Environment-friendly polyamide-imide insulating paint as well as preparation method and application thereof
By using nitrogen-free solvents and adjusting resin raw materials in polyamide-imide insulating paint, the problems of nitrogen oxide emissions and poor resin solubility are solved, and an environmentally friendly polyamide-imide insulating paint is prepared to reduce nitrogen oxides. The compounds emit and ensure the appearance and properties of the enameled wire.
Patent Information
- Application Number
- CN202410917123.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-10
Smart Images

Figure BDA0004935435680000131 
Figure BDA0004935435680000141 
Figure BDA0004935435680000142
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyamide-imide insulating varnish, and in particular to an environmentally friendly polyamide-imide insulating varnish and a preparation method and application thereof. Background Art
[0002] Polyamide-imide is a modified polyimide resin. It is widely used in the automotive industry, electrical and electronic, aviation and other fields due to its excellent heat resistance, flexibility, chemical stability and friction resistance. Polyamide-imide insulating varnish made of polyamide-imide is mainly used in the enameled wire industry.
[0003] At present, the method of synthesizing polyamide-imide mainly uses nitrogen-containing solvents. The polyamide-imide resin in the polyamide-imide insulating varnish is dissolved in N-methylpyrrolidone (NMP), N,N-dimethylacetamide (DMAC) or N,N-dimethylformamide (DMF). During the production process of enameled wire, the solvent is baked at high temperature in the enameling furnace and decomposed into NO, NO2 or other nitrogen oxides before being discharged. At present, when polyamide-imide insulating varnish is used for enameled wire on the market, its nitrogen oxide emissions are about 1500-2000mg / m 3 , nitrogen oxides can destroy the ozone layer and form ozone holes, which is very detrimental to the ecological environment. Therefore, it is urgent to develop an environmentally friendly polyamide-imide insulating varnish with low nitrogen oxide emissions. Summary of the invention
[0004] In order to solve the above technical problems, the purpose of the present invention is to provide an environmentally friendly polyamide-imide insulating varnish and its preparation method and application, using a nitrogen-free solvent to replace the original nitrogen-containing solvent for the production of polyamide-imide insulating varnish, and reducing the emission of nitrogen oxides during the enameled wire operation process by using a nitrogen-free solvent. However, the solubility and reactivity of commonly used polyamide-imide resins in nitrogen-free solvents are relatively poor. Therefore, the present invention also adjusts the type and proportion of raw materials for synthesizing polyamide-imide resins, improves the solubility of nitrogen-free solvents and polyamide-imide resins, and ensures the normal progress of the synthesis reaction, thereby producing an environmentally friendly polyamide-imide insulating varnish for application in the enameled wire industry.
[0005] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0006] A polyamide-imide insulating varnish, which comprises the following components by weight percentage: 20% to 30% of polyamide-imide resin and 70% to 80% of solvent;
[0007] The polyamide-imide resin is obtained by reacting anhydride, acid and isocyanate; the acid is adipic acid (AA) or trimellitic acid;
[0008] The solvent includes:
[0009] Butyrolactone;
[0010] One or both of propylene carbonate and dimethyl dibasic acid ester; and
[0011] One or more of xylene and high-boiling-point petroleum solvent;
[0012] The weight percentage of the butyrolactone in the solvent is 50% to 80%.
[0013] The present invention adopts different solvents in combination to improve the solubility and reactivity of nitrogen-free solvents and polyamide-imide resin. On the one hand, different solvents can improve the viscosity reduction effect of the resin. The combination of different solvents can reduce the viscosity of the insulating paint while keeping the solid content unchanged, which is more convenient for subsequent painting operations. On the other hand, different solvents have different boiling points. During the curing process of the enameled wire, due to the different boiling points of the solvents, the volatilization rate of the solvent can be effectively controlled, thereby ensuring the appearance of the subsequent enameled wire.
[0014] The difference between the polyamide-imide resin of the present invention and the existing polyamide-imide resin is that isocyanates with different structures are introduced, so that normal reaction can be carried out in a reaction system mainly based on ester solvents, and the goal of low nitrogen oxide emissions is achieved while ensuring the appearance and characteristics of the coating.
[0015] Furthermore, the molecular weight of the polyamide-imide resin is 40,000 to 50,000 Da.
[0016] Furthermore, the acid anhydride is selected from one or more of trimellitic anhydride (TMA), maleic anhydride and hexahydrophthalic anhydride, preferably TMA.
[0017] Further, the isocyanate includes 4,4-diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI) and toluene diisocyanate (TDI).
[0018] Among them, TMA and MDI are the main reaction raw materials, HDI can also improve the winding properties, and TDI can also improve the solubility of resin and solvent.
[0019] Furthermore, the molar ratio of the anhydride to the acid is 1:(0.01-0.5), the polyamide-imide structure contains amide and imine groups, the imine groups are mainly obtained by the reaction of the anhydride, and the amide groups are mainly obtained by the reaction of the carboxylic acid, TMA has both anhydride and carboxylic acid, and by using acid to replace part of the anhydride, the proportion of amide groups in the polyamide-imide resin will increase, thereby achieving the purpose of improving the winding property.
[0020] Furthermore, the molar ratio of the acid anhydride to the isocyanate is 1:(0.5-1.5).
[0021] In one embodiment of the present invention, the raw materials for synthesizing the polyamide-imide resin include, by mole percentage, 10% to 50% TMA, 10% to 50% MDI, 0.5% to 15% HDI, 0.5% to 15% TDI, and 1% to 20% AA.
[0022] In one embodiment of the present invention, the raw materials for synthesizing the polyamide-imide resin include, by mole percentage, 40% to 50% TMA, 40% to 50% MDI, 0.5% to 10% HDI, 0.5% to 10% TDI, and 1% to 10% AA.
[0023] In one embodiment of the present invention, the raw materials for synthesizing the polyamide-imide resin include, by mole percentage, 45% to 50% TMA, 40% to 45% MDI, 1% to 5% HDI, 1% to 5% TDI, and 1% to 5% AA.
[0024] Furthermore, the weight percentage of the propylene carbonate in the solvent is 0% to 30%.
[0025] Furthermore, the weight percentage of the dimethyl diacid ester in the solvent is 0% to 30%.
[0026] Furthermore, the weight percentage of xylene in the solvent is 0% to 30%, preferably 10% to 30%.
[0027] Furthermore, the weight percentage of the high boiling point petroleum solvent in the solvent is 0% to 30%, preferably 10% to 20%.
[0028] Furthermore, the high boiling point petroleum solvent includes trimethylbenzene, 100# aromatic solvent oil, and 150# aromatic solvent oil.
[0029] In one embodiment of the present invention, the weight percentage of butyrolactone in the solvent is 50% to 80%, the weight percentage of propylene carbonate and / or dimethyl dibasic acid ester in the solvent is 1% to 30%, and the weight percentage of xylene and / or high-boiling point petroleum solvent in the solvent is 10% to 30%.
[0030] In one embodiment of the present invention, the weight percentage of glycine butyrolactone in the solvent is 50% to 80%, the weight percentage of propylene carbonate and / or dimethyl dibasic acid ester in the solvent is 10% to 30%, and the weight percentage of xylene and / or high-boiling point petroleum solvent in the solvent is 10% to 20%.
[0031] A method for preparing a polyamide-imide insulating varnish comprises the following steps:
[0032] Adding a first solvent, anhydride, acid and isocyanate into a reaction kettle, raising the temperature in stages to react under an inert atmosphere, cooling to 60-80° C., adding a second solvent to dilute, and obtaining the polyamide-imide insulating varnish;
[0033] The first solvent comprises:
[0034] butyrolactone; and
[0035] One or both of propylene carbonate and dimethyl dibasic acid ester;
[0036] The acid is adipic acid (AA) or trimellitic acid;
[0037] The second solvent includes one or more of xylene and high-boiling-point petroleum solvent;
[0038] The specific method of the staged heating is: raising the temperature to 60-70°C within 1-2 hours, maintaining at 60-70°C for 1-3 hours, raising the temperature to 80-90°C within 2-4 hours, raising the temperature to 100-120°C within 2-4 hours, and raising the temperature to 130-140°C within 1-3 hours.
[0039] Furthermore, the reaction is carried out at a constant temperature of 130-140° C., and the polymerization degree (molecular weight) of the product is tested. When the molecular weight reaches the desired range, the reaction is terminated.
[0040] Furthermore, the reaction can be terminated by adding 5% to 10% by weight of the first solvent to reduce the temperature to 60 to 80° C.
[0041] The staged heating in the preparation method of the present invention is to prevent the risk of punching and overflowing caused by violent reactions. If the temperature is directly raised to 130-140° C., good polyamide-imide insulating varnish cannot be prepared, and the reaction in the middle is relatively violent, which poses a safety hazard.
[0042] Furthermore, the acid anhydride is selected from one or more of trimellitic anhydride (TMA), maleic anhydride and hexahydrophthalic anhydride, preferably TMA, and the isocyanate includes 4,4-diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI) and toluene diisocyanate (TDI).
[0043] Among them, TMA and MDI are the main reaction raw materials, HDI can also improve the winding properties, and TDI can also improve the solubility of resin and solvent.
[0044] Furthermore, the molar ratio of the acid anhydride to the acid is 1:(0.01-0.5), and the acid can replace a portion of the acid anhydride and play a role in improving the winding properties.
[0045] Furthermore, the molar ratio of the acid anhydride to the isocyanate is 1:(0.5-1.5).
[0046] In one embodiment of the present invention, the raw materials for synthesizing the polyamide-imide resin include, by mole percentage, 10% to 50% TMA, 10% to 50% MDI, 0.5% to 15% HDI, 0.5% to 15% TDI, and 1% to 20% AA.
[0047] In one embodiment of the present invention, the raw materials for synthesizing the polyamide-imide resin include, by mole percentage, 40% to 50% TMA, 40% to 50% MDI, 0.5% to 10% HDI, 0.5% to 10% TDI, and 1% to 10% AA.
[0048] In one embodiment of the present invention, the raw materials for synthesizing the polyamide-imide resin include, by mole percentage, 45% to 50% TMA, 40% to 45% MDI, 1% to 5% HDI, 1% to 5% TDI, and 1% to 5% AA.
[0049] In one embodiment of the present invention, the weight percentage of butyrolactone in the solvent is 50% to 80%, the weight percentage of propylene carbonate and / or dimethyl dibasic acid ester in the solvent is 1% to 30%, and the weight percentage of xylene and / or high-boiling point petroleum solvent in the solvent is 10% to 30%.
[0050] In one embodiment of the present invention, the weight percentage of glycine butyrolactone in the solvent is 50% to 80%, the weight percentage of propylene carbonate and / or dimethyl dibasic acid ester in the solvent is 10% to 30%, and the weight percentage of xylene and / or high-boiling point petroleum solvent in the solvent is 10% to 20%.
[0051] In a specific embodiment, a first solvent is added to a reaction kettle, and anhydride, acid and isocyanate are added under an inert atmosphere, the temperature is raised in stages for reaction, and after cooling to 60-80° C., a second solvent is added for dilution to obtain the polyamideimide insulating varnish.
[0052] In a specific embodiment, a first solvent (accounting for 50% to 60% by weight of the total solvent, the total solvent is the first solvent and the second solvent) is added to a reaction kettle, anhydride, acid and isocyanate are added under an inert atmosphere, the temperature is raised in stages to react, the first solvent (accounting for 10% to 30% by weight of the total solvent) is added and the temperature is lowered to 60 to 80°C, and the second solvent (accounting for 10% to 30% by weight of the total solvent) is added for dilution to obtain the polyamide-imide insulating varnish.
[0053] The present invention also protects the use of the environmentally friendly polyamide-imide insulating varnish in preparing enameled wires.
[0054] Compared with the prior art, the present invention has the following beneficial effects:
[0055] The present invention adopts a solvent without nitrogen element to replace the original nitrogen-containing solvent for the production of polyamide-imide insulating varnish, adjusts the type and proportion of raw materials for synthesizing polyamide-imide resin, improves the solubility of the nitrogen-free solvent and the polyamide-imide resin, so as to ensure the normal progress of the synthesis reaction, thereby producing an environmentally friendly polyamide-imide insulating varnish for application in the enameled wire industry and reducing the emission of nitrogen oxides in the enameled wire operation process. DETAILED DESCRIPTION
[0056] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0057] The present invention is further described below in conjunction with specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0058] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.
[0059] In the following examples, gel chromatography was used to test the degree of polymerization (molecular weight).
[0060] Example 1
[0061] A polyamide-imide insulating varnish comprises the following components by weight percentage: 30% polyamide-imide resin and 70% solvent; the solvent comprises by weight percentage: 66% butyrolactone, 20% dibasic acid dimethyl ester and 14% xylene.
[0062] The polyamide-imide insulating varnish of Example 1 is prepared according to the following method:
[0063] Add butyrolactone and dimethyl dibasic acid to the reactor, add TMA, MDI, HDI, TDI and AA (by mole percentage: TMA 48%, MDI 42%, HDI 4%, TDI 4%, AA 2%) under nitrogen atmosphere while stirring, raise the temperature to 65°C for 1 hour, maintain at 65°C for 2 hours, raise the temperature to 85°C for 3 hours, raise the temperature to 110°C within 3 hours, raise the temperature to 130°C within 2 hours, react at a constant temperature at 130°C, and test the degree of polymerization (molecular weight). When the molecular weight of the polyamide-imide resin reaches 41500Da, add butyrolactone and dimethyl dibasic acid, lower the temperature to 80°C to terminate the reaction, add xylene for dilution and adjustment of the final physical properties, filter and barrel after the adjustment.
[0064] Example 2
[0065] A polyamide-imide insulating varnish comprises the following components by weight percentage: 20% polyamide-imide resin and 80% solvent; the solvent comprises by weight percentage: 50% butyrolactone, 30% propylene carbonate and 20% xylene.
[0066] The polyamide-imide insulating varnish of Example 2 is prepared according to the following method:
[0067] Add butyrolactone and propylene carbonate to the reactor, and add TMA, MDI, HDI, TDI and AA (in molar percentage: TMA 42%, MDI 43%, HDI 5%, TDI 5%, AA 5%) under nitrogen atmosphere while stirring, raise the temperature to 65°C for 1 hour, maintain at 65°C for 2 hours, raise the temperature to 85°C for 3 hours, raise the temperature to 110°C within 3 hours, raise the temperature to 130°C within 2 hours, react at a constant temperature at 130°C, and test the degree of polymerization (molecular weight). When the molecular weight of the polyamide-imide resin reaches 47890Da, add butyrolactone and propylene carbonate, cool to 80°C to terminate the reaction, add xylene for dilution and adjustment of the final physical properties, filter and barrel after the adjustment.
[0068] Example 3
[0069] A polyamide-imide insulating varnish comprises the following components by weight percentage: 30% polyamide-imide resin and 70% solvent; the solvent comprises by weight percentage: 75% butyrolactone, 15% dibasic acid dimethyl ester and 10% 100# aromatic solvent oil.
[0070] The polyamide-imide insulating varnish of Example 3 is prepared according to the following method:
[0071] Add butyrolactone and dimethyl dibasic acid to the reactor, add TMA, MDI, HDI, TDI and AA (by mole percentage: TMA 50%, MDI 40%, HDI 4%, TDI 4%, AA 2%) under nitrogen atmosphere while stirring, raise the temperature to 65°C for 1 hour, maintain at 65°C for 2 hours, raise the temperature to 85°C for 3 hours, raise the temperature to 110°C within 3 hours, raise the temperature to 130°C within 2 hours, react at a constant temperature at 130°C, and test the degree of polymerization (molecular weight). When the molecular weight of the polyamide-imide resin reaches 40500Da, add butyrolactone and dimethyl dibasic acid, lower the temperature to 80°C to terminate the reaction, add 100# aromatic solvent oil for dilution and adjustment of the final physical properties, filter and barrel after the adjustment.
[0072] Example 4
[0073] A polyamide-imide insulating varnish comprises the following components by weight percentage: 30% polyamide-imide resin and 70% solvent; the solvent comprises by weight percentage: 70% butyrolactone, 8% propylene carbonate, 7% dibasic acid dimethyl ester, 10% xylene and 5% 100# aromatic solvent oil.
[0074] The polyamide-imide insulating varnish of Example 4 was prepared according to the following method:
[0075] Add butyrolactone, propylene carbonate and dimethyl dibasic acid into the reactor, add TMA, MDI, HDI, TDI and AA (by mole percentage: TMA 48%, MDI 42%, HDI 4%, TDI 4%, AA 2%) under nitrogen atmosphere while stirring, raise the temperature to 65°C for 1 hour, maintain at 65°C for 2 hours, raise the temperature to 85°C for 3 hours, raise the temperature to 110°C within 3 hours, raise the temperature to 130°C within 2 hours, react at a constant temperature at 130°C, and test the degree of polymerization (molecular weight). When the molecular weight of the polyamide-imide resin reaches 42000Da, add butyrolactone, propylene carbonate and dimethyl dibasic acid, cool to 80°C to terminate the reaction, add xylene and 100# aromatic solvent oil for dilution and adjustment of the final physical properties, filter and barrel after the adjustment.
[0076] Comparative Example 1
[0077] A polyamide-imide insulating varnish comprises the following components by weight percentage: 30% polyamide-imide resin and 70% solvent; the solvent comprises by weight percentage: 80% butyrolactone and 20% xylene.
[0078] The polyamide-imide insulating varnish of Comparative Example 1 was prepared according to the following method:
[0079] Add butyrolactone to the reactor, and add TMA, MDI, HDI, TDI and AA (by mole percentage: TMA 48%, MDI 42%, HDI 4%, TDI 4%, AA 2%) under nitrogen atmosphere while stirring, raise the temperature to 65°C for 1 hour, maintain at 65°C for 2 hours, raise the temperature to 85°C for 3 hours, raise the temperature to 110°C within 3 hours, raise the temperature to 130°C within 2 hours, react at a constant temperature at 130°C, and test the degree of polymerization (molecular weight). When the molecular weight of the polyamide-imide resin reaches 42800Da, add butyrolactone and cool to 80°C to terminate the reaction, add xylene for dilution and adjustment of the final physical properties, filter and barrel after the adjustment.
[0080] Comparative Example 2
[0081] A polyamide-imide insulating varnish comprises the following components by weight percentage: 30% polyamide-imide resin and 70% solvent; the solvent comprises by weight percentage: 80% butyrolactone and 20% 100# aromatic solvent oil.
[0082] The polyamide-imide insulating varnish of Comparative Example 2 was prepared according to the following method:
[0083] Add butyrolactone to the reactor, and add TMA, MDI, HDI, TDI and AA (by mole percentage: TMA 48%, MDI 45%, HDI 2%, TDI 3%, AA 2%) under nitrogen atmosphere while stirring, raise the temperature to 65°C for 1 hour, maintain at 65°C for 2 hours, raise the temperature to 85°C for 3 hours, raise the temperature to 110°C within 3 hours, raise the temperature to 130°C within 2 hours, react at a constant temperature at 130°C, and test the degree of polymerization (molecular weight). When the molecular weight of the polyamide-imide resin reaches 42560Da, add butyrolactone and cool to 80°C to terminate the reaction, add 100# solvent oil for dilution and adjustment of the final physical properties, filter and barrel after the adjustment.
[0084] Comparative Example 3
[0085] A polyamide-imide insulating varnish comprises the following components by weight percentage: 30% polyamide-imide resin and 70% solvent; the solvent comprises by weight percentage: 80% dibasic acid dimethyl ester and 20% xylene.
[0086] The polyamide-imide insulating varnish of Comparative Example 3 was prepared according to the following method:
[0087] Add dimethyl diacid to the reactor, and add TMA, MDI, HDI, TDI and AA (by mole percentage: TMA 48%, MDI 42%, HDI 4%, TDI 4%, AA 2%) under nitrogen atmosphere while stirring, raise the temperature to 65°C in 1 hour, maintain at 65°C for 2 hours, raise the temperature to 85°C in 3 hours, raise the temperature to 110°C within 3 hours, raise the temperature to 130°C within 2 hours, react at a constant temperature at 130°C, and test the degree of polymerization (molecular weight). When the molecular weight of the polyamide-imide resin reaches 43000Da, add dimethyl diacid and cool to 80°C to terminate the reaction, add xylene for dilution and adjustment of the final physical properties, filter and barrel after the adjustment.
[0088] Comparative Example 4
[0089] A polyamide-imide insulating varnish comprises the following components by weight percentage: 30% polyamide-imide resin and 70% solvent; the solvent comprises by weight percentage: 20% butyrolactone, 66% dibasic acid dimethyl ester and 14% xylene.
[0090] The polyamide-imide insulating varnish of Comparative Example 4 was prepared according to the following method:
[0091] Add butyrolactone and dimethyl dibasic acid to the reactor, add TMA, MDI, HDI, TDI and AA (by mole percentage: TMA 48%, MDI 42%, HDI 4%, TDI 4%, AA 2%) under nitrogen atmosphere while stirring, raise the temperature to 65°C for 1 hour, maintain at 65°C for 2 hours, raise the temperature to 85°C for 3 hours, raise the temperature to 110°C within 3 hours, raise the temperature to 130°C within 2 hours, react at a constant temperature at 130°C, and test the degree of polymerization (molecular weight). When the molecular weight of the polyamide-imide resin reaches 41980Da, add butyrolactone and cool to 80°C to terminate the reaction, add xylene for dilution and adjustment of the final physical properties, filter and barrel after the adjustment.
[0092] Comparative Example 5
[0093] A polyamide-imide insulating varnish comprises the following components by weight percentage: 30% polyamide-imide resin and 70% solvent; the solvent comprises by weight percentage: 66% butyrolactone, 20% dibasic acid dimethyl ester and 14% xylene.
[0094] The polyamide-imide insulating varnish of Comparative Example 5 was prepared according to the following method:
[0095] Add butyrolactone and dimethyl dibasic acid to the reactor, add TMA, MDI and AA (by mole percentage: TMA 48%, MDI 50%, AA 2%) while stirring under a nitrogen atmosphere, raise the temperature to 65°C for 1 hour, maintain at 65°C for 2 hours, raise the temperature to 85°C for 3 hours, raise the temperature to 110°C within 3 hours, raise the temperature to 130°C within 2 hours, react at a constant temperature at 130°C, and test the degree of polymerization (molecular weight). When the molecular weight of the polyamide-imide resin reaches 44500Da, add butyrolactone and dimethyl dibasic acid, lower the temperature to 80°C to terminate the reaction, add xylene for dilution and adjustment of the final physical properties, filter and barrel after the adjustment.
[0096] Comparative Example 6
[0097] A polyamide-imide insulating varnish comprises the following components by weight percentage: 30% polyamide-imide resin and 70% solvent; the solvent comprises by weight percentage: 66% butyrolactone, 20% dibasic acid dimethyl ester and 14% xylene.
[0098] The polyamide-imide insulating varnish of Comparative Example 6 was prepared according to the following method:
[0099] Add butyrolactone and dimethyl dibasic acid to the reactor, add TMA, MDI, HDI and TDI (by mole percentage: TMA 50%, MDI 42%, HDI 4%, TDI 4%) while stirring under a nitrogen atmosphere, raise the temperature to 65°C for 1 hour, maintain at 65°C for 2 hours, raise the temperature to 85°C for 3 hours, raise the temperature to 110°C within 3 hours, raise the temperature to 130°C within 2 hours, react at a constant temperature at 130°C, and test the degree of polymerization (molecular weight). When the molecular weight of the polyamide-imide resin reaches 57,800 Da, add butyrolactone and dimethyl dibasic acid, lower the temperature to 80°C to terminate the reaction, add xylene for dilution and adjustment of the final physical properties, filter and barrel after the adjustment.
[0100] Comparative Example 7
[0101] A polyamide-imide insulating varnish comprises the following components by weight percentage: 30% polyamide-imide resin and 70% solvent; the solvent comprises by weight percentage: 66% butyrolactone, 20% dibasic acid dimethyl ester and 20% diphenol.
[0102] The polyamide-imide insulating varnish of Comparative Example 7 was prepared according to the following method:
[0103] Add butyrolactone and dimethyl dibasic acid to the reactor, add TMA, MDI, HDI, TDI and AA (by mole percentage: TMA 48%, MDI 42%, HDI 4%, TDI 4%, AA 2%) under nitrogen atmosphere while stirring, raise the temperature to 65°C for 1 hour, maintain at 65°C for 2 hours, raise the temperature to 85°C for 3 hours, raise the temperature to 110°C within 3 hours, raise the temperature to 130°C within 2 hours, react at a constant temperature at 130°C, and test the degree of polymerization (molecular weight). When the molecular weight of the polyamide-imide resin reaches 43500Da, add butyrolactone and dimethyl dibasic acid, lower the temperature to 80°C to terminate the reaction, add diphenol for dilution and adjustment of the final physical properties, filter and barrel after the adjustment.
[0104] Comparative Example 8
[0105] A polyamide-imide insulating varnish comprises the following components by weight percentage: 30% polyamide-imide resin and 70% solvent; the solvent comprises by weight percentage: 66% butyrolactone, 20% dibasic acid dimethyl ester and 14% xylene.
[0106] The polyamide-imide insulating varnish of Comparative Example 8 was prepared according to the following method:
[0107] Add butyrolactone and dimethyl dibasic acid to the reactor, add TMA, MDI, HDI, TDI and AA (by mole percentage: TMA 48%, MDI 42%, HDI 4%, TDI 4%, AA 2%) under nitrogen atmosphere while stirring, raise the temperature to 130°C within 11 hours, react at a constant temperature at 130°C, and test the degree of polymerization (molecular weight). When the molecular weight of the polyamide-imide resin reaches 47600Da, add butyrolactone and dimethyl dibasic acid, cool to 80°C to terminate the reaction, add xylene for dilution and adjustment of the final physical properties, filter and barrel after the adjustment.
[0108] Comparative example: Commercial polyamide-imide insulating varnish
[0109] A polyamide-imide insulating varnish comprises the following components by weight percentage: 30% polyamide-imide resin and 70% solvent; the solvent comprises by weight percentage: 60% NMP, 15% DMAC, 10% DMF and 15% xylene.
[0110] The polyamide-imide insulating varnish of the control example was prepared according to the following method:
[0111] NMP and DMAC were added to the reactor, and TMA and MDI (by mole percentage: TMA 50%, MDI 50%) were added while stirring under a nitrogen atmosphere. The temperature was raised to 65°C for 1 hour, maintained at 65°C for 2 hours, raised to 85°C for 3 hours, raised to 110°C within 3 hours, and raised to 130°C within 2 hours. The reaction was carried out at a constant temperature of 130°C, and the degree of polymerization (molecular weight) was tested. When the molecular weight of the polyamide-imide resin reached 41500Da, NMP was added to cool the temperature to 80°C to terminate the reaction, and DMF was added for dilution and adjustment of the final physical properties. After the adjustment, the mixture was filtered and barreled.
[0112] Test Example 1
[0113] The reaction system state, coating appearance and state after storage at room temperature for 3 months of the polyamide-imide insulating varnish of Examples 1 to 4, Comparative Examples 1 to 8 and the reference example were observed. The results are shown in Table 1:
[0114] Table 1
[0115]
[0116]
[0117] Since the polyamide-imide insulating varnishes prepared in Comparative Examples 3 to 5 and Comparative Example 7 had turbid appearance, their viscosity over time was not tested.
[0118] The solvent of Comparative Example 3 does not contain butyrolactone, and the content of butyrolactone in the solvent of Comparative Example 4 is reduced, and the appearance of the prepared coating is turbid, which proves that the solubility of dimethyl dibasic acid in polyamide-imide resin is worse than that of butyrolactone; the raw material for synthesizing polyamide-imide resin in Comparative Example 5 does not contain HDI and TDI, resulting in poor solubility of resin and solvent, and the appearance of the reaction system and the coating is turbid; the raw material for synthesizing polyamide-imide resin in Comparative Example 6 does not contain AA, the molecular weight of the resin becomes higher, and the viscosity increases after storage at room temperature for 3 months, because AA is an aliphatic structure with a long straight chain, which can effectively regulate the reactivity and the later coating preservation during the reaction with the NCO group; Comparative Example 7 uses diphenol to replace xylene, resulting in a turbid appearance of the coating, indicating that diphenol has poor solubility in polyamide-imide; Comparative Example 8 does not use staged heating to react, resulting in a more violent reaction during the reaction process, severe floating of the liquid level, and a risk of overflow. At the same time, when performing polymerization degree detection, it is difficult to control the molecular weight we need.
[0119] Test Example 2
[0120] The polyamide-imide insulating varnish of Example 1, Comparative Examples 1-2 and Reference Example is used to prepare enameled wire, and the preparation method is as follows:
[0121] A heat exchange enameling furnace was used, the furnace length was 3.8 meters, the inlet and outlet temperatures were 440℃ / 480℃, the wire gauge was 0.4mm, the line speed was 12m / min, and the number of coating times was 7 times.
[0122] The prepared enameled wire was tested for relevant wire properties (enameled wire testing standard: GB / T6109.14-2008 / IEC60317-26:1990), and a third-party testing agency was commissioned to place a nitrogen oxide detection device at the discharge port of the enameling furnace to test the nitrogen oxide content during the enameled wire operation. The test results are shown in Table 2:
[0123] Table 2
[0124]
[0125]
[0126] From the test results in Table 2, it can be seen that the nitrogen oxide emissions of Example 1 and Comparative Examples 1-2 are much lower than those of the control example, meeting the comprehensive emission standard for atmospheric pollutants DB32 / 4041-2021 (the nitrogen oxide emission standard is 200 mg / m 3 ); The appearance of the enameled wires prepared in Comparative Examples 1 and 2 has particles. This is because Comparative Examples 1 and 2 only have two solvents, and the proportion of high-boiling point solvents is relatively high. When the coating is in the enameled wire operation, the amount of solvent volatilization is large when the coating passes through the evaporation section, which easily leads to particles on the surface of the wire. In Example 1, three solvents are used. The different boiling points of the three solvents can effectively control the solvent volatilization rate when entering the evaporation section, thereby ensuring that the enameled wire achieves a better appearance. Therefore, the appearance of the enameled wires prepared in Example 1 and the control example is equivalent; in terms of characteristics, the enameled wire prepared in Example 1 has better paint shrinkage (adhesion) and softening resistance (heat resistance) than the control example.
[0127] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A polyamide-imide insulating varnish, characterized in that: The polyamide-imide insulating varnish comprises the following components by weight percentage: 20% to 30% of polyamide-imide resin and 70% to 80% of solvent; The polyamide-imide resin is obtained by reacting anhydride, acid and isocyanate; the acid is adipic acid or trimellitic acid; The solvent includes: Butyrolactone; One or both of propylene carbonate and dimethyl dibasic acid ester; and One or more of xylene and high-boiling-point petroleum solvent; The weight percentage of the butyrolactone in the solvent is 50% to 80%.
2. The polyamide-imide insulating varnish according to claim 1, characterized in that: The weight percentage of the propylene carbonate in the solvent is 0% to 30%.
3. The polyamide-imide insulating varnish according to claim 1, characterized in that: The weight percentage of the dimethyl dibasic acid ester in the solvent is 0% to 30%.
4. The polyamide-imide insulating varnish according to any one of claims 1 to 3, characterized in that: The weight percentage of xylene in the solvent is 0% to 30%.
5. The polyamide-imide insulating varnish according to any one of claims 1 to 3, characterized in that: The weight percentage of the high boiling point petroleum solvent in the solvent is 0% to 30%.
6. A method for preparing a polyamide-imide insulating varnish, characterized in that: The following steps are involved: Adding a first solvent, anhydride, acid and isocyanate into a reaction kettle, raising the temperature in stages to react under an inert atmosphere, cooling to 60-80° C., adding a second solvent to dilute, and obtaining the polyamide-imide insulating varnish; The first solvent comprises: butyrolactone; and One or both of propylene carbonate and dimethyl dibasic acid ester; The acid is adipic acid or trimellitic acid; The second solvent includes one or more of xylene and high-boiling-point petroleum solvent; The specific method of the staged heating is: raising the temperature to 60-70°C within 1-2 hours, maintaining at 60-70°C for 1-3 hours, raising the temperature to 80-90°C within 2-4 hours, raising the temperature to 100-120°C within 2-4 hours, and raising the temperature to 130-140°C within 1-3 hours.
7. The preparation method according to claim 6, characterized in that: The acid anhydride is selected from one or more of trimellitic anhydride, maleic anhydride and hexahydrophthalic anhydride, and the isocyanate includes 4,4-diphenylmethane diisocyanate, hexamethylene diisocyanate and toluene diisocyanate.
8. The preparation method according to claim 6 or 7, characterized in that: The molar ratio of the acid anhydride to the acid is 1:(0.01-0.5).
9. The preparation method according to claim 6 or 7, characterized in that: The molar ratio of the acid anhydride to the isocyanate is 1:(0.5-1.5).
10. Use of the polyamide-imide insulating varnish according to any one of claims 1 to 5 or the polyamide-imide insulating varnish prepared by the method according to any one of claims 6 to 9 in preparing enameled wires.
Citation Information
Patent Citations
Polyamide resin, resin composition thereof, flame-retardant adhesive composition and adhesive sheet made of said composition, coverlay film, and printed wiring board
CN102171263A
Preparation method for environmental protection type polyamide-imide wire enamel
CN102942815A
Environment-friendly high-adhesion polyamide-imide paint and preparation method thereof
CN104152037A
Amide-imide resin for production of heat resistant fiber
CN1067436A
High-adhesiveness insulated base coat for enameled wire and preparation method of insulated base coat
CN109181527A