Preparation method of flame-retardant epoxy resin composite material containing phosphorus, nitrogen and sulfur oligomer
Through the synergistic effect of synthesizing phosphorus-containing nitrogen-sulfur oligomer flame retardants and epoxy resins, the problem of heat and smoke generated by the combustion of epoxy resin materials is solved, and low toxicity and high-efficiency flame retardant properties are achieved, which satisfies the needs of aerospace and other industries. Strict flame retardant requirements in the field.
Patent Information
- Application Number
- CN202410977122.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Epoxy resin materials generate a large amount of heat and toxic smoke during the combustion process, which poses a threat to personal and property safety. Existing halogen flame retardants have toxic risks, and a single phosphorus flame retardant is added in a large amount, making it difficult to meet flame retardant requirements. .
By synthesizing phosphorus-containing nitrogen-sulfur oligomer flame retardants and utilizing the synergistic effect of phosphorus, nitrogen, and sulfur elements, a flame-retardant epoxy resin composite material that is well compatible with epoxy resin is prepared with a simple process and high yield. High, only a low addition amount is needed to achieve high flame retardant effect.
It achieves low toxicity and high-efficiency flame retardant properties of epoxy resin composite materials, reaching a limiting oxygen index of 31.0% and a vertical combustion rating of UL-94 V-0, with simple production conditions and easy post-processing.
Smart Images

Figure CN118772373A_ABST
Abstract
Description
[0001] Technology
[0002] The invention belongs to the technical field of flame-retardant polymers, and in particular relates to a method for preparing a flame-retardant epoxy resin composite material containing phosphorus, nitrogen and sulfur oligomers. Background Art
[0003] Epoxy resin (EP) is a promising thermosetting resin that is widely used in various fields such as coatings, adhesives, electronics, and aerospace due to its excellent adhesion, chemical resistance, and excellent electrical insulation. However, EP materials are highly flammable and may produce a large amount of heat and toxic fumes during combustion. This poses a major threat to personal safety and property. Therefore, in order to meet the strict flame retardancy requirements of practical applications such as electronics and aerospace industries, there is an increasing demand for flame retardant modification of EP.
[0004] In previous studies, halogen flame retardants have been widely used to enhance the flame retardancy of EP. Most of these flame retardants can scavenge active free radicals in the gas phase. Although this method effectively slows down the burning rate, it must be acknowledged that the toxicity of halogen flame retardants poses potential risks to human health and the environment. Phosphorus-based flame retardants have the advantages of safety, high efficiency, and environmental protection, and are widely regarded as viable alternatives to halogenated flame retardants. They are widely used in various polymers, such as phosphates, phosphate nitrile, and especially 9,10-dihydro-9-oxo-10-phosphophenanthrene-10-oxide (DOPO). Due to its excellent flame retardant properties in different materials, DOPO has received widespread attention from academia and industry. However, a single DOPO-based flame retardant containing only phosphorus needs to be added in large quantities to ensure good flame retardancy. In order to overcome the above defects, other flame retardant elements such as nitrogen and sulfur are introduced into DOPO derivatives by physical blending or chemical synthesis. Different elements show synergistic effects on the gas phase and / or condensed phase, thereby significantly improving the flame retardant properties of DOPO derivatives. Nitrogen-containing flame retardants can release non-combustible gases during combustion, thereby diluting flammable pyrolysis byproducts and oxygen. Sulfur-containing flame retardants mainly work in the gas phase, inhibiting combustion by producing non-combustible gases, thereby reducing the concentration of combustible gases. In addition, the advantages of oligomers include low viscosity and rich functional groups. They have good compatibility with epoxy resins and are good substitutes for flame retardants in epoxy resin composites.
[0005] The new process for synthesizing phosphorus-nitrogen-sulfur oligomer flame retardant described in the present invention is original; the flame retardant described in the present invention has a large number of hydroxyl active groups, which can further react with substances with epoxy groups; through the synergistic effect of phosphorus, nitrogen and sulfur elements, its flame retardant efficiency and mechanical properties are improved; the process of the present invention has simple production conditions, high yield and simple post-treatment process. Summary of the invention
[0006] In order to solve the deficiencies in the prior art, the object of the present invention is to provide a method for preparing a flame-retardant epoxy resin composite material containing phosphorus, nitrogen and sulfur oligomers.
[0007] The present invention comprises the following steps:
[0008] (1) dissolving terephthalaldehyde in anhydrous ethanol to obtain solution A;
[0009] (2) Then, p-aminothiophenol is added to anhydrous ethanol and stirred until transparent to obtain solution B;
[0010] (3) Solution A and solution B are added to a three-necked flask successively, heated and stirred to obtain solution C;
[0011] (4) Filtering the solution D to obtain a precipitate, washing it with ethanol to remove residual p-aminothiophenol and terephthalaldehyde, and then drying it to obtain a powder E;
[0012] (5) dissolving 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide in ethanol to obtain solution F;
[0013] (6) adding powder E to solution F under stirring, heating and stirring to obtain solution G;
[0014] (7) filtering the solution G to obtain a precipitate, washing it with ethanol to remove the residual 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and then drying it to obtain a phosphorus, nitrogen and sulfur-containing oligomer;
[0015] (8) Adding phosphorus, nitrogen and sulfur oligomers to epoxy resin, adding curing agent after stirring, stirring again, then pouring the mixture into a mold, and curing in an oven to obtain a phosphorus, nitrogen and sulfur oligomer flame retardant epoxy resin composite material. The reaction process is shown in Formula 1:
[0016]
[0017] In the step (1), the mixing ratio of terephthalaldehyde to anhydrous ethanol is 1.2-1.3 g: 100-125 mL; solution A is obtained.
[0018] In the step (2), the mixing ratio of p-aminothiophenol to anhydrous ethanol is 1.2-1.3 g: 100-125 mL; and solution B is obtained.
[0019] The stirring in steps (2) and (6) is mechanical stirring, the stirring temperature is 85-90° C., and the stirring time is 2-3 hours to obtain solution C.
[0020] The steps (4) and (7) are vacuum filtration, the drying is vacuum drying, the drying temperature is 60-70° C., and the drying time is 6-12 hours.
[0021] In the step (5), the mixing ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and ethanol is 2.2-2.3 g: 100-125 mL.
[0022] In the step (6), the mixing ratio of powder E to anhydrous ethanol is 2.4-2.6 g: 100-125 mL; solution B is obtained.
[0023] In the step (7), the mixing mass ratio of the epoxy resin, the curing agent and the flame retardant phosphorus-nitrogen-sulfur oligomer is 90-100:24-25:1-10.
[0024] The curing temperature in step (7) is 80-120° C., and the curing time is 0.5-4 hours.
[0025] Compared with the prior art, the present invention has the following advantages:
[0026] (1) The present invention provides a method for preparing a flame retardant phosphorus, nitrogen and sulfur oligomer. The preparation process of the flame retardant phosphorus, nitrogen and sulfur oligomer is simple and easy to industrially produce.
[0027] (2) The present invention also utilizes the synthesized flame retardant phosphorus, nitrogen and sulfur oligomers to prepare a flame retardant epoxy resin composite material. Compared with pure epoxy resin, the epoxy resin composite material prepared by the preparation method only needs 2.5wt% of flame retardant to achieve a limiting oxygen index of 31.0% and a vertical burning rating of UL-94 V-0; the epoxy resin composite material prepared by the preparation method can achieve a limiting oxygen index of 34.2% and a vertical burning rating of UL94 V-0 with a flame retardant addition of 10wt%. The epoxy resin composite material obtained by the present invention has a small amount of flame retardant added and a good flame retardant effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The Fourier transform infrared spectra of terephthalaldehyde, p-aminothiophenol, intermediate product, DOPO and phosphorus, nitrogen and sulfur-containing oligomers in Example 1 are shown. DETAILED DESCRIPTION
[0029] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and embodiments of the specification, but the protection scope of the present invention is not limited to the following specific embodiments.
[0030] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0031] Unless otherwise specified, all reagents and raw materials used in the present invention are commercially available products or products that can be prepared by known methods.
[0032] The technical solution adopted by the invention is further described below in conjunction with the accompanying drawings and embodiments.
[0033] Example 1
[0034] The preparation of flame retardant phosphorus, nitrogen and sulfur oligomers specifically includes the following steps:
[0035] First, (0.01 mol, 1.20 g) of terephthalaldehyde and (0.01 mol, 1.25 g) of p-aminothiophenol were dissolved in 125 mL of ethanol, respectively, and then added into a three-necked flask, stirred at 85° C. for 4 h, filtered and dried at 60° C. for 10 h to obtain an intermediate product with a yield of 86.8%.
[0036] Then (0.01 mol, 2.16 g) DOPO was dissolved in 100 mL ethanol, and then (0.01 mol, 2.27 g) of the intermediate product was added and stirred in a three-necked flask at 85°C for 4 h. The crude product was filtered, washed with ethanol 3-5 times, and vacuum dried at 60°C for 12 h to obtain a flame retardant phosphorus, nitrogen and sulfur oligomer with a yield of 71.1%.
[0037] Figure 1 The following is the Fourier infrared spectrum of terephthalaldehyde, p-aminothiophenol, intermediates and phosphorus, nitrogen and sulfur oligomers. In the spectrum of terephthalaldehyde, 2870 cm -1 The peak at 2585 cm-1 of p-aminothiophenol disappears in the spectrum of the intermediate product. -1 (sulfur-hydrogen bond), 3450 and 3360 cm -1 The characteristic peak of OH (3400cm -1 ) and C=N(1700cm -1 ) appeared in the intermediate products respectively.
[0038] In the spectra of DOPO and phosphorus-nitrogen-sulfur oligomers, the -1 The characteristic peaks corresponding to P=O and POC functional groups were observed at 2390 cm -1 The pH peak at 1700 cm -1The disappearance of the C=N group peak at indicates that an addition reaction occurred between the PH in DOPO and the C=N of the intermediate product, thus confirming the successful synthesis of the phosphorus-nitrogen-sulfur oligomer.
[0039] Example 2
[0040] The preparation of flame retardant phosphorus, nitrogen and sulfur oligomer flame retardant epoxy resin composite material specifically comprises the following steps:
[0041] 80.0 g EP and 20 g 4,4-diaminodiphenylmethane (DDM) were heated and stirred in a 60°C water bath for 10 min, and then the mixture was poured into a standard-sized polytetrafluoroethylene mold coated with silicone oil, placed in an oven for curing, and then cooled and demolded to obtain pure EP.
[0042] 78.0 g of EP and 2.5 g of flame retardant phosphorus, nitrogen and sulfur oligomers were stirred for 10 min in a 60°C water bath and then 19.5 g of DDM were added. The stirring was continued for 10 min, and the mixture was poured into a standard-sized polytetrafluoroethylene mold coated with silicone oil, placed in an oven for curing, and then cooled and demolded to obtain Example 2.
[0043] 76.0 g of EP and 5.0 g of flame retardant phosphorus, nitrogen and sulfur oligomers were stirred for 10 min in a 60°C water bath and then 19.0 g of DDM were added. The stirring was continued for 10 min, and the mixture was poured into a standard-sized polytetrafluoroethylene mold coated with silicone oil, placed in an oven for curing, and then cooled and demolded to obtain Example 3.
[0044] 74.0 g of EP and 7.5 g of flame retardant phosphorus, nitrogen and sulfur oligomers were stirred for 10 min in a 60°C water bath and then 18.5 g of DDM were added. The stirring was continued for 10 min, and the mixture was poured into a standard-sized polytetrafluoroethylene mold coated with silicone oil, placed in an oven for curing, and then cooled and demolded to obtain Example 4.
[0045] 73.6 g EP and 10.0 g flame retardant phosphorus, nitrogen and sulfur oligomers were stirred for 10 min in a 60°C water bath and then 18.4 g DDM was added. The stirring was continued for 10 min. The mixture was then poured into a standard-sized polytetrafluoroethylene mold coated with silicone oil, placed in an oven for curing, and then cooled and demolded to obtain Example 5.
[0046] Table 1 Composition formula and test results of standard samples
[0047] Flame retardant addition amount (wt%) <![CDATA[EP+DDM a (wt%)]]> LOI(%) UL-94 Pure EP 0 100 25.8 NR Example 2 2.5 97.5 31.0 V-0 Example 3 5 95 32.3 V-0 Example 4 7.5 92.5 33.3 V-0 Example 5 10 95 25.8 V-0
[0048] EP+DDM a : The mass ratio of EP to DDM is 4:1.
Claims
1. A method for preparing a flame-retardant epoxy resin composite material containing phosphorus, nitrogen and sulfur oligomers, It is characterized in that The method comprises the following steps: (1) dissolving terephthalaldehyde in anhydrous ethanol to obtain solution A; (2) Then, p-aminothiophenol is added to anhydrous ethanol and stirred until transparent to obtain solution B; (3) Solution A and solution B are added to a three-necked flask successively, heated and stirred to obtain solution C; (4) Filtering the solution D to obtain a precipitate, washing it with ethanol to remove residual p-aminothiophenol and terephthalaldehyde, and then drying it to obtain a powder E; (5) dissolving 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide in ethanol to obtain solution F; (6) adding powder E to solution F under stirring, heating and stirring to obtain solution G; (7) filtering the solution G to obtain a precipitate, washing it with ethanol to remove the residual 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and then drying it to obtain a phosphorus, nitrogen and sulfur-containing oligomer; (8) Adding phosphorus, nitrogen and sulfur oligomers to epoxy resin, adding curing agent after stirring, stirring again, then pouring the mixture into a mold, putting it into an oven for curing to obtain a phosphorus, nitrogen and sulfur oligomer flame retardant epoxy resin composite material.
2. The method according to claim 1, It is characterized in that In the step (1), the mixing ratio of terephthalaldehyde to anhydrous ethanol is 1.2-1.3 g: 100-125 mL; and solution A is obtained.
3. The method according to claim 1, It is characterized in that In the step (2), the mixing ratio of p-aminothiophenol to anhydrous ethanol is 1.2-1.3 g: 100-125 mL; and solution B is obtained.
4. The method according to claim 1, It is characterized in that The stirring in steps (2) and (6) is mechanical stirring, the stirring temperature is 85-90° C., and the stirring time is 2-3 hours to obtain solution C.
5. The method according to claim 1, It is characterized in that In the step (4), the mixing mass ratio of the epoxy resin, the curing agent and the nicotinamide derivative is 70-80:19-20:0.1-10.
6. The method according to claim 1, It is characterized in that The steps (4) and (7) are vacuum filtration, the drying is vacuum drying, the drying temperature is 60-70° C., and the drying time is 6-12 hours.
7. The method according to claim 1, It is characterized in that In the step (5), the mixing ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and ethanol is 2.2-2.3 g: 100-125 mL.
8. The method according to claim 1, It is characterized in that In the step (6), the mixing ratio of powder E to anhydrous ethanol is 2.4-2.6 g: 100-125 mL; solution B is obtained.
9. The method according to claim 1, It is characterized in that In the step (7), the mixing mass ratio of the epoxy resin, the curing agent and the flame retardant phosphorus-nitrogen-sulfur oligomer is 90-100:24-25:1-10.
10. The method according to claim 1, It is characterized in that The curing temperature in step (7) is 80-120° C., and the curing time is 0.54 h.
Citation Information
Patent Citations
Preparation method of redox probe for marking CRP (C-Reactive Protein) impedance immunosensor
CN102914576A
Flame retardant containing phosphorus, nitrogen and sulfur and used for epoxy resin and preparation method of flame retardant
CN106009040A
Method for preparing nitrogen phosphate sulfur-containing reactive flame retardant applied to epoxy resin
CN106749413A
Preparation method and application of DOPO-containing diphenyl sulfone nitrogen phosphorus sulfur ternary synergistic flame retardant
CN110092944A
Preparation method of terephthalonitrile derivative flame-retardant epoxy resin composite material
CN113292823A