Fluorine-containing polyimide, preparation method of fluorine-containing polyimide, fluorine-containing polyimide film and preparation method of fluorine-containing polyimide film

By introducing a specific structure and optimized preparation method into polyimide, the problems of low transmittance and insufficient mechanical properties of traditional polyimide are solved, achieving both high transparency and high mechanical properties, which is suitable for the field of microelectronics.

CN118772404APending Publication Date: 2024-10-15CHANGCHUN INSTITUTE OF APPLIED CHEMISTRY CHINESE ACADEMY OF SCIENCES
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410884470.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Traditional aromatic polyimide has low transmittance in the field of microelectronics due to the tight arrangement of polymer chains and charge transfer complex effect, which limits its application in bottom-emission flexible display devices and is difficult to improve optical transparency. It is difficult to take into account the mechanical properties.

Method used

Optimize the polyimide molecular structure by introducing fluorine-containing substituents, flexible chain forging, alicyclic structures, asymmetric structures, bulky side groups and/or non-coplanar structures, and use copolymerization methods under inert gas and catalyst conditions Preparation of fluorine-containing polyimide film to improve its optical transparency and mechanical properties.

Benefits of technology

The polyimide achieves both excellent optical transparency and mechanical properties, reduces production costs, and improves processing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772404A_ABST
    Figure CN118772404A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of high polymer materials, and particularly relates to fluorine-containing polyimide, a preparation method thereof, a fluorine-containing polyimide film and a preparation method thereof. The fluorine-containing polyimide provided by the invention has a structure shown as a formula (I) or a formula (II), the molecular structure of polyimide is optimally designed, and a fluorine-containing substituent group, a flexible chain segment, an alicyclic structure, an asymmetric structure, a large-volume side group and / or a non-coplanar structure and the like are introduced into a polyimide molecular chain; the processing performance of the polyimide is improved, the production cost of the polyimide is reduced, and the polyimide has excellent optical transparency and mechanical properties. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and in particular relates to a fluorine-containing polyimide, a preparation method thereof, a fluorine-containing polyimide film and a preparation method thereof. Background Art

[0002] Polyimide has been widely used in the field of microelectronics due to its excellent comprehensive performance, structural diversity and designability. Among them, high-temperature resistant and highly transparent polyimide is considered to be one of the most promising transparent substrate materials in flexible displays. Traditional aromatic polyimide is generally polymerized by diamine with strong electron-donating ability and dianhydride with strong electron-accepting ability. The polymer molecular chains are closely arranged, and there are strong interactions between the aromatic rings, which will produce charge transfer complex (CTC) effects within or between polyimide chains, resulting in low transmittance in the visible light range, limiting its application in bottom-emitting flexible display devices.

[0003] In order to improve the optical transparency of polyimide films in the visible light region, the formation of CTC effect can be suppressed by reducing the stiffness of the polymer chain or reducing the intra-chain / inter-chain interactions, but at the same time sacrificing the mechanical properties of polyimide. Therefore, how to balance the optical transparency and mechanical properties of polyimide is particularly important. Summary of the invention

[0004] In view of this, an object of the present invention is to provide a fluorinated polyimide, a preparation method thereof, a fluorinated polyimide film and a preparation method thereof. The fluorinated polyimide provided by the present invention has both excellent optical transparency and mechanical properties.

[0005] The present invention provides a fluorinated polyimide having a structure of formula (I) or formula (II):

[0006]

[0007]

[0008] Where n1 and n2 represent the degree of polymerization, and the chemical structures of Ar1, Ar2 and Ar3 are as follows:

[0009] Ar1: Ar2: Ar3:

[0010] The present invention provides a method for preparing a fluorinated polyimide, comprising the following steps:

[0011] In the presence of an inert gas and a catalyst, the dianhydride monomer and the diamine monomer undergo a copolymerization reaction in a solvent to obtain a fluorinated polyimide;

[0012] The dianhydride monomer has the structure of formula (i):

[0013]

[0014] The diamine monomers are H2N-Ar1-NH2 and H2N-Ar3-NH2, or H2N-Ar2-NH2 and H2N-Ar3-NH2;

[0015] If the diamine monomers are H2N-Ar1-NH2 and H2N-Ar3-NH2, the fluorinated polyimide has a structure of formula (I):

[0016]

[0017] If the diamine monomers are H2N-Ar2-NH2 and H2N-Ar3-NH2, the fluorinated polyimide has a structure of formula (II);

[0018]

[0019] Where n1 and n2 represent the degree of polymerization, and the chemical structures of Ar1, Ar2 and Ar3 are as follows:

[0020] Ar1: Ar2: Ar3:

[0021] Preferably, the molar ratio of H2N-Ar1-NH2 to H2N-Ar3-NH2 is (1-10):1; the molar ratio of H2N-Ar2-NH2 to H2N-Ar3-NH2 is (1-10):1.

[0022] Preferably, the molar ratio of the dianhydride monomer to the diamine monomer is 1:(0.8-1.2).

[0023] Preferably, the catalyst is one or more of pyridine, picoline, triethylamine, picolinoline and isoquinoline; the amount of the catalyst used is 3-7% of the molar amount of the dianhydride monomer.

[0024] Preferably, the specific process of the copolymerization reaction includes:

[0025] a) mixing a dianhydride monomer, a diamine monomer and a solvent under an inert gas atmosphere, and heating them to perform a preliminary reaction;

[0026] b) adding a catalyst to the reaction system of step a), then raising the temperature to continue the reaction, to obtain a fluorine-containing polyimide.

[0027] Preferably, in step a), the heating temperature is 80-100° C., and the initial reaction time is 2-6 h; in step b), the terminal temperature of the heating is 160-200° C., and the reaction time is 2-6 h.

[0028] The present invention provides a fluorinated polyimide film, wherein the components of the fluorinated polyimide film include fluorinated polyimide of formula (I) and / or formula (II);

[0029]

[0030] Where n1 and n2 represent the degree of polymerization, and the chemical structures of Ar1, Ar2 and Ar3 are as follows:

[0031] Ar1: Ar2: Ar3:

[0032] The present invention provides a method for preparing a fluorinated polyimide film, comprising the following steps:

[0033] The casting solution is coated on a flat plate, and the temperature is increased to form a film to obtain a fluorinated polyimide film;

[0034] The casting solution contains a fluorinated polyimide having a structure of formula (I) and / or formula (II);

[0035]

[0036] Where n1 and n2 represent the degree of polymerization, and the chemical structures of Ar1, Ar2 and Ar3 are as follows:

[0037] Ar1: Ar2: Ar3:

[0038] Preferably, the temperature-raising method of the film-forming is gradient heating, and the film-forming temperature range is 60 to 270°C.

[0039] Compared with the prior art, the present invention provides a fluorine-containing polyimide, a preparation method thereof, a fluorine-containing polyimide film and a preparation method thereof. The fluorine-containing polyimide provided by the present invention has a structure of formula (I) or formula (II). The present invention optimizes the molecular structure of the polyimide, introduces fluorine-containing substituents, flexible chain forgings, alicyclic structures, asymmetric structures, bulky side groups and / or non-coplanar structures into the polyimide molecular chain, thereby improving the processing performance of the polyimide, reducing the production cost of the polyimide, and allowing the polyimide to have both excellent optical transparency and mechanical properties. DETAILED DESCRIPTION

[0040] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] The present invention provides a fluorinated polyimide having a structure of formula (I) or formula (II):

[0042]

[0043] Where n1 and n2 represent the degree of polymerization, and the chemical structures of Ar1, Ar2 and Ar3 are as follows:

[0044] Ar1: Ar2: Ar3:

[0045] In the fluorinated polyimide provided by the present invention, the ratio of n1 to n2 is preferably (1-10):1, specifically 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, 6.7:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1 or 10:1.

[0046] The present invention also provides a method for preparing fluorinated polyimide, comprising the following steps:

[0047] In the presence of an inert gas and a catalyst, the dianhydride monomer and the diamine monomer undergo a copolymerization reaction in a solvent to obtain a fluorinated polyimide;

[0048] The dianhydride monomer has the structure of formula (i):

[0049]

[0050] The diamine monomers are H2N-Ar1-NH2 and H2N-Ar3-NH2, or H2N-Ar2-NH2 and H2N-Ar3-NH2;

[0051] If the diamine monomers are H2N-Ar1-NH2 and H2N-Ar3-NH2, the fluorinated polyimide has a structure of formula (I):

[0052]

[0053] If the diamine monomers are H2N-Ar2-NH2 and H2N-Ar3-NH2, the fluorinated polyimide has a structure of formula (II);

[0054]

[0055] Where n1 and n2 represent the degree of polymerization, and the chemical structures of Ar1, Ar2 and Ar3 are as follows:

[0056] Ar1: Ar2: Ar3:

[0057] In the method for preparing fluorinated polyimide provided by the present invention, the molar ratio of H2N-Ar1-NH2 to H2N-Ar3-NH2 is preferably (1-10):1, specifically 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, 6.7:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9. .5:1 or 10:1; the molar ratio of H2N-Ar2-NH2 to H2N-Ar3-NH2 is preferably (1-10):1, specifically 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, 6.7:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1 or 10:1.

[0058] In the method for preparing fluorinated polyimide provided by the present invention, the molar ratio of the dianhydride monomer to the diamine monomer is preferably 1:(0.8-1.2), specifically 1:0.8, 1:0.85, 1:0.9, 1:0.95, 1:1, 1:1.0.5, 1:1.1, 1:1.15 or 1:1.2, and most preferably 1:1.

[0059] In the method for preparing fluorinated polyimide provided by the present invention, the inert gas includes but is not limited to nitrogen.

[0060] In the method for preparing fluorinated polyimide provided by the present invention, the catalyst is preferably one or more of pyridine, picoline, triethylamine, picolinoline and isoquinoline; the amount of the catalyst is preferably 3-7% of the molar amount of the dianhydride monomer, specifically 3%, 3.2%, 3.5%, 3.7%, 4%, 4.2%, 4.5%, 4.7%, 5%, 5.2%, 5.5%, 5.7%, 6%, 6.2%, 6.5%, 6.7% or 7%.

[0061] In the method for preparing fluorinated polyimide provided by the present invention, the solvent is a high boiling point solvent, including but not limited to one or more of phenol, polyhalogenated benzene, N-methylpyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAC) and dimethyl sulfoxide (DMSO), the phenol is preferably one or more of cresol, p-chlorophenol and m-cresol, the polyhalogenated benzene is preferably o-dichlorobenzene and / or 1,2,4-trichlorobenzene; the solvent is preferably N-methylpyrrolidone (NMP).

[0062] In the method for preparing the fluorinated polyimide provided by the present invention, in order to reduce the hydrolysis of the dianhydride monomer, the order of adding the monomers in the solvent is preferably to add the diamine first and then the dianhydride.

[0063] In the preparation method of fluorinated polyimide provided by the present invention, if a random copolymer is synthesized, the order of adding monomers in the solvent is to first add a diamine with lower reaction activity, then add a dianhydride, and finally add another diamine; if a block copolymer is synthesized, anhydride-terminated and amine-terminated oligomers are first synthesized at low temperature, respectively, and then the two oligomers are mixed to synthesize a polyimide solution at high temperature.

[0064] In the method for preparing the fluorinated polyimide provided by the present invention, in certain embodiments, the specific process of the copolymerization reaction preferably includes:

[0065] a) mixing a dianhydride monomer, a diamine monomer and a solvent under an inert gas atmosphere, and heating them to perform a preliminary reaction;

[0066] b) adding a catalyst to the reaction system of step a), then raising the temperature to continue the reaction, to obtain a fluorine-containing polyimide.

[0067] In the above-mentioned copolymerization process provided by the present invention, in step a), the heating temperature is preferably 80-100°C, specifically 80°C, 82°C, 85°C, 87°C, 90°C, 92°C, 95°C, 97°C or 100°C; the time of the preliminary reaction is preferably 2-6h, specifically 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h.

[0068] In the copolymerization process provided by the present invention, in step b), the terminal temperature of the heating is preferably 160-200°C, specifically 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C or 200°C; the reaction time is preferably 2-6h, specifically 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h.

[0069] In the copolymerization process provided by the present invention, after the copolymerization reaction is completed, the obtained reaction product liquid is poured into ethanol for precipitation, and the precipitate is washed and dried to obtain fluorinated polyimide powder.

[0070] The present invention also provides a fluorinated polyimide film, wherein the composition of the fluorinated polyimide film includes a fluorinated polyimide having a structure of formula (I) and / or formula (II);

[0071]

[0072] Where n1 and n2 represent the degree of polymerization, and the chemical structures of Ar1, Ar2 and Ar3 are as follows:

[0073] Ar1: Ar2: Ar3:

[0074] The present invention also provides a method for preparing a fluorinated polyimide film, comprising the following steps:

[0075] The casting solution is coated on a flat plate, and the temperature is increased to form a film to obtain a fluorinated polyimide film;

[0076] The casting solution contains a fluorinated polyimide having a structure of formula (I) and / or formula (II);

[0077]

[0078] Where n1 and n2 represent the degree of polymerization, and the chemical structures of Ar1, Ar2 and Ar3 are as follows:

[0079] Ar1: Ar2: Ar3:

[0080] In the film preparation method provided by the present invention, the content of the fluorinated polyimide in the casting solution is preferably 10 to 20 wt%, specifically 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%,

[0081] 16wt%, 17wt%, 18wt%, 19wt% or 20wt%.

[0082] In the thin film preparation method provided by the present invention, the solvent in the casting solution is preferably dimethylacetamide (DMAC).

[0083] In the thin film preparation method provided by the present invention, the material of the flat plate is preferably glass.

[0084] In the film preparation method provided by the present invention, the temperature rising method of the film forming is preferably gradient heating, the heating rate is preferably 3-7°C / min, and the film forming temperature range is preferably 60-270°C, more preferably 80-250°C.

[0085] In the thin film preparation method provided by the present invention, in some embodiments, the temperature rising procedure of the temperature rising film forming is specifically: firstly, the temperature is raised to the first temperature at a first heating rate and kept at the temperature for a first time; then, the temperature is raised to the second temperature at a second heating rate and kept at the temperature for a second time; then, the temperature is raised to the third temperature at a third heating rate and kept at the temperature for a third time; then, the temperature is raised to the fourth temperature at a fourth heating rate and kept at the temperature for a fourth time; then, the temperature is raised to the fifth temperature at a fifth heating rate and kept at the temperature for a fifth time; wherein, the first heating rate, the second heating rate, and the third heating rate are The first heating rate, the fourth heating rate and the fifth heating rate are independently selected to be 3-7°C / min, specifically 3°C / min, 4°C / min, 5°C / min, 6°C / min or 7°C / min; the first temperature is preferably 60-100°C, specifically 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C; the first time is preferably 1-3h, specifically 1h, 1.5h, 2h, 2.5h or 3h; the second temperature is preferably 100-14 0℃, specifically 100℃, 105℃, 110℃, 115℃, 120℃, 125℃, 130℃, 135℃ or 140℃; the second time is preferably 0.5-2h, specifically 0.5h, 1h, 1.5h or 2h; the third temperature is preferably 140-180℃, specifically 140℃, 145℃, 150℃, 155℃, 160℃, 165℃, 170℃, 175℃ or 180℃; the third time is preferably 0.5-2h, specifically 0.5h, 1h, 1.5h or 2h. 1h, 1.5h or 2h; the fourth temperature is preferably 180-220℃, specifically 180℃, 185℃, 190℃, 195℃, 200℃, 205℃, 210℃, 215℃ or 220℃; the fifth temperature is preferably 230-270℃, specifically 230℃, 235℃, 240℃, 245℃, 250℃, 255℃, 260℃, 265℃ or 270℃; the fifth time is preferably 0.5-2h, specifically 0.5h, 1h, 1.5h or 2h.

[0086] The technical solution provided by the present invention optimizes the molecular structure of polyimide and introduces fluorinated substituents, flexible chain forgings, alicyclic structures, asymmetric structures, bulky side groups and / or non-coplanar structures into the polyimide molecular chain, thereby improving the processing performance of polyimide, reducing the production cost of polyimide, and enabling the polyimide to have both excellent optical transparency and mechanical properties.

[0087] For the purpose of greater clarity, the invention is described in detail through the following examples.

[0088] Example 1

[0089] Dissolve 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFMB, corresponding to the diamine monomer H2N-Ar1-NH2 mentioned above) in NMP, then add 4,4'-(hexafluoroisopropylene) diphthalic anhydride (6FDA, corresponding to the dianhydride monomer of formula (i) mentioned above) in batches, and then add 4,4'-diaminodiphenyl ether (m-ODA, corresponding to the diamine monomer H2N-Ar3-NH2 mentioned above) to fully dissolve, keeping the total molar ratio of dianhydride monomer to diamine monomer at 1:1. Repeat the process. The entire three-necked flask reaction device is evacuated and filled with nitrogen, and the process is repeated at least 5 times; the temperature is raised to 90° C. and the reaction is carried out for 4 hours; according to the amount of isoquinoline being 5% of the molar number of the dianhydride monomer, isoquinoline is accurately measured with a pipette and slowly added into the reaction system, the temperature is raised to 180° C., and the reaction is continued for 4 hours; after the reaction is completed, the obtained polyimide solution is poured into excess ethanol for precipitation while hot, and the polyimide powder is continuously and vigorously stirred to obtain the polyimide powder; the precipitation is repeated 6 times, washed, and naturally air-dried to obtain a fluorine-containing polyimide powder having a structure of formula (I), which is recorded as I-PI.

[0090] The above-mentioned I-PI powder was dissolved in DMAc to prepare a polyimide solution with a solid content of 15wt%, filtered with a 0.2mm Teflon syringe, evenly coated on a glass plate, and filmed at a gradient heating rate of 5℃ / min. The heating program was: 80℃ / 2h, 120℃ / 1h, 160℃ / 1h, 200℃ / 1h, 250℃ / 1h.

[0091] In this embodiment, by adjusting the molar ratio of the two diamine monomers TFMB and m-ODA, I-PIs with different structures can be obtained. The specific adjustment is shown in Table 1:

[0092] Table 1 Diamine monomer composition of prepared I-PI copolymer polyimide

[0093] TFMB:m-ODA (molar ratio) I-PI(number) 18:2 I-PI10 14:6 I-PI30 10:10 I-PI50

[0094] Example 2

[0095] Dissolve 4,4'-diaminobenzanilide (DABA, corresponding to the diamine monomer H2N-Ar2-NH2 in the previous text) in NMP, then add 4,4'-(hexafluoroisopropylene) diphthalic anhydride (6FDA, corresponding to the dianhydride monomer of formula (i) in the previous text) in batches, and then add 4,4'-diaminodiphenyl ether (m-ODA, corresponding to the diamine monomer H2N-Ar3-NH2 in the previous text) to fully dissolve, keep the total molar ratio of dianhydride monomer to diamine monomer at 1:1, and repeatedly burn the entire three-mouth furnace in this process. The reaction device in the bottle is evacuated and filled with nitrogen, and the process is repeated at least 5 times; the temperature is raised to 90° C. and the reaction is carried out for 4 hours; according to the amount of isoquinoline being 5% of the molar number of the dianhydride monomer, isoquinoline is accurately measured with a pipette and slowly added into the reaction system, the temperature is raised to 180° C. and the reaction is continued for 4 hours; after the reaction is completed, the obtained polyimide solution is poured into excess ethanol for precipitation while hot, and the polyimide powder is continuously and vigorously stirred to obtain the polyimide powder; the precipitation is repeated 6 times, washed, and naturally air-dried to obtain a fluorine-containing polyimide powder having a structure of formula (II), which is recorded as II-PI.

[0096] The above II-PI powder was dissolved in DMAc to prepare a polyimide solution with a solid content of 15 wt%, filtered with a 0.2 mm Teflon syringe, evenly coated on a glass plate, and filmed at a gradient heating rate of 5 °C / min. The heating program was: 80 °C / 2h, 120 °C / 1h, 160 °C / 1h, 200 °C / 1h, 250 °C / 1h.

[0097] In this embodiment, by adjusting the molar ratio of the two diamine monomers DABA and m-ODA, II-PI with different structures can be obtained. The specific adjustment is shown in Table 2:

[0098] Table 2 Diamine monomer composition of prepared II-PI copolymer polyimide

[0099] DABA:m-ODA (molar ratio) II-PI(number) 18:2 II-PI10 14:6 II-PI30 10:10 II-PI50

[0100] Performance Evaluation

[0101] (1) The mechanical properties of I-PI and II-PI copolymer polyimide films are shown in Table 3:

[0102] Table 3 Mechanical properties of I-PI and II-PI copolymer polyimide films

[0103] Polyimide Tensile strength / MPa Elastic modulus / GPa Elongation at break / % I-PI10 130.6 1.4 5.4 I-PI30 145.5 1.0 6.4 I-PI50 163.3 0.7 10.9 II-PI10 178.1 0.7 8.0 II-PI20 189.4 0.5 10.5 II-PI30 199.0 0.3 13.8

[0104] Polyimide film is a molecular solid, and its mechanical properties mainly come from the destruction of secondary bonds (van der Waals forces or hydrogen bonds between molecular chains) and the breaking of chemical bonds within some molecular chains.

[0105] TFMB in the I-PI series of polyimides is a trifluoromethyl-containing biphenyl structure, which can provide strong rigidity for the molecular chain, making the elastic modulus of the polymer higher; it can also reduce the packing density of the molecular chain, thereby having a negative impact on the compactness, regularity and orientation of the molecular chain. 6FDA and m-ODA are flexible components that can improve the interchain entanglement of the polymer molecular chain, thereby increasing the elongation at break.

[0106] DABA and m-ODA in the II-PI series polyimide contain electron-rich groups, which improve the charge transfer complexation within / between the molecular chains and increase the secondary bond force of the molecular chains; secondly, the presence of linear DABA makes the molecular chain tightness, molecular chain regularity and orientation of the II-PI series film very high. Therefore, DABA improves the tensile strength of the II-PI series film. In addition, the amide bridging bond in DABA is not very rigid, which makes the elastic modulus of the II-PI series polyimide low. In the II-PI series polyimide, 6FDA, DABA and m-ODA all contain flexible components, that is, the II-PI series polyimide has more flexible components than the I-PI series polyimide, which can better improve the molecular chain entanglement of the polymer, thereby making the elongation at break greater.

[0107] (2) The optical transparency of I-PI and II-PI copolymerized polyimide films is shown in Table 4:

[0108] Table 4 Optical transparency of I-PI and II-PI copolymer polyimide films

[0109] Polyimide transparency(%) I-PI10 ≥85 I-PI30 ≥86 I-PI50 ≥88 II-PI10 ≥68 II-PI20 ≥73 II-PI30 ≥75

[0110] Generally, the degree of transparency is related to the charge transfer complex effect generated within or between polyimide chains. Traditional aromatic polyimides are generally polymerized from diamines with strong electron-donating ability and dianhydrides with strong electron-accepting ability. The polymer molecular chains are closely arranged, and there are strong interactions between aromatic rings. The electronic polarization rate of trifluoromethyl is very low, which can significantly reduce the CTC effect in polyimide molecules, resulting in low transmittance in the visible light range and improved light transmittance. At the same time, the ether bond in the I-PI system is a hydrophilic group, which increases the surface energy of the polyimide and can reduce the hydrophobicity of the I-PI system.

[0111] Transparency is related to the fluorine functional groups in the polymer chain. Therefore, the I-PI system contains more trifluoromethyl groups than the II-PI system, which makes the polyimide molecular chain bend and twist, hindering the flow of electron transfer complexes along the molecular chain, thereby reducing the CTC effect within the molecule and improving the optical transparency of the polyimide film.

[0112] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A fluorinated polyimide, characterized in that: Having the structure of formula (I) or formula (II): Where n1 and n2 represent the degree of polymerization, and the chemical structures of Ar1, Ar2 and Ar3 are as follows: Ar1: Ar2: Ar3:

2. A method for preparing a fluorinated polyimide, characterized in that: The following steps are involved: In the presence of an inert gas and a catalyst, the dianhydride monomer and the diamine monomer undergo a copolymerization reaction in a solvent to obtain a fluorinated polyimide; The dianhydride monomer has the structure of formula (i): The diamine monomers are H2N-Ar1-NH2 and H2N-Ar3-NH2, or H2N-Ar2-NH2 and H2N-Ar3-NH2; If the diamine monomers are H2N-Ar1-NH2 and H2N-Ar3-NH2, the fluorinated polyimide has a structure of formula (I): If the diamine monomers are H2N-Ar2-NH2 and H2N-Ar3-NH2, the fluorinated polyimide has a structure of formula (II); Where n1 and n2 represent the degree of polymerization, and the chemical structures of Ar1, Ar2 and Ar3 are as follows: Ar1: Ar2: Ar3:

3. The preparation method according to claim 2, characterized in that: The molar ratio of the H2N-Ar1-NH2 to the H2N-Ar3-NH2 is (1-10):1; the molar ratio of the H2N-Ar2-NH2 to the H2N-Ar3-NH2 is (1-10):

1.

4. The preparation method according to claim 2, characterized in that: The molar ratio of the dianhydride monomer to the diamine monomer is 1:(0.8-1.2).

5. The preparation method according to claim 2, characterized in that: The catalyst is one or more of pyridine, picoline, triethylamine, picolinoline and isoquinoline; the amount of the catalyst is 3-7% of the molar amount of the dianhydride monomer.

6. The preparation method according to claim 2, characterized in that: The specific process of the copolymerization reaction includes: a) mixing a dianhydride monomer, a diamine monomer and a solvent under an inert gas atmosphere, and heating them to perform a preliminary reaction; b) adding a catalyst to the reaction system of step a), then raising the temperature to continue the reaction, to obtain a fluorine-containing polyimide.

7. The preparation method according to claim 6, characterized in that: In step a), the heating temperature is 80-100° C., and the initial reaction time is 2-6 hours; in step b), the terminal temperature of the heating is 160-200° C., and the reaction time is 2-6 hours.

8. A fluorinated polyimide film, characterized in that: The composition of the fluorinated polyimide film includes fluorinated polyimide of formula (I) and / or formula (II); Where n1 and n2 represent the degree of polymerization, and the chemical structures of Ar1, Ar2 and Ar3 are as follows: Ar1: Ar2: Ar3:

9. A method for preparing a fluorinated polyimide film, characterized in that: The following steps are involved: The casting solution is coated on a flat plate, and the temperature is increased to form a film to obtain a fluorinated polyimide film; The casting solution contains a fluorinated polyimide having a structure of formula (I) and / or formula (II); Where n1 and n2 represent the degree of polymerization, and the chemical structures of Ar1, Ar2 and Ar3 are as follows: Ar1: Ar2: Ar3:

10. The preparation method according to claim 9, characterized in that: The temperature rise method of the film formation is gradient temperature rise, and the film formation temperature range is 60 to 270°C.

Citation Information

Patent Citations

  • Fluorine-containing alicyclic copolymerized polyimide film material and preparation method thereof

    CN110183851A

  • Transparent polyimide film

    CN111205642A

  • Low-thermal-expansion transparent polyimide film and preparation method thereof

    CN112194790A

  • Polyimide film with low expansion coefficient and preparation method

    CN113845674A

  • Preparation method of high-transparency low-yellowing high-performance polyamide acid resin and polyimide film

    CN116925352A