, characterized in that: In step S3, the reaction temperature is 55-70° C., and the reaction time is 2.5-4.5 h.
6. The method for preparing the phosphorus-containing intrinsic flame-retardant epoxy resin according to claim 2, characterized in that: In step S3, solution B is slowly added to solution A under continuous stirring.
7. An application of the phosphorus-containing intrinsic flame-retardant epoxy resin as claimed in claim 1, characterized in that: The following steps are involved: S01. Place the flame retardant epoxy resin in a dry container, and heat and stir until it is completely melted; S02. Add curing agent to the melt and stir vigorously until the curing agent is evenly mixed; S03, placing the above mixture in a vacuum drying oven and evacuating the air to remove bubbles; S04. After degassing, pour the mixture into a preheated mold to prepare a specimen, and place it in a vacuum drying oven for curing; S05, after the curing is completed, cooling and demoulding are performed to obtain a cured product.
8. The use of the phosphorus-containing intrinsic flame-retardant epoxy resin as claimed in claim 7, characterized in that: In step S02: The curing agent is 4,4'-diaminodiphenylmethane; The curing agent was added in batches within 5 minutes.
9. The use of the phosphorus-containing intrinsic flame-retardant epoxy resin as claimed in claim 7, characterized in that: In step S03: The vacuum drying temperature is 100-130°C; The vacuum drying time shall not exceed 5 minutes.
10. The use of the phosphorus-containing intrinsic flame-retardant epoxy resin as claimed in claim 7, characterized in that: In step S04, the curing process is: baking at 120° C. for 2 hours, then heating to 150° C. and baking for another 2 hours.
Citation Information
Patent Citations
Epoxy resin or compound with phosphonate as molecular skeleton and synthesizing process thereof
CN100999568A
Silicon-phosphor-containing heat-stable hybridized epoxide resin and the preparing method and application thereof
CN101113196A
Flame-retardant epoxy resin composite material and preparation method thereof
CN114685937A
Magnesium hydroxide / epoxy phosphate composite flame retardant as well as preparation method and application thereof
CN116589748A
Epoxy phosphate ester resin, its production and coating composition containing the resin
US5389704A