Preparation method of piperazine phosphate-melamine phosphate-ammonium phosphate copolymerized flame retardant as well as product and application thereof
Through the preparation of piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, the problem that traditional flame retardants are easy to precipitate and hydrolyze in high temperature and high humidity environments is solved, and the efficient flame retardant performance of polyolefin materials is maintained. and cost reduction.
Patent Information
- Application Number
- CN202411113281.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-10-15
AI Technical Summary
Traditional intumescent flame retardants are prone to precipitation and hydrolysis problems in high temperature, high humidity and water environments, leading to flame retardant failure of polyolefin materials. Existing modification technology cannot fundamentally solve this problem.
Using the preparation method of piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, piperazine diphosphate, melamine phosphate and ammonium dihydrogen phosphate are formed through polymerization reaction to form a copolymer, which has an acid source, a gas source and a carbon source. Functional intumescent flame retardant solves the problem of easy precipitation and hydrolysis of traditional ammonium polyphosphate.
The prepared copolymer flame retardant in the polyolefin material maintains the V-0 flame retardant performance after boiling for 168 hours, has no surface precipitates, has low cost and is hydrolysis resistant.
Smart Images

Figure CN118772419A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of flame retardant preparation, and relates to a preparation method of a piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, a product thereof and an application thereof. Background Art
[0002] Intumescent flame retardants are considered to be an important development direction in the field of environmentally friendly halogen-free flame-retardant polyolefin materials. They have the characteristics of low smoke emission, low toxic gas generation and good flame retardant effect. They have been actually applied in industrial applications in materials such as polypropylene, polyethylene, and polyolefin elastomers. The resulting flame retardant materials can be used to prepare electrical housings, automobile bumpers, industrial pipelines, wires and cables and other products.
[0003] Intumescent flame retardants are generally composed of three parts: (1) Acid source, usually inorganic acid or inorganic acid compound, such as phosphoric acid, phosphate ester, boric acid, ammonium polyphosphate, etc.; (2) Carbon source, mainly polyhydroxy compounds or carbohydrates with high carbon content, such as starch, pentaerythritol, etc.; (3) Gas source, generally nitrogen-containing compounds, such as urea, melamine, ammonium polyphosphate, etc. Under the action of high heat, the substances produced by the decomposition of the acid source catalyze the cross-linking of the carbon source into carbon, forming a thick intumescent carbon layer on the surface of the material, thereby playing a role in heat insulation and oxygen isolation, and stopping combustion in the early stage of combustion.
[0004] Traditional intumescent flame retardants generally use ammonium polyphosphate as an acid source and pentaerythritol as a carbon source. They have the advantages of high flame retardant efficiency and low price, and are widely used in polyolefins. However, ammonium polyphosphate is an inorganic substance. In high temperature, high humidity and water environments, it is easy to cause flame retardant precipitation and hydrolysis problems, resulting in flame retardant failure and surface blooming of polyolefin materials. Although the hydrolysis resistance of ammonium polyphosphate can be improved by surface modification, surface treatment, microencapsulation and other technologies, it cannot fundamentally solve the problem.
[0005] In recent years, many intumescent flame retardants have emerged that combine two or even three of the functions of acid source, carbon source, and gas source in the same molecular structure. Most of these flame retardant molecules contain phosphorus and nitrogen elements. When decomposed by heat, they can produce acidic substances to dehydrate the system, and can also decompose to produce non-flammable gases to expand the carbon layer. At the same time, they can also eliminate the molecular defects of a single acid source, carbon source, or gas source.
[0006] Therefore, it is necessary to develop a new type of intumescent flame retardant that has the functions of acid source, gas source and carbon source and is resistant to hydrolysis, so as to provide a new idea for the preparation of environmentally friendly flame-retardant polyolefins. Summary of the invention
[0007] In view of this, one of the objects of the present invention is to provide a method for preparing a piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant; a second object of the present invention is to provide a piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant; a third object of the present invention is to provide an application of a piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant in the preparation of a flame-retardant polyolefin material; a fourth object of the present invention is to provide a flame-retardant polyolefin material; and a fifth object of the present invention is to provide a method for preparing a flame-retardant polyolefin material.
[0008] In order to achieve the above object, the present invention provides the following technical solutions:
[0009] 1. A method for preparing a piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, the preparation method comprising the following steps:
[0010] The piperazine diphosphate, melamine phosphate, ammonium dihydrogen phosphate and urea are ground into powder and mixed evenly, and placed in an oven for polymerization reaction. After the reaction is completed, the mixture is cooled and ground into powder to obtain a piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant.
[0011] Preferably, the molar ratio of the mixture formed by piperazine diphosphate and melamine phosphate to diammonium phosphate is 2:1.5-2;
[0012] The molar ratio of piperazine diphosphate to melamine phosphate in the mixture formed by piperazine diphosphate and melamine phosphate is 0.7-0.9:1.1-1.3;
[0013] The molar ratio of the diammonium phosphate to the urea is 2:2-2.4.
[0014] Further preferably, the molar ratio of the mixture formed by piperazine diphosphate and melamine phosphate to diammonium phosphate is 2:2;
[0015] The molar ratio of piperazine diphosphate to melamine phosphate in the mixture formed by piperazine diphosphate and melamine phosphate is 0.8:1.2;
[0016] The molar ratio of the diammonium phosphate to the urea is 2:2.2.
[0017] Preferably, the polymerization reaction temperature is 250-270° C. and the time is 1-3 hours.
[0018] More preferably, the polymerization reaction is carried out at a temperature of 260° C. and for a time of 2 h.
[0019] 2. The piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant prepared according to the above preparation method.
[0020] 3. Application of the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant in the preparation of flame-retardant polyolefin materials.
[0021] 4. Flame-retardant polyolefin material, which comprises the following components in parts by weight: 70-77 parts of polyolefin, 23-30 parts of the above-mentioned piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, 0.3-0.8 parts of antioxidant and 0.3-0.5 parts of processing lubricant.
[0022] Preferably, the polyolefin is any one or more of polyethylene, polypropylene, polybutylene, vinyl elastomer, propylene elastomer or EPDM rubber;
[0023] The antioxidant is any one or more of antioxidant 1010, antioxidant 168, antioxidant 1098 or antioxidant 1076;
[0024] The processing lubricant is any one or more of calcium stearate, zinc stearate, montan wax, silicone wax, polyester sodium or pentaerythritol stearate.
[0025] 5. A method for preparing the flame retardant polyolefin material, comprising the following steps:
[0026] Polyolefin, piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, antioxidant and processing lubricant are uniformly mixed and placed in an extruder, and flame-retardant polyolefin material can be obtained through melting, blending, extrusion, drawing, pelletizing and drying.
[0027] Preferably, the temperature of each section of the extruder from the main feeding port to the die head is: 170-200°C, 180-210°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 180-210°C, 220-230°C;
[0028] The rotation speed of the extruder is 300-350 r / min.
[0029] The beneficial effects of the present invention are as follows: the present invention discloses a preparation method of a piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, which mainly comprises grinding piperazine diphosphate, melamine phosphate, ammonium dihydrogen phosphate and urea into powder and then mixing them evenly, placing them in an oven for polymerization reaction, cooling after the reaction is completed, and grinding them into powder to obtain the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, and copolymerizing easily soluble and easily hydrolyzable ammonium phosphate, insoluble and insoluble piperazine phosphate and melamine phosphate to form an intumescent flame retardant having a carbon source, an acid source and a gas source. The copolymer flame retardant prepared by the preparation method of the present invention contains piperazine phosphate, melamine phosphate and ammonium phosphate structures in its structural formula, thus solving the problem that traditional ammonium polyphosphate is easy to precipitate and hydrolyze. Meanwhile, the low-cost ammonium phosphate is added during the preparation process, and the cost is lower than that of piperazine pyrophosphate and melamine polyphosphate compound flame retardant. The copolymer flame retardant can be applied to the preparation of polyolefin materials, and the flame retardant performance of the prepared flame-retardant polyolefin material still remains at V-0 level after being boiled in water for 168 hours, and no precipitates are left on the surface.
[0030] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:
[0032] Figure 1 This is the infrared spectrum analysis result of the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant prepared in Example 1;
[0033] Figure 2 This is the nuclear magnetic resonance phosphorus spectrum analysis of the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant prepared in Example 1. DETAILED DESCRIPTION
[0034] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the illustrations provided in the following embodiments only illustrate the basic concept of the present invention in a schematic manner, and the following embodiments and features in the embodiments can be combined with each other without conflict.
[0035] Examples 1 to 8
[0036] A piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, the specific preparation method is as follows:
[0037] Piperazine diphosphate, melamine phosphate, ammonium dihydrogen phosphate and urea (the molar numbers of various materials added in each embodiment are as shown in Table 1) are ground into powder and mixed evenly, placed in an oven for polymerization reaction (the temperature and time of the polymerization reaction in each embodiment are respectively as shown in Table 1), cooled after the reaction is completed, and ground into powder to obtain piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant.
[0038] Table 1 Examples 1 to 8 and Comparative Examples 1 to 8 are the ratios of the components and the polymerization temperature and time in the preparation process of piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant
[0039]
[0040]
[0041] Comparative Examples 1 to 8
[0042] A piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, the specific preparation method is as follows:
[0043] Piperazine diphosphate, melamine phosphate, ammonium dihydrogen phosphate and urea (the molar numbers of various materials added in each embodiment are as shown in Table 1) are ground into powder and mixed evenly, placed in an oven for polymerization reaction (the temperature and time of the polymerization reaction in each embodiment are respectively as shown in Table 1), cooled after the reaction is completed, and ground into powder to obtain piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant.
[0044] Examples 9 to 18
[0045] Flame retardant polyolefin material, the specific preparation method is as follows:
[0046] The polyolefin, piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant (the product prepared by the preparation method of the above different embodiments), antioxidant, and processing lubricant are mixed evenly (the relevant components and parts in each embodiment are as shown in Table 2) and placed in an extruder (wherein the temperatures of each section of the extruder from the main feed port to the die are: 180°C, 190°C, 200°C, 200°C, 210°C, 210°C, 200°C, 200°C, 200°C, and the speed of the extruder is 350r / min), and then melted, blended, extruded, drawn, pelletized, and dried.
[0047] Table 2 Proportions of the components in the flame-retardant polyolefins of Examples 9 to 17 and Comparative Examples 9 to 14
[0048]
[0049] In the above Table 1, polypropylene is polypropylene resin (SP179, melt index 10 g / 10 min, Lanzhou Petrochemical), polyethylene is polyethylene resin (HDPE 5000S, melt index 3 g / 10 min, Daqing Petrochemical), vinyl elastomer (POE, 8200, melt index 5 g / 10 min, Dow Chemical), ammonium polyphosphate system flame retardant (TC100, Chongqing Kejufu New Materials Co., Ltd.), antioxidant is anti-1076, and processing lubricant is silicone wax (grade E525).
[0050] Comparative Examples 9 to 14
[0051] Flame retardant polyolefin material, the specific preparation method is as follows:
[0052] The polyolefin, piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, antioxidant and processing lubricant are uniformly mixed (the relevant components and parts in each embodiment are as shown in Table 2) and placed in an extruder (wherein the temperatures of each section of the extruder from the main feed port to the die are: 180°C, 190°C, 200°C, 200°C, 210°C, 210°C, 200°C, 200°C, 200°C, and the speed of the extruder is 350r / min), and then melted, blended, extruded, drawn, pelletized and dried.
[0053] Example 19 to Example 24
[0054] Flame retardant polyolefin material, the specific preparation method is as follows:
[0055] 740g of polyolefin, 250g of piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant prepared according to the method in Example 1, 5.0g of antioxidant, and 4.0g of processing lubricant were mixed evenly (the relevant components and parts in each embodiment are as shown in Table 3) and placed in an extruder (wherein the temperature of each section of the extruder from the main feed port to the die head and the speed of the extruder are as shown in Table 3), and then melted, blended, extruded, stretched, pelletized, and dried.
[0056] Table 3 Different components of flame-retardant polyolefin materials and extruder parameters and speed in Examples 19 to 24
[0057]
[0058] Performance Testing
[0059] The piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, diammonium phosphate, melamine phosphate and piperazine diphosphate prepared in Example 1 were subjected to infrared spectroscopy analysis, and the results are as follows: Figure 1 As shown. Figure 1 It can be seen from the infrared spectrum analysis results that the infrared spectrum peaks of the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant prepared in Example 1 are obviously different from those of diammonium phosphate, melamine phosphate and piperazine diphosphate. -1 The peak is the characteristic peak of the stretching vibration absorption of POP, indicating that a polycondensation reaction occurred during the preparation process of Example 1, proving that a product with a structure of piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant was prepared in Example 1.
[0060] The piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant prepared in Example 1 was subjected to nuclear magnetic resonance phosphorus spectrum analysis, and the results are as follows: Figure 2 As shown. Figure 2 It can be seen that the NMR phosphorus spectrum of the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant prepared in Example 1 simultaneously shows a free phosphorus peak with a chemical shift of -1.02, a terminal phosphorus peak with chemical shifts of -10.28 and -11.31, and an intermediate phosphorus peak with a chemical shift of -23.62. The presence of the terminal and intermediate phosphorus peaks indicates that the product prepared by the preparation method of Example 1 does indeed contain the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant structure.
[0061] Similarly, the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant prepared in the other embodiments is subjected to infrared spectrum and nuclear magnetic resonance phosphorus spectrum analysis, and the results are basically the same as those in the above embodiment 1, which shows that the preparation method of the present invention can indeed prepare piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant. The piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant of the present invention contains piperazine phosphate structure, melamine phosphate structure and ammonium phosphate structure at the same time. In the polymerization process, the following situations may exist: (1) the piperazine phosphate structure, melamine phosphate structure and ammonium phosphate structure are randomly copolymerized; (2) the piperazine phosphate structure, melamine phosphate structure and ammonium phosphate structure are alternately copolymerized; (3) the piperazine phosphate structure, melamine phosphate structure and ammonium phosphate structure are block copolymerized.
[0062] In order to verify the performance and polymerization process of the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant prepared by the present invention, the yield, TG (1% thermal weight loss), and flame retardant color tests were performed on the corresponding flame retardants in Examples 1 to 8 and Comparative Examples 1 to 8. The test results are shown in Table 4. The specific test method is as follows:
[0063] (1) Yield test: the total weight of the mixture of piperazine diphosphate, melamine phosphate, ammonium dihydrogen phosphate and urea before high-temperature polymerization is m1, the weight of the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant prepared after high-temperature polymerization is m2, and the flame retardant yield = m1÷m2*100%;
[0064] (2) TG (1% thermal weight loss): carried out in accordance with the latest standard of ASTM E2550;
[0065] (3) Flame retardant color: judged by the eyes as white, gray, or black.
[0066] Table 4 Comparison of yield, TG (1% thermal weight loss), and color performance of the flame retardants prepared in Examples 1 to 8 and Comparative Examples 1 to 8
[0067]
[0068]
[0069] In order to verify the performance of the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant obtained by the present invention in polyolefin, the flame retardant polyolefin materials prepared in Examples 9 to 18, Comparative Examples 9 to 15 and Examples 19 to 24 were tested for flame retardant properties, flame retardant properties after boiling and precipitates on the surface of the specimens. The test results are shown in Table 5. The specific test methods are as follows:
[0070] (1) Flame retardant properties: According to the latest UL94 standard, the flame retardant polyolefin materials prepared in Examples 9 to 18, Comparative Examples 9 to 15 and Examples 19 to 24 were placed in an oven and dried at 100° C. for 3 h, and then each material was injection molded into UL94 standard specimens using an injection molding machine;
[0071] (2) Boiling test: carried out in accordance with the latest UL746C standard, with a boiling temperature of 85°C and a boiling time of 168 hours;
[0072] (3) Spline surface precipitate test: The spline surface is judged visually.
[0073] Table 5 Comparison of flame retardancy, flame retardancy after boiling and surface precipitates of the flame retardant polyolefin materials prepared in Examples 9 to 24 and Comparative Examples 9 to 15
[0074]
[0075]
[0076] As can be seen from Table 4, the polymerization temperature and time have a crucial influence on the performance of piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, which is specifically manifested in: by comparing Example 1, Example 5-8 and Comparative Examples 1-4, it can be found that when the polymerization temperature exceeds 270°C or the polymerization time exceeds 3h, the color of the prepared copolymer flame retardant turns black, indicating that the polymerization temperature is too high and the polymerization time is too long, resulting in carbonization of the copolymer flame retardant; when the polymerization temperature is lower than 250°C or the polymerization time is less than 1h, the yield of the copolymer flame retardant is too large, and the TG (1% thermal weight loss) temperature is low, indicating that the polymerization temperature is too low and the polymerization time is too short, resulting in incomplete polymerization of the copolymer flame retardant. It is thus shown that when the polymerization temperature is 250-270°C and the polymerization time is 1-3h, the yield, TG (1% thermal weight loss) and color performance of the prepared piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant are optimal.
[0077] It can be seen from Table 4 and Table 5 that the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant is applied to polyolefin materials, and the ratio of piperazine diphosphate, melamine phosphate, ammonium dihydrogen phosphate and urea in the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant has a crucial influence on the flame retardant properties of polyolefin materials. Piperazine phosphate is used as a carbon source in the copolymer flame retardant, melamine phosphate is used as a gas source, and ammonium phosphate is used as an acid source. By comparing Examples 1 to 4, Examples 9 to 12 and Comparative Examples 5 to 12, it can be found that when the molar ratio of piperazine diphosphate to melamine phosphate is too much (Comparative Example 6) or too little (Comparative Example 5), the carbon source is too much or too little, which affects the flame retardant efficiency of the copolymer flame retardant. When applied to the preparation of flame-retardant polyolefin materials, the material is not flame retardant; when piperazine phosphate is When the molar sum of melamine phosphate and the molar ratio of diammonium phosphate are too much (Comparative Example 8) or too little (Comparative Example 7), the acid source is too much or too little, which will also affect the flame retardant efficiency of the copolymer flame retardant. When it is applied to the preparation of flame-retardant polyolefin materials, the material is not flame retardant. At the same time, too much diammonium phosphate leads to excessive precipitation of easily hydrolyzed ammonium phosphate in the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, and in the water boiling experiment, a small amount of precipitate is produced on the surface of the sample. Therefore, the ratio of piperazine diphosphate, melamine phosphate, ammonium dihydrogen phosphate and urea affects the proportion of carbon source, gas source and acid source in the copolymer. Only the appropriate ratio (the molar ratio of the molar sum of piperazine diphosphate and melamine phosphate to ammonium dihydrogen phosphate is 2:1.5-2, the molar ratio of piperazine diphosphate to melamine phosphate is 0.7-0.9:1.1-1.3, and the molar ratio of ammonium dihydrogen phosphate to urea is 2:2-2.4) can achieve the optimal flame retardant efficiency. When applied to polyolefin materials, the materials reach V-0 flame retardancy.
[0078] At the same time, by comparing Examples 9 to 18 and Comparative Examples 13 to 15, it can be found that when the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant is applied to polyolefin materials (polypropylene, polyethylene, vinyl elastomer), the flame retardant performance of the polyolefin material reaches V-0 level, and the material remains flame retardant at V-0 level after boiling, and there is no precipitate on the surface of the spline; while using the ammonium polyphosphate (APP) system flame retardant, the flame retardant performance of the polyolefin material reaches V-0 level, but the flame retardant of the material fails after boiling, is not flame retardant, and there are precipitates on the surface of the spline.
[0079] In addition, it can be seen from the properties of the flame-retardant polyolefin materials prepared in Examples 19 to 24 in Table 5 that when the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant prepared by the present invention is used to prepare a flame-retardant polyolefin material, the polyolefin is changed between any one or more of polyethylene, polypropylene, polybutene, vinyl elastomer, propylene-based elastomer or EPDM rubber, the antioxidant is changed between any one or more of antioxidant 1010, antioxidant 168, antioxidant 1098 or antioxidant 1076, and the processing lubricant is changed between any one or more of calcium stearate, zinc stearate, montan wax, silicone wax, polyester sodium or pentaerythritol stearate. Flame-retardant polyolefin materials with flame retardancy of V-0 grade, flame retardancy of V-0 grade after boiling for 168h, and no precipitate on the surface of the specimen after boiling for 168h can be obtained.
[0080] In summary, the present invention discloses a preparation method of piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, which mainly comprises grinding piperazine diphosphate, melamine phosphate, ammonium dihydrogen phosphate and urea into powder and then mixing them evenly, placing them in an oven for polymerization reaction, cooling after the reaction is completed, and grinding them into powder to obtain piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, and copolymerizing easily soluble and easily hydrolyzable ammonium phosphate, insoluble and insoluble piperazine phosphate and melamine phosphate to form an intumescent flame retardant having a carbon source, an acid source and a gas source. The copolymer flame retardant prepared by the preparation method of the present invention contains piperazine phosphate, melamine phosphate and ammonium phosphate structures in its structural formula, thus solving the problem that traditional ammonium polyphosphate is easy to precipitate and hydrolyze. Meanwhile, the low-cost ammonium phosphate is added during the preparation process, and the cost is lower than that of piperazine pyrophosphate and melamine polyphosphate compound flame retardant. The copolymer flame retardant can be applied to the preparation of polyolefin materials. The flame retardant performance of the prepared polyolefin material still remains at V-0 level after being boiled in water for 168 hours, and no precipitates are left on the surface.
[0081] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, characterized in that: The preparation method comprises the following steps: The piperazine diphosphate, melamine phosphate, ammonium dihydrogen phosphate and urea are ground into powder and mixed evenly, and placed in an oven for polymerization reaction. After the reaction is completed, the mixture is cooled and ground into powder to obtain a piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant.
2. The preparation method according to claim 1, characterized in that: The molar ratio of the mixture formed by piperazine diphosphate and melamine phosphate to diammonium phosphate is 2:1.5-2; The molar ratio of piperazine diphosphate to melamine phosphate in the mixture formed by piperazine diphosphate and melamine phosphate is 0.7-0.9:1.1-1.3; The molar ratio of the diammonium phosphate to the urea is 2:2-2.
4.
3. The preparation method according to claim 2, characterized in that: The molar ratio of the mixture formed by piperazine diphosphate and melamine phosphate to diammonium phosphate is 2:2; The molar ratio of piperazine diphosphate to melamine phosphate in the mixture formed by piperazine diphosphate and melamine phosphate is 0.8:1.2; The molar ratio of the diammonium phosphate to the urea is 2:2.
2.
4. The preparation method according to claim 1, characterized in that: The polymerization reaction temperature is 250-270°C and the reaction time is 1-3h; The polymerization reaction was carried out at a temperature of 260° C. and for a time of 2 hours.
5. The piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant prepared according to the preparation method according to any one of claims 1 to 4.
6. Use of the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant according to claim 5 in the preparation of flame-retardant polyolefin materials.
7. Flame retardant polyolefin material, characterized in that: The flame retardant polyolefin material comprises the following components in parts by weight: 70-77 parts of polyolefin, 23-30 parts of the piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant according to claim 5, 0.3-0.8 parts of antioxidant and 0.3-0.5 parts of processing lubricant.
8. The flame retardant polyolefin material according to claim 7, characterized in that: The polyolefin is any one or more of polyethylene, polypropylene, polybutylene, vinyl elastomer, propylene elastomer or EPDM rubber; The antioxidant is any one or more of antioxidant 1010, antioxidant 168, antioxidant 1098 or antioxidant 1076; The processing lubricant is any one or more of calcium stearate, zinc stearate, montan wax, silicone wax, polyester sodium or pentaerythritol stearate.
9. The method for preparing the flame retardant polyolefin material according to any one of claims 7 to 8, characterized in that: The preparation method comprises the following steps: Polyolefin, piperazine phosphate-melamine phosphate-ammonium phosphate copolymer flame retardant, antioxidant and processing lubricant are uniformly mixed and placed in an extruder, and flame-retardant polyolefin material can be obtained through melting, blending, extrusion, drawing, pelletizing and drying.
10. The preparation method according to claim 8, characterized in that: The temperatures of the extruder from the main feed port to the die are: 170-200°C, 180-210°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 180-210°C, 220-230°C; The rotation speed of the extruder is 300-350 r / min.