Liquid-state all-solid-content high-and-low-temperature-resistant chassis corrosion-resistant wax and preparation method thereof
Through the oxygen curing and moisture curing technology of liquid full-solid high and low temperature resistant chassis anti-corrosion wax, a dense resin film and a self-healing wax film are formed, which solves the adhesion and cracking problems of the automobile chassis in high and low temperature environments, and improves the product's durability. Safety and durability for global shipping and storage.
Patent Information
- Application Number
- CN202411054310.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-08-02
AI Technical Summary
Existing anti-corrosion wax products for automobile chassis have problems such as adhesion, cracking, and dust adsorption in high and low temperature environments. Moreover, traditional solvent-based and water-based products have shortcomings such as VOC, difficulty in drying, and high storage and transportation requirements. They cannot meet the high-temperature resistance of the automobile export market. Low temperature anti-corrosion requirements.
It adopts liquid full solid high and low temperature resistant chassis anti-corrosion wax, which can quickly achieve the surface drying effect at normal temperature through the dual methods of oxygen curing and moisture curing, forming a dense high temperature resistant resin film, which can self-repair at low temperatures to avoid solvents and Mineral oil, using guarana esterified epoxy hydroxyl-terminated polybutadiene and organic zirconium and iron chelates to form a cross-linked film.
It achieves the anti-corrosion effect of not adhering or adsorbing pollutants at high temperatures, and not cracking at low temperatures, improves drying speed and adhesion, solves the safety, environmental protection and durability issues of traditional products, and is suitable for transportation in different environments around the world. and storage.
Smart Images

Figure CN118772701A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of anti-corrosion wax, and in particular relates to a liquid all-solid high and low temperature resistant chassis anti-corrosion wax used in the automotive field. Background Art
[0002] With the export of passenger cars and commercial vehicles in recent years, the annual export volume of automobiles has increased year by year, but the rust problem has also gradually become prominent, especially the vehicle chassis system, which is more susceptible to seawater corrosion during sea transportation, causing many overseas quality disputes. Traditional chassis anti-corrosion is generally based on spray wax, generally using solvent-based protective wax, sprayed on the vehicle chassis through airless spraying. Solvent-based products generally have problems such as dark color, high VOC, and low flash point, and cannot be used directly in the assembly workshop. Due to the defects of solvent products in color, safety and VOC, automobile OEMs have also gradually developed water-based chassis anti-corrosion wax products, but water-based wax products still contain a small amount of solvent (100g / L), and for some OEMs, there are still VOC problems. At the same time, water-based products have defects such as difficulty in drying in winter, poor water resistance, difficulty in line baking, and high temperature requirements for storage and transportation. Therefore, neither water-based products nor solvent-based products can perfectly solve the problem of vehicle chassis anti-corrosion.
[0003] In addition, both water-based products and solvent-based anti-corrosion waxes have problems with high and low temperature resistance in different environments around the world during the subsequent transportation and storage process after spraying on the vehicle chassis. The most prominent problem is that high temperature easily causes dust and foreign organisms to stick to the wax film, while low temperature causes the wax film to crack and fall off. Therefore, how to solve the problem of chassis anti-corrosion wax being resistant to high temperatures without sticking and low temperatures without cracking is a problem that needs to be solved for future vehicle exports.
[0004] The existing all-solid wax systems are all vegetable oil systems, which are dried by oxygen curing (for example, CN113402980A, a kind of automobile chassis anti-rust wax and its preparation method). They have high viscosity and require a large amount of mineral oil (≥25%), which leads to slow drying speed. Increasing the drying speed by cobalt-based drying agents will cause serious oil seepage on the surface during the drying process, and it is easy to absorb dust. It cannot meet the requirements of GB / T1728-2020 Method A (blowing cotton ball method), and the film texture is relatively soft and has poor stone impact resistance. This system is more suitable for cavity wax systems with low strength and drying requirements. The cobalt element is safety-restricted and the color is generally dark, so it is not suitable for the chassis corrosion protection requirements of exported vehicles. A large amount of dust and even biological substances will lead to complaints from overseas customers. Summary of the invention
[0005] In order to solve the above-mentioned technical problems, the purpose of the present invention is a liquid all-solid high and low temperature resistant chassis anticorrosion wax. The anticorrosion wax provided by the present invention can achieve a surface dry effect in a relatively short time through oxygen curing and moisture curing at room temperature. Therefore, the present invention does not contain any solvents, and does not need to add additional mineral oil to dilute the viscosity, reaching nearly 100% solid content. At the same time, the present invention forms a double bond and hydroxyl common structure through guarana esterification of epoxy-terminated hydroxyl polybutadiene. The surface layer is in contact with moisture and oxygen in the air, and a non-sticky tough film is formed in a short time, and the microcrystalline wax is enclosed in the film. A dense high-temperature resistant resin film is formed on the surface, and the wax content is small, which avoids the anti-stickiness of the microcrystalline wax under high temperature. At the same time, the inner layer of the film is less and less in contact with the oxygen and moisture of the outer layer, and the degree of cross-linking is getting lower and lower. The wax content in the cross-linked layer is high, and the wax film is getting softer and softer, forming a very good adhesion to the substrate. Under low temperature conditions, it is not easy to crack. Even if the outer layer is broken under the action of external force, the inner wax film is in contact with oxygen and moisture again, and a cross-linked film can be formed again, forming a self-repairing wax film.
[0006] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a liquid all-solid anti-corrosion wax for high and low chassis, characterized in that it includes, by weight, 63 parts of epoxy-terminated hydroxyl polybutadiene guarana ester, 35 parts of microcrystalline wax, 0.3 parts of organic alkoxy titanate chelate, 0.7 parts of organic zirconium chelate, and 1 part of propylene glycol solution of organic iron chelate.
[0007] The above-mentioned liquid all-solid high and low temperature resistant chassis anti-corrosion wax, the preparation method of the epoxy-terminated hydroxyl polybutadiene guarana ester comprises the following steps:
[0008] 1) Hydroxyl-terminated polybutadiene was dissolved in toluene solution, and the catalyst 2-carboxyethylphenylphosphinate CEPPA was added at 1200 rpm.
[0009] After 10 min, formic acid and hydrogen peroxide were added at a certain temperature and stirred at a low speed for 24 hours to carry out epoxidation to obtain a liquid epoxy-terminated hydroxyl polybutadiene and toluene mixture;
[0010] 2) dissolving guarana acid in a mixture of the above-mentioned liquid epoxy-terminated hydroxyl polybutadiene and toluene, adding tert-butyl furancarboxylic acid chromium catalyst to the above-mentioned solution, maintaining a relatively high temperature, stirring at a low speed, dehydrating, and performing an esterification reaction to obtain a toluene solution of epoxy-terminated hydroxyl polybutadiene modified with guarana acid, removing toluene, and obtaining a room temperature liquid epoxy-terminated hydroxyl polybutadiene guarana acid ester.
[0011] In the above-mentioned liquid all-solid high and low temperature resistant chassis anti-corrosion wax, in step 1), the molecular weight of the terminal hydroxyl polybutadiene is 800-1000.
[0012] The above-mentioned liquid all-solid high and low temperature resistant chassis anti-corrosion wax, in step 1), the mass ratio of terminal hydroxyl polybutadiene: 2-carboxyethylphenylphosphinic acid CEPPA: formic acid: hydrogen peroxide = 500:0.2:10:30.
[0013] The above-mentioned liquid all-solid high and low temperature resistant chassis anti-corrosion wax, in step 1), the certain temperature is under the condition of 55°C.
[0014] In the above-mentioned liquid all-solid high and low temperature resistant chassis anti-corrosion wax, in step 2), the higher temperature is 85°C.
[0015] The above-mentioned liquid all-solid high and low temperature resistant chassis anti-corrosion wax is characterized in that the microcrystalline wax has an oil content of 5-8% and a melting point of 78°C.
[0016] The above-mentioned liquid all-solid high and low temperature resistant chassis anti-corrosion wax, the organic alkoxy titanate chelate has a trade name of TYZOR IBAY.
[0017] The above-mentioned liquid all-solid high and low temperature resistant chassis anticorrosive wax has an organic zirconium chelate whose trade name is TYZOR 223. The propylene glycol solution of the organic iron chelate is a propylene glycol solution of a triethanolamine iron complex, and the mass fraction of the triethanolamine iron complex is 35%.
[0018] The above-mentioned method for preparing a liquid all-solid high and low temperature resistant chassis anti-corrosion wax comprises heating 63 parts of epoxy-terminated hydroxyl polybutadiene guarana ester to 90°C, adding 35 parts of microcrystalline wax, dispersing at a high temperature of 1200 rpm, cooling to 50°C, adding 0.3 parts of organic alkoxy titanate chelate and 0.7 parts of organic zirconium chelate, and 1 part of propylene glycol solution of organic iron chelate, stirring to obtain a liquid all-solid high and low temperature resistant chassis anti-corrosion wax.
[0019] Compared with the traditional technology, the invention has the following advantages:
[0020] 1. The fully solid high and low temperature resistant chassis anticorrosion wax provided by the present invention is different from the drying methods of traditional solvent-based anticorrosion wax, water-based anticorrosion wax, and high solid wax. No solvents and mineral oils are introduced into the formula. Oxygen curing and wet curing methods are adopted. Organic titanium, zirconium, and iron driers are used to quickly form a solid film on the surface without oil precipitation, solving the safety and environmental emission problems in the vehicle spraying process. In addition, under the dual drying method, the drying speed is increased by 80% compared with the traditional fully solid wax, ensuring the speed limit problem of the existing passenger car production line and not polluting the assembly line. The polybutadiene structure in the structure of the present invention has high elasticity, can well resist stone impact and protect the electrophoretic layer, while the traditional high solid wax modified with vegetable oil does not have high elasticity and is difficult to resist stone impact.
[0021] 2. The all-solid high and low temperature resistant chassis anti-corrosion wax provided by the present invention adopts guarana esterified epoxy-terminated hydroxyl polybutadiene, which contains double bonds and hydroxyl groups, and is cured by organic zirconium iron chelate and titanate. When the wax film comes into contact with the air, the oxygen and moisture on the surface come into contact with the wax film. Under the action of dual curing, a gradient cross-linked film is formed in a short time, and the degree of cross-linking gradually decreases from the outside to the inside, and a high temperature resistant resin cross-linked film is formed on the surface. Under 120°C, the surface resin layer does not stick back, and there will be no problem of adsorbing pollutants under high temperature conditions. Under low temperature conditions, since the inner wax film has a low degree of cross-linking, a small molecular weight, good toughness, and is not easy to crack, even under external force conditions, the outer wax film on the surface breaks, and the inner wax film comes into contact with moisture and air again. Under the action of the drying agent, the outer high temperature resistant film can continue to be formed, forming a self-repairing wax film. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a mechanism diagram of a liquid all-solid high and low temperature resistant chassis anti-corrosion wax according to the present invention.
[0023] The figure is marked as: 1-oligomeric epoxy-terminated hydroxyl polybutadiene guarana ester crosslinking layer. DETAILED DESCRIPTION
[0024] The present invention is described in detail below with reference to the embodiments.
[0025] Example 1 A liquid all-solid high and low temperature resistant chassis anticorrosion wax
[0026] (I) The formula composition is as follows
[0027] Proportion by weight
[0028]
[0029] In this embodiment, the microcrystalline wax has an oil content of 5-8% and a melting point of 78° C. The trade name of the organic alkoxy titanate chelate is TYZOR IBAY, the trade name of the organic zirconium chelate is TYZOR 223, and the organic iron chelate is a propylene glycol solution of a triethanolamine iron complex (mass fraction of 35%).
[0030] (II) The preparation method is as follows:
[0031] 1. Preparation of epoxy-terminated hydroxyl-polybutadiene guarana ester:
[0032] 500g of hydroxy-terminated polybutadiene (molecular weight 800-1000) is dissolved in 1000mL toluene solution, and 0.2g of catalyst 2-carboxyethylphenylphosphinic acid (CEPPA) is added. After 1200 rpm, 10g of formic acid and 30g of hydrogen peroxide are added at 55°C, and stirred at low speed for 24h to carry out epoxidation to obtain a liquid mixture of epoxy-terminated polybutadiene and toluene. 120g of the above solution is taken, 21g of guarana acid is dissolved in the mixture of the above liquid epoxy polybutadiene resin and toluene, 0.7g of tert-butyl furancarboxylic acid chromium catalyst is added to the above solution, the temperature is maintained at 85°C, stirred at low speed for 6h, and then dehydrated and esterified to obtain a toluene solution of epoxy-terminated polybutadiene modified by guarana acid, and then toluene is distilled off in high-speed dispersion to obtain epoxy-terminated polybutadiene guarana acid ester in liquid form at room temperature.
[0033] 2. Preparation of liquid all-solid high and low temperature resistant chassis anti-corrosion wax:
[0034] Take 63g of the prepared liquid epoxy-terminated hydroxyl polybutadiene guarana ester, heat to 90°C, add microcrystalline wax, disperse at high temperature at 1200 rpm, cool to 50°C, add 0.3g of TYZOR IBAY organic alkoxy titanate chelate, 0.7g of organic zirconium chelate (trade name TYZOR 223), 1g of propylene glycol solution of triethanolamine iron complex (mass fraction of 35%), stir for 10min, and obtain the liquid all-solid high and low temperature resistant chassis anti-corrosion wax of the present invention.
[0035] (III) Comparative proportion and performance testing
[0036] 1. Comparative Example 1
[0037] Linseed oil long oil alkyd resin was used to replace the epoxy-terminated hydroxyl polybutadiene guarana ester in Example 1, and other components and proportions remained unchanged, and the preparation method remained unchanged.
[0038] 2. Comparative Example 2
[0039] Microcrystalline wax (melting point 90° C., oil content 3%) was used to replace the microcrystalline wax in Example 1, and other components and proportions remained unchanged, and the preparation method remained unchanged.
[0040] 3. Comparative Example 3
[0041] The TYZOR IBAY organic alkoxy titanate chelate, the organic zirconium chelate TYZOR 223 and the propylene glycol solution of the triethanolamine iron complex (mass fraction of 35%) in Example 1 are replaced by a cobalt manganese cyclohexane compound drier, and the other components and proportions remain unchanged, and the preparation method remains unchanged.
[0042] 4. Comparative Example 4
[0043] The hydroxy-terminated polybutadiene with a molecular weight of 3000 was used to replace the hydroxy-terminated polybutadiene with a molecular weight of 800-1000 in Example 1, and the other components and proportions remained unchanged, and the preparation method remained unchanged.
[0044] Specific detection technical indicators are shown in Table 1:
[0045] Table 1 Comparison of the performance of the anticorrosive wax prepared in the examples and comparative examples
[0046]
[0047] As can be seen from Table 1, the liquid all-solid high and low temperature resistant chassis anti-corrosion wax is a light yellow flowable liquid at room temperature (25°C), with a flash point ≥200°C, a surface drying time of 1h, a solid content greater than 99.5%, resistance to stone impact (affected area ≤10.7%), high temperature adhesion resistance of 100°C, low temperature cracking resistance of -50°C, and salt spray resistance of 3000h (100 microns).
[0048] Comparative Example 1: The linseed oil long oil alkyd resin system is limited to the oxidation drying method, which is not as fast as the oxygen curing and hydroxyl curing methods of the present invention, and has a high crosslinking density. It cannot meet the drying requirements of GB / T1728 Method A, and is still prone to dust absorption during the later drying process. In addition, the linseed oil long oil alkyd resin itself has a large viscosity, and has a poor viscosity reduction effect on the compatibility of microcrystalline wax, resulting in excessive viscosity and inability to spray directly. Alkyd resin is also unable to wrap a sufficient amount of microcrystalline wax molecules, resulting in a poor surface sealing effect, affecting the salt spray test time. The double bond and hydroxyl dual curing of the present invention can form a dense network structure, which can wrap a large amount of microcrystalline wax microstructures, thereby reducing the attraction between microcrystalline waxes, thereby reducing the overall product viscosity and increasing the salt spray time. Due to the poor crosslinking strength, the linseed oil long oil alkyd resin has an anti-stone impact effect that is not as good as the present invention.
[0049] Comparative Example 2 uses high melting point microcrystalline wax and low oil content. Although the components are very similar to those of Example 1, the high melting point microcrystalline wax and low oil content will directly lead to insufficient adhesion between the inner layer of the wax film and the substrate at low temperatures. Due to the lack of low molecular weight liquid oil, the low polymerized double bonds and hydroxyl curing method of the inner layer cannot bond the high molecular weight wax crystals at low temperatures, resulting in cracking of the inner wax structure due to stress within the crystals. While Example 1 uses medium oil content and medium melting point microcrystalline wax. The wax molecular weight is relatively moderate, and it is diluted with low molecular weight oil. The wax crystals have a smaller tendency to precipitate and better flexibility. With the help of double bonds and hydroxyl groups, it can better help improve the adhesion of the wax at low temperatures and avoid low temperature cracking.
[0050] Comparative Example 3 uses the traditional naphthenate cobalt manganese drier, which will result in too dark a color and EU restrictions, which will have certain restrictions on export vehicles. In terms of drying, the contribution of cobalt manganese drier to surface drying is not as high as that of organic chelate zirconium iron and titanate, and zirconium / titanium can passivate the substrate, improve adhesion, and increase salt spray resistance time.
[0051] Comparative Example 4 uses a large molecular weight of terminal hydroxyl polybutadiene to participate in the reaction. Due to the large molecular weight, liquid epoxy terminal hydroxyl polybutadiene guarana ester cannot be formed during the synthesis process, resulting in the formation of a final solid product that cannot be used.
[0052] The mechanism of liquid all-solid high and low temperature resistant chassis anti-corrosion wax is as follows Figure 1 As shown in the figure, during the drying process, from outside to inside, the degree of crosslinking decreases from high to low. The outer layer is dense, the crosslinking layer contains less wax, and the film has better drying properties. The inner layer has a slightly lower degree of crosslinking, a large amount of wax in the crosslinking layer, good adhesion, and good toughness. And because of the high oil content, at low temperatures, the crystals precipitated by wax are separated by low molecular weight oil, avoiding the cracking problem caused by internal stress.
Claims
1. A liquid all-solid anti-corrosion wax for high and low chassis, characterized in that: The mixture is prepared in proportion by weight and includes 63 parts of epoxy-terminated hydroxyl polybutadiene guarana ester, 35 parts of microcrystalline wax, 0.3 parts of organic alkoxy titanate chelate, 0.7 parts of organic zirconium chelate and 1 part of propylene glycol solution of organic iron chelate.
2. The liquid all-solid high and low temperature resistant chassis anti-corrosion wax according to claim 1, characterized in that: The preparation method of the epoxy-terminated hydroxyl-polybutadiene guarana ester comprises the following steps: 1) Dissolve the hydroxy-terminated polybutadiene in a toluene solution, add a catalyst 2-carboxyethylphenylphosphinic acid CEPPA, add formic acid and hydrogen peroxide at 1200 rpm, stir at a low speed for 24 hours at a certain temperature, and perform epoxidation to obtain a liquid epoxy-terminated hydroxy-terminated polybutadiene and toluene mixture; 2) dissolving guarana acid in a mixture of the above-mentioned liquid epoxy-terminated hydroxyl polybutadiene and toluene, adding tert-butyl furancarboxylic acid chromium catalyst to the above-mentioned solution, maintaining a relatively high temperature, stirring at a low speed, dehydrating, and performing an esterification reaction to obtain a toluene solution of epoxy-terminated hydroxyl polybutadiene modified with guarana acid, removing toluene, and obtaining a room temperature liquid epoxy-terminated hydroxyl polybutadiene guarana acid ester.
3. The liquid all-solid high and low temperature resistant chassis anti-corrosion wax according to claim 2, characterized in that: In step 1), the molecular weight of the hydroxy-terminated polybutadiene is 800-1000.
4. The liquid all-solid high and low temperature resistant chassis anti-corrosion wax according to claim 2, characterized in that: In step 1), the mass ratio of hydroxy-terminated polybutadiene: 2-carboxyethylphenylphosphinic acid CEPPA: formic acid: hydrogen peroxide is 500:0.2:10:
30.
5. The liquid all-solid high and low temperature resistant chassis anti-corrosion wax according to claim 2, characterized in that: In step 1), the certain temperature is 55°C.
6. The liquid all-solid high and low temperature resistant chassis anti-corrosion wax according to claim 2, characterized in that: In step 2), the higher temperature is 85°C.
7. The liquid all-solid high and low temperature resistant chassis anti-corrosion wax according to claim 1, characterized in that: The microcrystalline wax has an oil content of 5-8% and a melting point of 78°C.
8. The liquid all-solid high and low temperature resistant chassis anti-corrosion wax according to claim 1, characterized in that: The trade name of the organic alkoxy titanate chelate is TYZOR IBAY.
9. The liquid all-solid high and low temperature resistant chassis anti-corrosion wax according to claim 1, characterized in that: The trade name of the organic zirconium chelate is TYZOR 223. The propylene glycol solution of the organic iron chelate is a propylene glycol solution of a triethanolamine iron complex, and the mass fraction of the triethanolamine iron complex is 35%.
10. The method for preparing a liquid all-solid high and low temperature resistant chassis anticorrosive wax according to claim 1, characterized in that: Heat 63 parts of epoxy-terminated hydroxyl polybutadiene guarana ester to 90°C, add 35 parts of microcrystalline wax, disperse at high temperature at 1200 rpm, cool to 50°C, add 0.3 parts of organic alkoxy titanate chelate, 0.7 parts of organic zirconium chelate and 1 part of propylene glycol solution of organic iron chelate, stir to obtain a liquid all-solid high and low temperature resistant chassis anti-corrosion wax.
Citation Information
Patent Citations
Anti-rust wax for automobile chassis and preparation method thereof
CN113402980A
Automobile cavity anticorrosion wax and preparation method thereof
CN112029390A
Anti-corrosion wax for automobile chassis and manufacturing process of anti-corrosion wax
CN117210106A
Curable polyolefin composition and cured product
US20240141112A1