Phosphorus-containing polysiloxane reactive flame retardant as well as preparation method and application thereof

By preparing cyclic siloxane with active groups and reacting with bifunctional compounds, grafting phosphorus-containing compounds to synthesize reactive phosphorus-containing polysiloxane flame retardants solves the problems of flammability and poor compatibility of polymer materials. , achieving efficient flame retardant and droplet resistance properties and meeting environmental protection requirements.

CN118772414AInactive Publication Date: 2024-10-15BEIJING UNIV OF CHEM TECH

Patent Information

Application Number
CN202310372018.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing polymer materials are flammable, and existing flame retardants in the materials have poor compatibility and are easy to migrate, affecting the mechanical properties of the base material, making it difficult to effectively improve its flame retardancy and droplet resistance.

Method used

By preparing cyclic siloxane with new active groups and reacting with bifunctional compounds, the molecular weight and active group content of polysiloxane are controlled, and the phosphorus-containing compound is grafted to synthesize reactive phosphorus-containing polysiloxane barrier. Flame retardant forms a network structure to enhance the flame retardancy and droplet resistance of the base material.

Benefits of technology

It achieves efficient flame retardant effect and droplet resistance without affecting the mechanical properties of the base material. It is in line with the development trend of halogen-free and does not produce toxic gases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772414A_ABST
    Figure CN118772414A_ABST
Patent Text Reader

Abstract

The invention provides a phosphorus-containing polysiloxane reactive flame retardant as well as a preparation method and application thereof. The phosphorus-containing polysiloxane reactive flame retardant is prepared from the following raw materials: cyclic active siloxane 1, a catalyst 1, a bifunctional compound, cyclic inactive siloxane, a catalyst 2, an end-capping reagent, a phosphorus-containing substance and a catalyst 3. The preparation method comprises the following steps: reacting cyclic active siloxane 1 with a bifunctional compound in the presence of a catalyst 1 to obtain cyclic active siloxane 2, performing ring-opening copolymerization on the cyclic active siloxane 2, cyclic inactive siloxane and an end-capping reagent in the presence of a catalyst 2 to obtain linear or linear ring-shaped active polysiloxane 3, and performing ring-opening copolymerization on the linear or linear ring-shaped active polysiloxane 3. And finally reacting with a phosphorus-containing substance in the presence of a catalyst 3 to obtain the phosphorus-containing polysiloxane reactive flame retardant. The flame retardant has a phosphorus-containing structure, the content of active groups is controllable, the flame retardant effect and the anti-dripping effect are good, toxic gas is not generated after high-temperature combustion, and the halogen-free development trend of the flame retardant is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flame retardants, and more particularly to a phosphorus-containing polysiloxane reactive flame retardant and a preparation method and application thereof. Background Art

[0002] Polymer materials are used in all aspects of life, but most polymer materials are flammable and pose a danger to people's lives. Some polymer materials can also cause fires due to severe droplets, which limits their application in industries with high flame retardancy requirements. Therefore, it is necessary to make polymer materials flame retardant, and polymer materials with severe droplets need to be made anti-droplet to expand their application range.

[0003] With the trend of halogen-free, environmentally friendly flame retardants have received extensive attention, especially phosphorus-containing and silicon-containing compounds. Phosphorus-containing compounds have a highly efficient flame retardant effect, but there are problems such as poor material compatibility, easy migration, and easy hydrolysis. These problems will seriously affect the mechanical properties of the base material, thereby affecting the use of the base material; polysiloxane in the silicon-based flame retardant has good anti-dripping, low smoke and heat resistance. When it is used in polymers, it can enhance the melt viscosity of the polymer, and can form a silicon dioxide carbon layer when burned at high temperature, and can also increase the melt viscosity of the polymer, so that the polymer can support its own weight without producing droplets. Therefore, polysiloxane has excellent anti-droplet and flame retardant effects on polymers with severe droplets. In addition to the high flame retardancy of phosphorus compounds, phosphorus and silicon compounds work together to play a synergistic flame retardant role, which can effectively improve the flame retardancy of polymer materials.

[0004] At present, there are two main ways to introduce flame retardants into polymers. One is an additive flame retardant, which is physically combined with the matrix polymer and requires a large amount of usage to achieve a flame retardant effect. There are problems such as poor compatibility with the matrix, which will seriously affect the mechanical properties of the polymer. The other is a reactive flame retardant, which is prepared by grafting onto the polymer chain through a chemical reaction, and then the flame retardant is fixed in the molecular structure of the matrix material through a reaction. The flame retardant molecules are not easy to migrate, not only does it not cause the problem of poor compatibility with the matrix, but it can also increase the melt viscosity of the polymer, solving the problem of affecting the mechanical properties of the polymer, while improving the flame retardancy of the polymer.

[0005] The existing technology mainly prepares phosphorus-containing polysiloxane flame retardants by grafting active polysiloxane with phosphorus-containing substances. The flame retardants prepared by this method have a fixed molecular weight and a fixed phosphorus-containing group ratio. At the same time, since polysiloxane raw materials are easily available, researchers mostly directly use polysiloxane as a raw material to prepare flame retardants. The molecular weight, viscosity and active group content are restricted by manufacturers, and the controllability of the product is poor.

[0006] Therefore, it is necessary to prepare a cyclic siloxane with a new active group with controllable structure, in which the molecular weight and active group content can be controlled, prepare the active polysiloxane by ring-opening polymerization, and then graft phosphorus-containing compounds to synthesize a reactive phosphorus-containing polysiloxane flame retardant. The proportion of the phosphorus-containing compound that can be grafted depends on the structure of the ring-opening product, so that the structure of the final product of the grafted phosphorus-containing compound is controlled. Summary of the invention

[0007] In order to solve the technical problems existing in the prior art, the present invention provides a phosphorus-containing polysiloxane reactive flame retardant and a preparation method and application thereof.

[0008] The present invention uses cyclic active siloxane and bifunctional compound as monomers, and under the action of a catalyst, a cyclic siloxane with a new active group is prepared by reaction; the cyclic active siloxane is copolymerized with an inactive polysiloxane to prepare a linear or linear ring polysiloxane, which contains a variety of side groups and has good temperature resistance; finally, the active side groups are reacted with a phosphorus-containing compound to prepare a phosphorus-containing polysiloxane. The cyclic siloxane prepared by the reaction of the cyclic active siloxane with the bifunctional compound has a new active group, and the molecular weight and active group content of the polysiloxane can be controlled by ring-opening polymerization and ring-opening copolymerization, thereby determining the proportion of the phosphorus-containing substance that can be grafted. Therefore, the designed phosphorus-containing polysiloxane flame retardant can be obtained by controlling the feed ratio, and the flame retardant can give full play to the synergistic flame retardant effect of silicon and phosphorus elements. The polysiloxane will form SiO at high temperature. 2 It migrates to the surface of the substrate, enhances the melt viscosity of the substrate material, and the phosphorus-containing compound forms polyphosphoric acid when heated. The polyphosphoric acid is dehydrated to form an inorganic carbon layer, which blocks material exchange and heat exchange, achieving better flame retardant and anti-melting droplet effects. The reactivity of the flame retardant ensures that it can react with the substrate to form a network structure, thereby having little effect on the mechanical properties of the substrate.

[0009] Compared with the prior art, the phosphorus-containing structure and active group content of the phosphorus-containing polysiloxane reactive flame retardant provided by the present invention can be controlled, and the obtained flame retardant has the characteristics of anti-dripping, low smoke and heat resistance of polysiloxane, and has the high flame retardancy of phosphorus-containing compounds, giving full play to the synergistic flame retardant effect of silicon and phosphorus elements, and the designed flame retardant is grafted onto the molecular structure of the base material through a chemical reaction, and the flame retardant molecules do not migrate, so the mechanical properties of the base material are less affected, and the anti-melting dripping property of the base material is increased, and the designed and synthesized flame retardant contains two elements of phosphorus and silicon, and does not produce toxic gas after high-temperature combustion, which is in line with the development trend of halogen-free flame retardants.

[0010] One of the purposes of the present invention is to provide a phosphorus-containing polysiloxane reactive flame retardant.

[0011] The phosphorus-containing polysiloxane reactive flame retardant is prepared from raw materials including cyclic active siloxane 1, catalyst 1, bifunctional compound, cyclic inactive siloxane, catalyst 2, end-capping agent, phosphorus-containing substance and catalyst 3.

[0012] In a preferred embodiment of the present invention,

[0013] The structure of the cyclic active siloxane 1 is:

[0014]

[0015] Where: 6≥m+n≥3, m and n are integers greater than or equal to 0, and m and n cannot be 0 at the same time;

[0016] R 1 , R 2 , R 3 , R 4 are independently selected from one of hydrogen, hydroxyl, amino, vinyl, epoxy, methyl, alkoxy, phenyl, and phenoxy, and R 1 , R 2 , R 3 , R 4 At least one of them is an active group, and the active group is a hydrogen atom, a hydroxyl group, an amino group, a vinyl group or an epoxy group;

[0017] The bifunctional compound is at least one of allyl glycidyl ether, allyl alcohol, methallyl alcohol, eugenol, allylamine, N-methylallylamine, 3-allyl bromide, 3-allyl chloride, 3-bromo-2-methylpropene, and 3-chloro-2-methylpropene; preferably at least one of allyl glycidyl ether, methallyl alcohol, and eugenol;

[0018] The catalyst 1 is a transition metal catalyst, preferably at least one of platinum, palladium, rhodium and nickel catalysts; more preferably a platinum catalyst.

[0019] In a preferred embodiment of the present invention,

[0020] The structural formula of the cyclic inactive siloxane is:

[0021]

[0022] Where: 6≥p+q≥3, p and q are integers greater than or equal to 0, and p and q cannot be 0 at the same time; R 5 , R 6 , R 7 , R 8 Each independently selected from methyl, ethyl and phenyl;

[0023] The catalyst 2 is LiOH, NaOH, KOH and its silicon alkoxide, methyl lithium, ethyl lithium, propyl lithium, n-butyl lithium, phenyl lithium, tetramethylammonium hydroxide, tetramethylammonium hydroxide silicon alkoxide, tetrabutylphosphonium hydroxide silicon alkoxide, Et 4 NOH、Bu 4 At least one of POH, linear phosphazene chloride; preferably Et 4 At least one of NOH and tetramethylammonium hydroxide;

[0024] The end-capping agent is hexamethyldisiloxane, 1,1,3,3-tetramethyldisiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(3-epoxy)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(3-hydroxypropyl)-1,1,3,3-tetramethyldisiloxane, methanol, ethanol, water, small molecule hydroxy silicone oil, small molecule amino silicone oil, trimethylsilanol, dimethylchlorosilane, trimethylmonochlorosilane, triethylmonochlorosilane, trimethylmethoxysilane, 3,3'-dithiodipropionic acid; preferably hexamethyldisiloxane, 1,1,3,3-tetramethyldi At least one of siloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(3-glycidyloxy)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(3-hydroxypropyl)-1,1,3,3-tetramethyldisiloxane, and 1,3-divinyl-1,1,3,3-tetramethyldisiloxane; the small molecule hydroxy silicone oil is preferably at least one of terminal hydroxy silicone oil, terminal hydroxypropyl silicone oil, side hydroxy silicone oil, and side hydroxypropyl silicone oil; the small molecule amino silicone oil is preferably at least one of terminal amino silicone oil, terminal aminopropyl silicone oil, side amino silicone oil, and side aminopropyl silicone oil;

[0025] The phosphorus-containing substance is a compound containing an active PH bond, preferably 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO). diphenylphosphine oxide diphenylphosphine Dimethyl phosphite Diethyl phosphite Dibutyl phosphite Phenylphosphonic acid Phosphorous acid Hypophosphorous acid 5,5-Dimethyl-1,3,2-dioxaphosphine 2-oxide Phosphorolane Phosphorinane 2-Hydrogen-2-oxygen-1,3,2-oxazaphosphorolane 5,10-Dihydro-phosphazine-10-oxide At least one of;

[0026] The catalyst 3 is at least one of triphenylphosphine, tributylphosphine, tri-tert-butylphosphine, azobisisobutyronitrile, organic tin compounds, and phosphazene catalysts; preferably at least one of triphenylphosphine and azobisisobutyronitrile; the organic tin compound is preferably Bu 2 SnO、Bu 3 SnCl、Ph 3 At least one of SnCl.

[0027] The second object of the present invention is to provide a method for preparing a phosphorus-containing polysiloxane reactive flame retardant, comprising the following steps:

[0028] (1) reacting the cyclic active siloxane 1 with the bifunctional compound in the presence of the catalyst 1 to obtain the cyclic active siloxane 2;

[0029] (2) subjecting the cyclic active siloxane 2 obtained in step (1) to a ring-opening copolymerization reaction with the cyclic inactive siloxane and the end-capping agent in the presence of the catalyst 2 to obtain a linear or linear annular active polysiloxane 3;

[0030] (3) reacting the linear or linear ring-shaped active polysiloxane 3 obtained in step (2) with the phosphorus-containing substance in the presence of a catalyst 3 to obtain the phosphorus-containing polysiloxane reactive flame retardant.

[0031] Step (1) prepares a cyclic siloxane 2 with a new active group; step (2) prepares a linear or linear ring polysiloxane containing a variety of side groups and having good temperature resistance;

[0032] The linear or linear cyclic active polysiloxane 3 obtained in step (2) means that the polysiloxane obtained by the reaction has two forms: one is a completely open-ring linear structure, which is a linear active polysiloxane 3; the other is a partially open-ring, partially unopened linear cyclic structure, which is a linear cyclic active polysiloxane 3. The conditions that affect the ratio of the two structures are: the size of the cyclosiloxane ring D 3 >D 4 >D 5 >D 6 , D 3 The larger the ring tension, the easier it is to open the ring, and the easier it is to obtain a linear structure; the cyclosiloxane substituents Me>Et>Ph>phenoxy, the larger the substituent, the more difficult it is to open the ring, and a linear ring structure exists; when the reaction temperature is 90-120°C, cyclosiloxanes whose substituents are hydrogen atoms, hydroxyl groups, amino groups, vinyl groups, epoxy groups, methyl groups, and alkoxy groups can open the ring, and when the reaction temperature is 130-180°C, cyclosiloxanes whose substituents are phenyl groups and phenoxy groups can open the ring. When there are two or more cyclosiloxanes, controlling the reaction temperature can control the existence form of the polysiloxane obtained by the reaction.

[0033] In a preferred embodiment of the present invention,

[0034] Step (1), slowly adding an excess of the bifunctional compound to a mixed solution of the cyclic active siloxane 1 and the catalyst for reaction, and then removing the excess of the bifunctional compound; and / or,

[0035] Step (2), heating the cyclic active siloxane 2, the cyclic inactive siloxane, the catalyst 2 and the end-capping agent to carry out a ring-opening polymerization reaction, then heating the catalyst 2 to decompose the catalyst 2, and rotary evaporating to remove small molecular substances.

[0036] In a preferred embodiment of the present invention,

[0037] Step (1),

[0038] The molar ratio of the Si-H group of the cyclic active siloxane 1 to the C=C double bond group of the bifunctional compound is 1:(1.1-2.0), preferably 1:(1.1-1.8);

[0039] The amount of the catalyst 1 is 0.005 to 0.02 times the total mass of the reactants in step (1), preferably 0.01 to 0.02 times the total mass of the reactants in step (1);

[0040] Step (2),

[0041] The molar ratio of the cyclic inactive siloxane to the cyclic active siloxane 2 is 1:(1-10), preferably 1:(1-5);

[0042] The molar ratio of the catalyst 2 to the cyclic active siloxane 2 is 1:(1-10 5 ), preferably 1: (60-110);

[0043] The molar ratio of the cyclic active siloxane 2 to the end-capping agent is 1:(10 -3 ~10 4 ); preferably 1:(10 -1 ~1);

[0044] The molecular weight of the linear or linear annular active polysiloxane 3 is 500 to 20,000, preferably 1,000 to 5,000;

[0045] Step (3),

[0046] The molar ratio of the linear or linear annular active polysiloxane 3 to the phosphorus-containing substance is 1:(1-30), preferably 1:(4-16);

[0047] The amount of the catalyst 3 used is 0.005 to 0.01 times the total mass of the reactants in step (3), preferably 0.005 to 0.008 times the total mass of the reactants in step (3).

[0048] In a preferred embodiment of the present invention,

[0049] Step (1),

[0050] Reaction temperature: 25-120°C, preferably 65-90°C; and / or,

[0051] Reaction time: 1 to 12 hours, preferably 8 to 12 hours; and / or,

[0052] Step (2),

[0053] The reaction temperature is 60 to 120°C, preferably 90 to 120°C; and / or,

[0054] The reaction time is 1 to 12 hours; preferably 4 to 8 hours; and / or,

[0055] Step (3),

[0056] The reaction temperature is 130 to 200°C, preferably 130 to 180°C; and / or,

[0057] The reaction time is 10 to 48 hours, preferably 12 to 24 hours.

[0058] In a preferred embodiment of the present invention,

[0059] Step (2),

[0060] The decomposition catalyst temperature is 130 to 180°C, preferably 130 to 150°C.

[0061] The third object of the present invention is to provide a phosphorus-containing polysiloxane reactive flame retardant obtained by the above preparation method, wherein the molecular weight of the phosphorus-containing polysiloxane reactive flame retardant is 1000-30000, preferably 2000-8000.

[0062] A fourth object of the present invention is to provide an application of a phosphorus-containing polysiloxane reactive flame retardant in a matrix material, preferably in polyurea, polyurethane or epoxy.

[0063] Compared with the prior art, the present invention has the following beneficial effects:

[0064] The present invention prepares cyclic siloxane with new active groups by reacting cyclic active siloxane with a bifunctional compound, and then prepares linear or linear annular active polysiloxane by a ring-opening polymerization equilibrium reaction. The molecular weight and active group content of the active polysiloxane can be controlled by the ring-opening polymerization reaction, and finally a phosphorus-containing compound is grafted to synthesize a phosphorus-containing polysiloxane reactive flame retardant. The flame retardant has the characteristics of low smoke and heat resistance of polysiloxane, and the high flame retardancy of the phosphorus-containing compound, and gives full play to the synergistic flame retardancy of silicon and phosphorus elements, and has a high flame retardant effect and an excellent anti-melting dripping effect.

[0065] The reactive polysiloxane designed and synthesized by the present invention is a polysiloxane of a new structure, which has good reactivity and flame retardancy. Theoretically, the higher the proportion of phosphorus-containing substances grafted to the flame retardant, the better the flame retardant effect of the flame retardant. Therefore, the polysiloxane flame retardant with a high phosphorus content can be controlled and synthesized to achieve a high flame retardancy effect. The oxygen index of the phosphorus-containing polysiloxane reactive flame retardant synthesized in the embodiment of the present invention can reach up to 34.6%, which is a flame retardant grade and has an excellent flame retardant effect.

[0066] The phosphorus-containing polysiloxane reactive flame retardant provided by the present invention can react with the base material, thereby bonding to the structural network of the base material, so that it has little effect on the mechanical properties of the base material, and has an anti-melting droplet effect, and can also play a flame retardant role on the base material with serious melting droplets. In addition, the phosphorus-containing polysiloxane reactive flame retardant does not contain halogen elements, and does not produce toxic and harmful gases to cause environmental pollution when heated and burned. It is an environmentally friendly flame retardant and conforms to the development trend of non-halogenated flame retardants.

[0067] The active polysiloxane prepared by the present invention is used as a raw material to participate in the synthesis of polycarbonate to prepare transparent, intrinsically flame-retardant polycarbonate. BRIEF DESCRIPTION OF THE DRAWINGS

[0068] Figure 1 is the infrared spectrum of the active cyclic siloxane 2 prepared in Example 1;

[0069] Figure 2 This is the infrared spectrum of the active linear siloxane 3 prepared in Example 1;

[0070] Figure 3 This is the infrared spectrum of the phosphorus-containing polysiloxane reactive flame retardant prepared in Example 1. DETAILED DESCRIPTION

[0071] The present invention is described in detail below in conjunction with specific drawings and embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.

[0072] The raw materials used in the examples are all conventional commercially available raw materials;

[0073] Test methods and related standards in the embodiments:

[0074] Limiting oxygen index standard: Test specimen: length × width × thickness = 100mm × 6.5mm × 3mm; The limiting oxygen index test is carried out according to GB / T 2406-2009, and the instrument used is the limiting oxygen index tester of Suzhou Testtech Testing Instrument Technology Co., Ltd.;

[0075] Vertical combustion standard: Test specimen: length × width × thickness = 130mm × 13mm × 3mm; vertical combustion test is carried out according to GB / T2408-1996, and the instrument used is GF Z-6 vertical combustion instrument of Nanjing Jiangning Analytical Instrument Factory;

[0076] Viscosity standard: Test sample amount: about 30g; the viscosity test is carried out according to GB / T 10247-2008, and the instrument used is the BROOKFIELD rotational viscometer of Brookfield Company of the United States.

[0077] Example 1

[0078] 1. Preparation of cyclic reactive siloxane:

[0079] Weigh 0.083 mol (19.96 g) of 1,3,5,7-tetramethylcyclotetrasiloxane and 0.88 g of platinum catalyst into a dry three-necked flask, weigh 0.598 mol (68.26 g) of allyl glycidyl ether into a dry dropping funnel, add a magnetic particle, condense and reflux at 90°C, slowly drop allyl glycidyl ether, react after the addition is complete, the reaction time is about 12 hours, and after the reaction, remove the excess allyl glycidyl ether by rotary evaporation to obtain the active cyclic siloxane tetramethyl-tetra-γ-glycidyl ether oxypropylcyclotetrasiloxane. The infrared spectrum is shown in the figure below. Figure 1 shown.

[0080] 2. Preparation of linear or linear ring active polysiloxane:

[0081] Weigh 0.029 mol (20.22 g) of tetramethyl-tetra-γ-glycidyloxypropylcyclotetrasiloxane and 0.029 mol (23.00 g) of octaphenylcyclotetrasiloxane in a dry three-necked flask, add a magnetic particle and condense and reflux at 120°C, weigh 0.029 mol (4.71 g) of hexamethyldisiloxane and 0.47 mmol (0.043 g) of tetramethylammonium hydroxide (TMAH), react for about 8 hours, heat to 150°C and stir for 30 minutes to decompose the catalyst, then remove the small molecular substances generated by the reaction by rotary evaporation at 150°C to obtain the open-loop linear active polysiloxane product. The viscosity, molecular weight and color state of the open-loop product are statistically shown in Table 1. The infrared spectrum is shown in Figure 1. Figure 2 shown.

[0082] 3. Preparation of phosphorus-containing polysiloxane reactive flame retardant:

[0083] Weigh 6.02 mmol (10.00 g) of the above-prepared ring-opening product and 0.024 mol DOPO (5.19 g) into a dry single-mouth bottle, heat to 130°C, condense and reflux until DOPO is completely melted, add 0.29 mmol (0.076 g) of triphenylphosphine, and continue the reaction for about 12 hours to obtain the final product, phosphorus-containing polysiloxane reactive flame retardant. The infrared spectrum is shown in the figure below. Figure 3 shown.

[0084] Figure 1 Medium, 1047cm -1 The Si-O-Si characteristic absorption peak is at 908cm -1 The characteristic absorption peak of epoxy is 2160cm -1 The characteristic absorption peak of Si-H bond disappears at 1659cm -1 The disappearance of the characteristic absorption peak of C=C double bond proves the successful progress of the reaction.

[0085] Figure 2 Medium, 1591cm -1 The characteristic absorption peak of benzene ring is 908cm -1 The characteristic absorption peak of epoxy is 1058cm -1 、1017cm -1 The characteristic absorption peak of Si-O-Si is split into two peaks, which proves the successful occurrence of the ring-opening reaction.

[0086] Figure 3 Medium, 1058cm -1 、1017cm -1 The characteristic absorption peak of Si-O-Si is 1218 cm -1 The characteristic absorption peak of P=O double bond is 904cm -1The characteristic absorption peak of PO-Ph is 2436cm -1 The characteristic absorption peak of the PH bond disappeared, proving the successful occurrence of the reaction.

[0087] The prepared flame retardant was added to E51 epoxy resin cured by diaminodiphenylmethane (DDM) curing agent, and the flame retardant accounted for 8% of the total mass of the system. The flame retardant performance test results are shown in Table 2.

[0088] The prepared flame retardant was added to polyurea, and the flame retardant accounted for 5% of the total mass of the system. The flame retardant performance test results are shown in Table 2.

[0089] Example 2

[0090] 1. Preparation of cyclic reactive siloxane: same as in Example 1;

[0091] 2. Preparation of linear or linear ring active polysiloxane:

[0092] Weigh 0.029mol (20.22g) of tetramethyl-tetra-γ-glycidyloxypropylcyclotetrasiloxane and 0.0145mol (11.50g) of octaphenylcyclotetrasiloxane in a dry three-necked flask, add a magnetic particle and condense and reflux at 120°C, weigh 0.0145mol (2.35g) of hexamethyldisiloxane and 0.35mmol (0.032g) of tetramethylammonium hydroxide (TMAH), react for about 8h, heat to 150°C and stir for 30min to decompose the catalyst, then remove the small molecular substances generated by the reaction by rotary evaporation at 150°C to obtain the ring-opening product. The viscosity, molecular weight and color state of the ring-opening product are statistically shown in Table 1.

[0093] 3. Preparation of phosphorus-containing polysiloxane reactive flame retardant:

[0094] Weigh 4.25 mmol (10.00 g) of the above-prepared ring-opening product and 0.017 mol (3.67 g) of DOPO in a dry single-mouth bottle, heat to 130°C, condense and reflux until DOPO is completely melted, add 0.26 mmol (0.068 g) of triphenylphosphine, and continue the reaction for about 12 hours to obtain the final product, reactive phosphorus-containing polysiloxane. The prepared flame retardant is added to the E51 epoxy resin cured by DDM, and the flame retardant accounts for 8% of the total mass of the system. The flame retardant test results are shown in Table 2.

[0095] Example 3

[0096] 1. Preparation of cyclic reactive siloxane: same as in Example 1;

[0097] 2. Preparation of linear or linear ring active polysiloxane:

[0098] Weigh 0.036mol (25.10g) of tetramethyl-tetra-γ-glycidyloxypropylcyclotetrasiloxane and 0.012mol (9.52g) of octaphenylcyclotetrasiloxane in a dry three-necked flask, add a magnetic particle and condense and reflux at 120°C, weigh 0.0120mol (1.95g) of hexamethyldisiloxane and 0.38mmol (0.035g) of tetramethylammonium hydroxide (TMAH), react for about 8h, heat to 150°C and stir for 30min to decompose the catalyst, then remove the small molecular substances generated by the reaction by rotary evaporation at 150°C to obtain the ring-opening product. The viscosity, molecular weight and color state of the ring-opening product are statistically shown in Table 1.

[0099] 3. Preparation of phosphorus-containing polysiloxane reactive flame retardant:

[0100] Weigh 3.28 mmol (10.00 g) of the above-prepared ring-opening product and 0.020 mol (4.32 g) of DOPO into a dry single-necked bottle, heat to 130° C., condense and reflux until DOPO is completely melted, add 0.42 mmol (0.11 g) of triphenylphosphine, and continue the reaction for about 12 h to obtain the final product, phosphorus-containing polysiloxane reactive flame retardant.

[0101] The prepared flame retardant was added to the E51 epoxy resin cured by DDM, and the flame retardant accounted for 8% of the total mass of the system. The flame retardant performance test results are shown in Table 2.

[0102] Example 4

[0103] 1. Preparation of cyclic reactive siloxane: same as in Example 1;

[0104] 2. Preparation of linear or linear ring active polysiloxane:

[0105] Weigh 0.043 mol (29.97 g) of tetramethyl-tetra-γ-glycidyloxypropylcyclotetrasiloxane and 0.010 mol (7.93 g) of octaphenylcyclotetrasiloxane in a dry three-necked flask, add a magnetic particle and condense and reflux at 120°C, weigh 0.010 mol (1.62 g) of hexamethyldisiloxane and 0.42 mmol (0.038 g) of tetramethylammonium hydroxide (TMAH), react for about 8 hours, heat to 150°C and stir for 30 minutes to decompose the catalyst, then remove the small molecular substances generated by the reaction by rotary evaporation at 150°C to obtain the ring-opening product. The viscosity, molecular weight and color state of the ring-opening product are statistically shown in Table 1.

[0106] 3. Preparation of phosphorus-containing polysiloxane reactive flame retardant:

[0107] Weigh 2.67 mmol (10.00 g) of the above-prepared open-ring product and 0.030 mol (6.49 g) of DOPO into a dry single-necked bottle, heat to 130° C., condense and reflux until DOPO is completely melted, add 0.31 mmol (0.081 g) of triphenylphosphine, and continue the reaction for about 12 h to obtain the final product, phosphorus-containing polysiloxane reactive flame retardant.

[0108] The prepared flame retardant was added to the E51 epoxy resin cured by DDM, and the flame retardant accounted for 5% of the total mass of the system. The flame retardant performance test results are shown in Table 2.

[0109] The prepared flame retardant was added to polyurea, and the flame retardant accounted for 10% of the total mass of the system. The flame retardant performance test results are shown in Table 2.

[0110] Example 5

[0111] 1. Preparation of cyclic reactive siloxane: same as in Example 1;

[0112] 2. Preparation of linear or linear ring active polysiloxane:

[0113] Weigh 0.050mol (34.85g) of tetramethyl-tetra-γ-glycidyloxypropylcyclotetrasiloxane and 0.010mol (7.93g) of octaphenylcyclotetrasiloxane in a dry three-necked flask, add a magnetic particle and condense and reflux at 120°C, weigh 0.010mol (1.62g) of hexamethyldisiloxane and 0.47mmol (0.043g) of tetramethylammonium hydroxide (TMAH), react for about 8h, heat to 150°C and stir for 30min to decompose the catalyst, then remove the small molecular substances generated by the reaction by rotary evaporation at 150°C to obtain the ring-opening product. The viscosity, molecular weight and color state of the ring-opening product are statistically shown in Table 1.

[0114] 3. Preparation of phosphorus-containing polysiloxane reactive flame retardant:

[0115] Weigh 2.25 mmol (10.00 g) of the above-prepared ring-opening product and 0.036 mol (7.78 g) of DOPO into a dry single-necked bottle, heat to 130° C., condense and reflux until DOPO is completely melted, add 0.34 mmol (0.089 g) of triphenylphosphine, and continue the reaction for about 24 h to obtain the final product, phosphorus-containing polysiloxane reactive flame retardant.

[0116] The prepared flame retardant was added to the E51 epoxy resin cured by DDM, and the flame retardant accounted for 5% of the total mass of the system. The flame retardant performance test results are shown in Table 2.

[0117] Example 6

[0118] 1. Preparation of cyclic reactive siloxane: same as in Example 1;

[0119] 2. Preparation of linear or linear ring-shaped reactive polysiloxane: same as in Example 2;

[0120] 3. Preparation of phosphorus-containing polysiloxane reactive flame retardant:

[0121] Weigh 4.25 mmol (10.00 g) of the above-prepared open-ring product and 0.017 mol (3.17 g) of diphenylphosphine into a dry single-necked bottle, heat to 180°C for condensation and reflux, then add 0.26 mmol (0.068 g) of triphenylphosphine, and continue the reaction for about 14 h to obtain the final product, phosphorus-containing polysiloxane reactive flame retardant.

[0122] The prepared flame retardant was added to the E51 epoxy resin cured by DDM, and the flame retardant accounted for 10% of the total mass of the system. The flame retardant performance test results are shown in Table 2.

[0123] The prepared flame retardant was added to polycarbonate, and the flame retardant accounted for 15% of the total mass of the system. The flame retardant performance test results are shown in Table 2.

[0124] Example 7

[0125] 1. Preparation of cyclic reactive siloxane: same as in Example 1;

[0126] 2. Preparation of linear or linear annular reactive polysiloxane: same as in Example 3;

[0127] 3. Preparation of phosphorus-containing polysiloxane reactive flame retardant:

[0128] Weigh 3.28 mmol (10.00 g) of the above-prepared open-ring product and 0.020 mol (3.72 g) of diphenylphosphine into a dry single-necked bottle, heat to 180°C for condensation and reflux, then add 0.26 mmol (0.068 g) of triphenylphosphine, and continue the reaction for about 14 h to obtain the final product, phosphorus-containing polysiloxane reactive flame retardant.

[0129] The prepared flame retardant was added to the E51 epoxy resin cured by DDM, and the flame retardant accounted for 10% of the total mass of the system. The flame retardant performance test results are shown in Table 2.

[0130] The prepared flame retardant was added to polyurethane, and the flame retardant accounted for 5% of the total mass of the system. The flame retardant performance test results are shown in Table 2.

[0131] Example 8

[0132] 1. Preparation of cyclic reactive siloxane: same as in Example 1;

[0133] 2. Linear or linear annular reactive polysiloxane: same as in Example 4;

[0134] 3. Preparation of phosphorus-containing polysiloxane reactive flame retardant:

[0135] Weigh 2.67 mmol (10.00 g) of the above-prepared ring-opening product and 0.030 mol (4.14 g) of diethyl phosphite into a dry single-necked bottle, heat to 130 ° C, condense and reflux, then add 0.27 mmol (0.071 g) of triphenylphosphine, and continue the reaction for about 12 hours to obtain the final product, phosphorus-containing polysiloxane reactive flame retardant.

[0136] The prepared flame retardant was added to the E51 epoxy resin cured by DDM, and the flame retardant accounted for 10% of the total mass of the system. The flame retardant performance test results are shown in Table 2.

[0137] Example 9

[0138] 1. Preparation of cyclic reactive siloxane: same as in Example 1;

[0139] 2. Preparation of linear or linear annular reactive polysiloxane: same as in Example 5;

[0140] 3. Preparation of phosphorus-containing polysiloxane reactive flame retardant:

[0141] Weigh 2.25 mmol (10.00 g) of the above-prepared ring-opening product and 0.036 mol (3.96 g) of dimethyl phosphite into a dry single-necked bottle, heat to 130° C., condense and reflux, then add 0.27 mmol (0.071 g) of triphenylphosphine, and continue the reaction for about 16 h to obtain the final product, reactive phosphorus-containing polysiloxane.

[0142] The prepared flame retardant was added to the E51 epoxy resin cured by DDM, and the flame retardant accounted for 15% of the total mass of the system. The flame retardant performance test results are shown in Table 2.

[0143] Example 10

[0144] 1. Preparation of cyclic reactive siloxane:

[0145] Weigh 0.112 mol (19.98 g) of 2,4,6-trimethylcyclotrisiloxane and 1.24 g of platinum catalyst into a dry three-necked flask, weigh 0.370 mol (42.23 g) of allyl glycidyl ether into a dry dropping funnel, add a magnetic particle, condense and reflux at 65°C, slowly drop allyl glycidyl ether, react after the addition is complete, the reaction time is about 8 hours, and after the reaction, the excess allyl glycidyl ether is removed by rotary evaporation to obtain the active cyclic siloxane trimethyl-tri-γ-glycidyl ether oxypropyl cyclotrisiloxane.

[0146] 2. Preparation of linear or linear ring active polysiloxane:

[0147] Weigh 0.038 mol (19.79 g) of trimethyl-tri-γ-glycidyloxypropylcyclotrisiloxane and 7.68 mmol (1.71 g) of hexamethylcyclotrisiloxane in a dry three-necked flask, add a magnetic bar and condense and reflux at 90°C, weigh 7.68 mmol (1.91 g) of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and 0.47 mmol (0.043 g) of tetramethylammonium hydroxide (TMAH), react for about 4 hours, heat to 130°C and stir for 30 minutes to decompose the catalyst, then remove the small molecular substances generated by the reaction at 150°C by rotary evaporation to obtain a ring-opened linear active polysiloxane product. The viscosity, molecular weight and color state of the ring-opened product are statistically shown in Table 1.

[0148] 3. Preparation of phosphorus-containing polysiloxane reactive flame retardant:

[0149] Weigh 3.24 mmol (9.99 g) of the above-prepared open-ring product and 0.013 mol (2.81 g) of DOPO into a dry single-necked bottle, heat to 180° C., condense and reflux until DOPO is completely melted, add 0.39 mmol (0.102 g) of triphenylphosphine, and continue the reaction for about 24 h to obtain the final product, phosphorus-containing polysiloxane reactive flame retardant.

[0150] The prepared flame retardant was added to the E51 epoxy resin cured by DDM, and the flame retardant accounted for 10% of the total mass of the system. The flame retardant performance test results are shown in Table 2.

[0151] Table 1 Molecular weight, viscosity and color state of the reactive polysiloxane obtained in step (2) of Examples 1 to 9

[0152] Theoretical molecular weight Measured molecular weight Viscosity (mPa.s) color Example 1 1652.65 1660.32 920 Brown red liquid Example 2 2349.73 2352.37 1030 Brown red liquid Example 3 3046.82 3048.39 1120 Brown red liquid Example 4 3743.91 3746.95 1190 Brown red liquid Example 5 4440.99 4445.24 1240 Brown red liquid Example 6 2349.73 2352.37 1030 Brown red liquid Example 7 3046.82 3048.39 1120 Brown red liquid Example 8 3743.91 3746.95 1190 Brown red liquid Example 9 4440.99 4445.24 1240 Brown red liquid Example 10 3076.97 3082.66 1100 Light red liquid

[0153] Table 1 shows the molecular weight, viscosity and color state of the active polysiloxane obtained in step (2) of Examples 1 to 10. It can be seen that the measured molecular weight of the obtained linear or linear ring-shaped active polysiloxane is between 1660.32 and 4445.24, which is close to the theoretical molecular weight, and the viscosity is between 920 and 1240 mPa.s. The molecular weight and viscosity are controllable, the active group content is controllable, and the proportion of the grafted phosphorus-containing substance can be controlled.

[0154] Table 2 Flame retardant effect of the flame retardants prepared in Examples 1 to 9 in the substrate

[0155]

[0156] Table 2 shows the flame retardant effects of the flame retardants prepared in Examples 1 to 10 in the substrate. From the oxygen index test and vertical combustion test results in Table 2, it can be seen that the reactive phosphorus-containing polysiloxane flame retardant prepared in the present invention has good flame retardant effects on polyurea, polyurethane, polycarbonate and epoxy, has high flame retardant efficiency, and does not contain halogen, meeting the environmental protection requirements of halogen-free.

Claims

1. A phosphorus-containing polysiloxane reactive flame retardant is prepared from raw materials including a cyclic active siloxane 1, a catalyst 1, a bifunctional compound, a cyclic inactive siloxane, a catalyst 2, a capping agent, a phosphorus-containing substance, and a catalyst 3.

2. The phosphorus-containing polysiloxane reactive flame retardant according to claim 1, characterized in that: The structure of the cyclic active siloxane 1 is: Where: 6≥m+n≥3, m and n are integers greater than or equal to 0, and m and n cannot be 0 at the same time; R1, R2, R3, and R4 are independently selected from one of hydrogen atom, hydroxyl group, amino group, vinyl group, epoxy group, methyl group, alkoxy group, phenyl group, and phenoxy group, and at least one of R1, R2, R3, and R4 is hydrogen atom, hydroxyl group, amino group, vinyl group, or epoxy group; and / or, The bifunctional compound is at least one of allyl glycidyl ether, allyl alcohol, methallyl alcohol, eugenol, allylamine, N-methylallylamine, 3-allyl bromide, 3-allyl chloride, 3-bromo-2-methylpropene, and 3-chloro-2-methylpropene; and / or, The catalyst 1 is a transition metal catalyst, preferably at least one of platinum, palladium, rhodium and nickel catalysts.

3. The phosphorus-containing polysiloxane reactive flame retardant according to claim 1, characterized in that: The structural formula of the cyclic inactive siloxane is: Wherein: 6≥p+q≥3, p and q are integers greater than or equal to 0, and p and q cannot be 0 at the same time; R5, R6, R7, R8 are independently selected from one of methyl, ethyl, and phenyl; and / or, The catalyst 2 is at least one of LiOH, NaOH, KOH and silicon alkoxides thereof, methyl lithium, ethyl lithium, propyl lithium, n-butyl lithium, phenyl lithium, tetramethylammonium hydroxide, tetramethylammonium hydroxide silicon alkoxide, tetrabutylphosphonium hydroxide silicon alkoxide, Et4NOH, Bu4POH, and linear phosphazene chloride; and / or, The end-capping agent is hexamethyldisiloxane, 1,1,3,3-tetramethyldisiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(3-epoxy)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(3-hydroxypropyl)-1,1,3,3-tetramethyldisiloxane, 1,3-divinyl-1,1,3,3-tetramethyldisiloxane, methanol, ethanol, water, small molecules Hydroxy silicone oil, small molecule amino silicone oil, trimethylsilanol, dimethylchlorosilane, trimethylmonochlorosilane, triethylmonochlorosilane, trimethylmethoxysilane, 3,3'-dithiodipropionic acid; the small molecule hydroxy silicone oil is preferably at least one of terminal hydroxy silicone oil, terminal hydroxypropyl silicone oil, side hydroxy silicone oil, and side hydroxypropyl silicone oil; the small molecule amino silicone oil is preferably at least one of terminal amino silicone oil, terminal aminopropyl silicone oil, side amino silicone oil, and side aminopropyl silicone oil; and / or, The phosphorus-containing substance is a compound containing an active PH bond, preferably at least one of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, diphenylphosphine, diphenylphosphine, dimethyl phosphite, diethyl phosphite, dibutyl phosphite, phenylphosphonic acid, phosphorous acid, hypophosphorous acid, 5,5-dimethyl-1,3,2-dioxaphosphine 2-oxide, phospholane, phosphahexane, 2-hydrogen-2-oxo-1,3,2-oxazaphosphahexane, and 5,10-dihydro-phosphaazine-10-oxide; and / or, The catalyst 3 is at least one of triphenylphosphine, tributylphosphine, tri-tert-butylphosphine, azobisisobutyronitrile, an organic tin compound, and a phosphazene catalyst; the organic tin compound is preferably at least one of Bu2SnO, Bu3SnCl, and Ph3SnCl.

4. A method for preparing the phosphorus-containing polysiloxane reactive flame retardant according to any one of claims 1 to 3, comprising the following steps: (1) reacting the cyclic active siloxane 1 with the bifunctional compound in the presence of the catalyst 1 to obtain the cyclic active siloxane 2; (2) subjecting the cyclic active siloxane 2 obtained in step (1) to a ring-opening copolymerization reaction with the cyclic inactive siloxane and the end-capping agent in the presence of the catalyst 2 to obtain a linear or linear annular active polysiloxane 3; (3) reacting the linear or linear ring-shaped active polysiloxane 3 obtained in step (2) with the phosphorus-containing substance in the presence of a catalyst 3 to obtain the phosphorus-containing polysiloxane reactive flame retardant.

5. The method for preparing the phosphorus-containing polysiloxane reactive flame retardant according to claim 4, characterized in that: Step (1), slowly adding an excess of a bifunctional compound dropwise to a mixed solution of the cyclic active siloxane 1 and the catalyst for reaction, and then removing the excess of the bifunctional compound; and / or, Step (2), heating the cyclic active siloxane 2, the cyclic inactive siloxane, the catalyst 2 and the end-capping agent to carry out a ring-opening polymerization reaction, then heating the catalyst 2 to decompose the catalyst 2, and rotary evaporating to remove small molecular substances.

6. The method for preparing the phosphorus-containing polysiloxane reactive flame retardant according to claim 4, characterized in that: Step (1), The molar ratio of the Si-H group of the cyclic reactive siloxane 1 to the C=C double bond group of the bifunctional compound is 1:(1.1-2.0), preferably 1:(1.1-1.8); and / or, The amount of the catalyst 1 is 0.005 to 0.02 times the total mass of the reactants in step (1), preferably 0.01 to 0.02 times the total mass of the reactants; and / or, Step (2), The molar ratio of the cyclic inactive siloxane to the cyclic active siloxane 2 is 1:(1-10), preferably 1:(1-5); and / or, The molar ratio of the catalyst 2 to the cyclic active siloxane 2 is 1:(1-10 5 ), preferably 1: (60-110); and / or, The molar ratio of the cyclic active siloxane 2 to the end-capping agent is 1:(10 -3 ~10 4 ); preferably 1:(10 -1 ~1); and / or, The molecular weight of the linear or linear annular active polysiloxane 3 is 500 to 20,000, preferably 1,000 to 5,000; and / or, Step (3), The molar ratio of the linear or linear ring-shaped active polysiloxane 3 to the phosphorus-containing substance is 1:(1-30), preferably 1:(4-16); and / or, The amount of the catalyst 3 used is 0.005 to 0.01 times the total mass of the reactants in step (3), preferably 0.005 to 0.008 times the total mass of the reactants.

7. The method for preparing the phosphorus-containing polysiloxane reactive flame retardant according to claim 4, characterized in that: Step (1), Reaction temperature: 25-120°C, preferably 65-90°C; and / or, Reaction time: 1 to 12 hours, preferably 8 to 12 hours; and / or, Step (2), The reaction temperature is 60 to 120°C, preferably 90 to 120°C; and / or, The reaction time is 1 to 12 hours; preferably 4 to 8 hours; and / or, Step (3), The reaction temperature is 130 to 200°C, preferably 130 to 180°C; and / or, The reaction time is 10 to 48 hours, preferably 12 to 24 hours.

8. The method for preparing the phosphorus-containing polysiloxane reactive flame retardant according to claim 5, characterized in that: Step (2), The decomposition catalyst temperature is 130 to 180°C, preferably 130 to 150°C.

9. A phosphorus-containing polysiloxane reactive flame retardant obtained by the preparation method according to any one of claims 4 to 8.

10. Use of the phosphorus-containing polysiloxane reactive flame retardant according to any one of claims 1 to 3 and 9 in a matrix material, preferably in polyurea, polyurethane or epoxy.

Citation Information

Patent Citations

  • New method for preparing allyl ether modified silicone oil

    CN106633067A

  • Multifunctional alkoxy-terminated polysiloxane polymer and preparation method thereof

    CN111440321A

  • Phosphorus-containing polysiloxane reactive flame retardant, preparation method and application

    CN115703886A

  • Epoxy phosphorus-containing polysiloxane, preparation method thereof and prepared epoxy composition

    CN115894926A

  • Additive phosphorus-containing polysiloxane compound for thermosetting resins, flame retardant composition comprising same, and articles made therefrom

    US20200291232A1

Cited By

  • Preparation method of insulated halogen-free low-smoke fire-resistant cable

    CN119361260A

  • Moisture-absorbing sweat-permeable chenille yarn and production process thereof

    CN119571514A

  • Novel fluorine-free halogen-free flame-retardant high-performance PC material and preparation method thereof

    CN119899507A

  • Nanoscale organic silicon clustered phosphinic acid flame retardant and preparation method thereof

    CN119955105A

  • Nanoscale organosilicon cluster hypophosphite flame retardant and preparation method thereof