Preparation method and application of water-dispersible zinc oxide quantum dots with adjustable and controllable fluorescence color
By changing the temperature and zinc-base concentration ratio of the sol-gel method, combined with APTES surface modification, water-dispersed zinc oxide quantum dots with multiple fluorescent colors were prepared, which solved the problem of insufficient fluorescence performance of zinc oxide quantum dots in aqueous solutions in the existing technology. The problem of stability is achieved, the fluorescent color can be controlled and stably dispersed, and its application scope is expanded.
Patent Information
- Application Number
- CN202410884763.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-15
AI Technical Summary
The fluorescence properties of existing zinc oxide quantum dots prepared by the sol-gel method are unstable in aqueous solutions, and the increase in particle size leads to a red shift and quenching of the fluorescence color, which limits the application of multi-color fluorescent zinc oxide quantum dots in aqueous environments. .
Using Zn(Ac)2 and LiOH as raw materials, by changing the temperature and zinc-alkali concentration ratio, combined with APTES surface modifier, zinc oxide quantum dots with multiple fluorescent colors and water dispersibility were prepared to achieve fluorescent colors in a larger wavelength range Adjustable within.
Successfully prepared zinc oxide quantum dots in various fluorescent colors such as blue, green, and yellow, with particle sizes of 2.5nm, 3.6nm, and 4.3nm. They have good crystal structure and stable water dispersion, and the fluorescence emission peak ranges from the blue light band to The orange-yellow light band can be controlled, which expands its application prospects in the fields of fluorescent inks, light-emitting diodes, and cell imaging.
Smart Images

Figure CN118772871A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of water-dispersible zinc oxide quantum dots with adjustable fluorescent color, belonging to the technical field of fluorescent materials. Background Art
[0002] Zinc oxide quantum dots (ZnO QDs) are a II-VI wide bandgap direct bandgap semiconductor material with a particle size between 1nm and 10nm. They can be excited by ultraviolet light to emit fluorescence at room temperature and are an excellent fluorescent material. Compared with cadmium and selenium quantum dots, ZnO QDs have diverse preparation methods, are environmentally friendly, and have no biological toxicity. They have been widely used in light-emitting diodes, anti-counterfeiting printing, cell imaging and other fields.
[0003] Common methods for preparing ZnO QDs include hydrothermal method, microemulsion method, sol-gel method, etc. Among them, sol-gel method has become the mainstream preparation method due to its advantages of simple operation, controllable reaction conditions, easy doping, surface modification, and relatively uniform particle size distribution of prepared ZnO QDs. Han et al. used ZnCl2 and LiOH as raw materials and prepared blue and green fluorescent ZnO QDs by sol-gel method by changing the molar ratio of LiOH to ZnCl2; Ye et al. used Zn(Ac)2 and LiOH as raw materials and prepared blue-green to yellow-green fluorescent ZnO QDs by adjusting the reaction conditions, and determined the conditions for fluorescence tuning of ZnO quantum dots. Although the ZnO QDs prepared by the above sol-gel method can achieve the controllable spectral range of the fluorescent color part, the fluorescence performance is unstable in aqueous solution. The reason is that ZnO QDs have a high surface energy and will agglomerate in water, causing the particle size to increase and the fluorescence color to red-shift. When the particle size increases to a certain extent, the fluorescence is quenched. This phenomenon limits the application of multicolor fluorescent ZnO QDs in aqueous environments. Summary of the invention
[0004] The purpose of the present invention is to solve the deficiencies of the prior art and provide a method for preparing water-dispersible zinc oxide quantum dots with adjustable fluorescence color. The method uses Zn(Ac)2 and LiOH as raw materials and APTES as a surface modifier. By changing the process conditions such as temperature and zinc-alkali concentration ratio, multi-fluorescent color, water-dispersible ZnO QDs are prepared, and the fluorescence color of ZnOQDs can be adjusted within a large wavelength range. The specific scheme is as follows:
[0005] A method for preparing water-dispersible zinc oxide quantum dots with adjustable fluorescent color comprises the following steps:
[0006] (1) adding zinc acetate dihydrate to anhydrous ethanol and stirring until completely dissolved to obtain a zinc acetate ethanol solution;
[0007] (2) adding lithium hydroxide to anhydrous ethanol and stirring evenly to obtain a lithium hydroxide ethanol solution, adding the lithium hydroxide ethanol solution to the zinc acetate ethanol solution obtained in step (1), stirring to react, and obtaining a ZnO QDs solution;
[0008] (3) Add 3-aminopropyltriethoxysilane to deionized water, mix well, and then add the obtained solution dropwise to the ZnO QDs solution obtained in step (2). After stirring for reaction, collect the precipitate by centrifugation, wash and dry to obtain the product.
[0009] In step (2), the stirring reaction temperature is 0-80°C.
[0010] Furthermore, in step (2), the molar ratio of zinc acetate dihydrate to lithium hydroxide is 1:(1-4).
[0011] Furthermore, in step (3), the centrifugal conditions are: 8000 r / min, 5 min.
[0012] Furthermore, in step (3), the washing method uses anhydrous ethanol, and the number of washing times is 3-5 times.
[0013] Furthermore, in step (3), the drying temperature is 50-60° C. and the drying time is 4-6 hours.
[0014] The water-dispersible zinc oxide quantum dots with adjustable fluorescent color are prepared by the above method.
[0015] The water-dispersible zinc oxide quantum dots with adjustable fluorescent color prepared by the above method are used in the preparation of fluorescent ink.
[0016] The water-dispersible zinc oxide quantum dots with adjustable fluorescence color prepared by the above method are applied in light-emitting diodes and cell imaging.
[0017] Beneficial effects of the present invention:
[0018] 1) The present invention adopts a sol-gel method to prepare water-dispersible ZnO QDs with adjustable fluorescence color. By changing the reaction conditions, ZnO QDs with different fluorescence emission peaks can be obtained, thereby achieving the regulation of the fluorescence emission peak of ZnO QDs from the blue light band to the orange-yellow light band.
[0019] 2) The present invention uses LiOH as an alkali source to prepare ZnO QDs with various fluorescent colors such as yellow, green, and blue, which solves the problem that other alkali sources cannot prepare blue fluorescent ZnO QDs, provides an experimental scheme for the controllable preparation of multi-color fluorescent ZnO QDs, and expands its application prospects.
[0020] 3) The blue, green and yellow fluorescent ZnO QDs prepared by the method of the present invention have a particle size of 2.5 nm, 3.6 nm and 4.3 nm, have a good crystal structure, and are successfully modified by APTES, and can be stably dispersed in aqueous solution. The corresponding fluorescence emission peaks are 480 nm, 518 nm and 568 nm, respectively. The difference in their fluorescent colors is caused by surface defects. The yellow and green fluorescence originate from oxygen vacancies, and the blue fluorescence originates from zinc interstitials.
[0021] 4) The water-dispersible zinc oxide quantum dots with adjustable fluorescence color prepared by the present invention can be used to prepare fluorescent inks, and can also be used in the fields of light-emitting diodes, cell imaging, etc., and have good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The fluorescence emission spectra of ZnO QDs prepared in Examples 1-5;
[0023] Figure 2 The fluorescence emission spectra of ZnO QDs prepared in Example 1 and Examples 6-9;
[0024] Figure 3 TEM images of ZnO QDs prepared in Example 4, Example 6, and Example 8;
[0025] Figure 4 This is a size distribution diagram of ZnO QDs prepared in Example 4, Example 6, and Example 8;
[0026] Figure 5 XRD diffraction patterns of ZnO QDs prepared in Example 4, Example 6, and Example 8;
[0027] Figure 6 FTIR spectra of ZnO QDs prepared in Example 4, Example 6, and Example 8;
[0028] Figure 7 This is the full XPS spectrum of ZnO QDs prepared in Example 4, Example 6, and Example 8;
[0029] Figure 8 The UV-visible absorption spectra and absorption band gap diagrams of ZnO QDs prepared in Example 4, Example 6, and Example 8;
[0030] Fig. 9 Actual pictures of ZnO QDs prepared in Example 4, Example 6, and Example 8 under sunlight and ultraviolet light;
[0031] Fig.10 The fluorescence emission spectra and color gamut diagrams of ZnO QDs prepared in Example 4, Example 6, and Example 8;
[0032] Fig.11 This is a combined pattern printed using the ZnO QDs prepared in Example 4, Example 6, and Example 8. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is clearly and completely described below in conjunction with the accompanying drawings and specific embodiments.
[0034] Example 1
[0035] A method for preparing water-dispersible zinc oxide quantum dots with adjustable fluorescent color comprises the following steps:
[0036] (1) adding 10 mmol of zinc acetate dihydrate to 100 mL of anhydrous ethanol and stirring the mixture under magnetic stirring at 78° C. until the mixture is completely dissolved to obtain a zinc acetate ethanol solution;
[0037] (2) adding 10 mmol of lithium hydroxide to 100 mL of anhydrous ethanol and stirring to obtain a lithium hydroxide ethanol solution, adding the lithium hydroxide ethanol solution to the zinc acetate ethanol solution obtained in step (1), stirring and reacting at 20° C. for 1 h to obtain a ZnO QDs solution;
[0038] (3) Add 2 mL of 3-aminopropyltriethoxysilane to 6 mL of deionized water, mix well, and then add the resulting solution dropwise to the ZnO QDs solution obtained in step (2). After stirring for 1 hour, centrifuge at 8000 r / min for 5 minutes, collect the precipitate, wash it three times with anhydrous ethanol, and dry it in a 50°C forced air drying oven for 5 hours to obtain ZnO QDs powder.
[0039] Example 2
[0040] In step (2), the temperature of the stirring reaction is 0°C, and the rest is the same as in Example 1.
[0041] Example 3
[0042] In step (2), the temperature of the stirring reaction is 40° C., and the rest is the same as in Example 1.
[0043] Example 4
[0044] In step (2), the temperature of the stirring reaction is 60° C., and the rest is the same as in Example 1, to obtain ZnO QDs powder, which is recorded as Y-ZnO QDs.
[0045] Example 5
[0046] In step (2), the temperature of the stirring reaction is 80° C., and the rest is the same as in Example 1.
[0047] Example 6
[0048] In step (2), the amount of lithium hydroxide used is 15 mmol, and the rest is the same as in Example 1, to obtain ZnO QDs powder, which is recorded as G-ZnO QDs.
[0049] Example 7
[0050] In step (2), the amount of lithium hydroxide used is 20 mmol, and the rest is the same as in Example 1.
[0051] Example 8
[0052] In step (2), the amount of lithium hydroxide used is 30 mmol, and the rest is the same as in Example 1, to obtain ZnO QDs powder, which is recorded as B-ZnO QDs.
[0053] Example 9
[0054] In step (2), the amount of lithium hydroxide used is 40 mmol, and the rest is the same as in Example 1.
[0055] 1. The fluorescence emission spectra of the ZnO QDs prepared in Examples 1-9 were measured using a fluorescence spectrometer (PL, FS5, Edinburgh, UK).
[0056] Figure 1 From the fluorescence emission spectra of ZnO QDs prepared in Examples 1-5, it can be seen that as the reaction temperature gradually decreases, the fluorescence emission peak position gradually blue-shifts from 578 nm to 530 nm, and the fluorescence color gradually changes from orange-yellow to green. When the reaction temperature drops from 20°C to 0°C, there is no obvious change in the fluorescence emission peak position.
[0057] Figure 2 From the fluorescence emission spectra of ZnO QDs prepared in Example 1 and Examples 6-9, it can be seen that as the amount of LiOH is gradually increased, the fluorescence emission peak shifts from 532 nm to 477 nm, and the fluorescence color gradually changes from green to blue, indicating that the fluorescence emission peak of ZnO QDs can be blue-shifted by changing the molar ratio of zinc acetate dihydrate to LiOH; when the molar ratio of zinc acetate dihydrate to LiOH is increased from 1:3 to 1:4, the position of the fluorescence emission peak no longer changes significantly.
[0058] 2. The morphology of the ZnO QDs (ie, Y-ZnO QDs, G-ZnO QDs and B-ZnO QDs) prepared in Examples 4, 6 and 8 was tested using a transmission electron microscope (TEM, JEM-2100UHR, JEOL Ltd.).
[0059] Figure 3 TEM images of ZnO QDs prepared in Example 4, Example 6, and Example 8, wherein: Figure 3 (a) is the TEM image of Y-ZnOQDs. Figure 3 (b) is the TEM image of G-ZnO QDs. Figure 3 (c) is the TEM image of B-ZnO QDs. It can be seen that B-ZnO QDs, G-ZnO QDs, and Y-ZnO QDs are all spherical with relatively uniform particle size distribution and have good dispersibility in water.
[0060] 3. The particle size of ZnO QDs prepared in Example 4, Example 6 and Example 8 was measured using a laser particle size analyzer (NANO-S90, Malvern Instruments Ltd., UK).
[0061] Figure 4 This is a size distribution diagram of ZnO QDs prepared in Example 4, Example 6, and Example 8, wherein: Figure 4 a is the size distribution diagram of B-ZnO QDs, Figure 4 b is the size distribution diagram of G-ZnO QDs. Figure 4 c is the size distribution diagram of Y-ZnO QDs. It can be seen that the particle sizes of ZnO QDs of different fluorescent colors are different. With the red shift of the fluorescence wavelength, the particle size gradually increases. The particle sizes of B-ZnO QDs, G-ZnO QDs, and Y-ZnO QDs are gradually increasing. The particle size of B-ZnO QDs is between 1 and 5 nm, and the average particle size is 2.5 nm; the particle size of G-ZnO QDs is between 2 and 6 nm, and the average particle size is 3.6 nm; the particle size of Y-ZnO QDs is between 2 and 8 nm, and the average particle size is 4.3 nm.
[0062] 4. The structures of the ZnO QDs prepared in Examples 4, 6 and 8 were analyzed using an X-ray diffractometer (XRD, Ultima IV, Rigaku Corporation, Japan).
[0063] Figure 5From the XRD diffraction patterns of the ZnO QDs prepared in Example 4, Example 6, and Example 8, it can be seen that diffraction peaks corresponding to the (100), (002), (101), (102), (110), (103), and (112) crystal planes appear, which is consistent with the crystal structure of hexagonal wurtzite ZnO. At the same time, the appearance of the aminopropylsiloxane diffraction peak
[16] indicates that APTES has successfully modified the ZnO QDs. In addition, no other diffraction peaks appear, indicating that the ZnO QDs are pure and free of impurities. For ZnO QDs with different fluorescent colors, the diffraction peak widths are different. The diffraction peak of Y-ZnO QDs is the narrowest, followed by G-ZnO QDs, and the widest of B-ZnO QDs. The width of the diffraction peak represents the size of its particle size. According to the Scherrer formula
[17] , the wider the diffraction peak, the smaller the particle size. Y-ZnO QDs has the largest particle size, followed by G-ZnO QDs, and B-ZnO QDs has the smallest particle size.
[0064] 5. The surface functional group information of the ZnO QDs prepared in Example 4, Example 6 and Example 8 was determined using a Fourier transform infrared spectrometer (FT-IR, VERTEX-80, Bruker, Germany).
[0065] Figure 6 FTIR spectra of ZnO QDs prepared in Example 4, Example 6, and Example 8. In the figure, 3413 cm -1 The peak at 2932 cm comes from the stretching vibration of OH. -1 and 1409cm -1 The absorption peak is the stretching vibration of the CH bond, 460cm -1 The absorption peak is the stretching vibration of Zn-O, at 1584 cm -1 and 1012cm -1 The stretching vibrations of NH and Si-O appeared at the positions, respectively, indicating that APTES has been successfully coated on the surface of ZnO QDs of various fluorescent colors, allowing ZnO QDs to be stably dispersed in aqueous solution.
[0066] 6. The surface elements of the ZnO QDs prepared in Example 4, Example 6 and Example 8 were analyzed using an X-ray photoelectron spectrometer (XPS, AXIS UltraDLD, Shimadzu Corporation, UK).
[0067] Figure 7 This is the full XPS spectrum of ZnO QDs prepared in Example 4, Example 6, and Example 8, wherein: Figure 7 a is the full XPS spectrum, Figure 7b is the high-resolution spectrum of Zn 2p. It can be seen that the surfaces of ZnO QDs with different fluorescent colors all have Si 1s, C1s, O 1s, and Zn 2p peaks, among which Zn 2p and O 1s come from ZnO QDs, and C 1s and Si 1s come from APTES
[18] . This confirms that APTES is successfully coated on the surface of ZnO QDs. The peak of Zn 2p is further processed to obtain the following: Figure 7 The high-resolution spectrum shown in b shows that the peaks at 1044.5 eV and 1021.5 eV correspond to Zn 2p 1 / 2 With Zn2p 3 / 2 The energy difference between the two peaks is 23 eV, which is consistent with the standard value of 22.97 eV, indicating that Zn 2+ Exists in the form of oxides.
[0068] 7. The optical absorption properties of the ZnO QDs prepared in Example 4, Example 6 and Example 8 were tested using an ultraviolet visible spectrophotometer (UV-Vis, TU-1900, Beijing Puxi General Instrument Co., Ltd.).
[0069] Figure 8 The UV-visible absorption spectra and absorption band gap diagrams of ZnO QDs prepared in Example 4, Example 6, and Example 8, wherein: Figure 8 (a) is the UV-visible absorption spectrum, Figure 8 (b) is the absorption band gap diagram, Figure 8 (a) It can be seen that B-ZnO QDs, G-ZnO QDs, and Y-ZnO QDs have exciton absorption peaks at 300nm, 329nm, and 345nm, respectively. The reason for this phenomenon is that ZnO QDs have large exciton binding energy at room temperature; the gradual red shift of the absorption peaks of B-ZnO QDs, G-ZnO QDs, and Y-ZnO QDs also further indicates that the particle size of ZnO QDs gradually increases; in general, compared with the absorption peak of bulk ZnO at 380nm, the absorption peaks of ZnO QDs have all undergone a significant blue shift, indicating that the size of the prepared ZnO QDs is at the nanometer level and has the size effect of quantum dots. By converting the UV-visible absorption spectrum of ZnO QDs, the absorption band gap diagram of ZnO QDs can be obtained. The relationship between the absorption coefficient of ZnO QDs and the band gap energy is shown in the following formula:
[0070] (ahv) 2 =A(hv-Eg)
[0071] Where A is a constant, a, hv, and Eg are the absorption coefficient, photon energy, and optical band gap, respectively. Draw a graph with (ahv)2 as the ordinate and hv as the abscissa, and draw a tangent to the straight line of the curve. The abscissa where (ahv)2=0 is the absorption band gap. Figure 8 (b) is the absorption band gap diagram. It can be seen that the absorption band gaps of B-ZnO QDs, G-ZnO QDs, and Y-ZnO QDs are 3.69 eV, 3.50 eV, and 3.40 eV, respectively, which are larger than the absorption band gap of 3.37 eV of bulk ZnO, indicating that ZnO QDs have a quantum confinement effect.
[0072] 8. The ZnO QDs prepared in Example 4, Example 6, and Example 8 were photographed under sunlight and ultraviolet light respectively.
[0073] Fig. 9 These are the actual pictures of ZnO QDs prepared in Example 4, Example 6, and Example 8 under sunlight and ultraviolet light. It can be seen that B-ZnO QDs, G-ZnO QDs, and Y-ZnO QDs are all white powders under sunlight, and emit bright blue, green, and yellow fluorescence respectively under ultraviolet light.
[0074] 9. The ZnO QDs prepared in Example 4, Example 6, and Example 8 were dispersed in water respectively, the fluorescence emission spectra were tested, and the chromaticity coordinates were calculated based on the spectral data.
[0075] Fig.10 The fluorescence emission spectra and color gamut diagrams of ZnO QDs prepared in Example 4, Example 6, and Example 8 are shown, wherein: Fig.10 a is the fluorescence emission spectrum, Fig.10 b is the color gamut diagram, Fig.10 It can be seen from a that under 310nm ultraviolet light, the fluorescence emission peaks of B-ZnO QDs, G-ZnO QDs, and Y-ZnO QDs aqueous solutions are located at 480nm, 518nm, and 568nm, respectively. The chromaticity coordinates of ZnO QDs are further calculated based on the spectral data, and the fluorescence color is expressed by the position in the color gamut diagram, as shown in Fig.10 As shown in b, the chromaticity coordinates of B-ZnO QDs, G-ZnO QDs, and Y-ZnO QDs are (0.23, 0.31), (0.30, 0.40), and (0.42, 0.47), respectively, which more intuitively reflects the fluorescent color.
[0076] Application testing:
[0077] 1. The ZnO QDs prepared in Example 4, Example 6, and Example 8 were dissolved in water respectively to obtain B-ZnO QDs aqueous solution, G-ZnO QDs aqueous solution, and Y-ZnO QDs aqueous solution, and then the three ZnO QDs aqueous solutions were used as fluorescent inks to print combined patterns.
[0078] Fig.11 This is a combination pattern printed with ZnO QDs prepared in Example 4, Example 6, and Example 8. In the figure, blue clouds, green leaves, and yellow flowers are printed by B-ZnO QDs, G-ZnO QDs, and Y-ZnO QDs, respectively. The pattern is invisible under sunlight, but the combination pattern emits bright blue, green, and yellow fluorescence under ultraviolet light. After spraying a 1 mmol / L concentration of CuCl2 aqueous solution on the pattern area, the fluorescence of the combination pattern is quenched, and the original fluorescent pattern cannot be observed under ultraviolet light. The reason why CuCl2 solution causes fluorescence quenching of ZnO QDs aqueous solution is that Cu 2+ Will cause ZnO QDs to agglomerate, and Cu 2+ The presence of Cu can cause energy transfer in ZnO QDs, resulting in fluorescence quenching. This feature makes the pattern printed by ZnO QDs aqueous solution not limited to single anti-counterfeiting under ultraviolet light, but also can be printed by spraying Cu 2+ The solution distinguishes the authenticity, achieves a double anti-counterfeiting effect, and improves the security of anti-counterfeiting.
[0079] The ZnO QDs prepared in the embodiment of the present invention can also be formulated into fluorescent ink for printing a two-dimensional code pattern. The printed two-dimensional code pattern is invisible under sunlight, and the fluorescent two-dimensional code is clearly visible under ultraviolet light. Therefore, fluorescent anti-counterfeiting can be combined with two-dimensional code anti-counterfeiting and applied to the packaging of medicines, cosmetics, tobacco and alcohol, so as to achieve one code for one object and enhance the anti-counterfeiting performance. This shows that the ZnO QDs prepared by the present invention have excellent fluorescence performance and good practical application value.
Claims
1. A method for preparing water-dispersible zinc oxide quantum dots with adjustable fluorescent color, characterized in that: The steps include: (1) adding zinc acetate dihydrate to anhydrous ethanol and stirring until completely dissolved to obtain a zinc acetate ethanol solution; (2) adding lithium hydroxide to anhydrous ethanol and stirring evenly to obtain a lithium hydroxide ethanol solution, adding the lithium hydroxide ethanol solution to the zinc acetate ethanol solution obtained in step (1), stirring to react, and obtaining a ZnO QDs solution; (3) adding 3-aminopropyltriethoxysilane to deionized water, mixing well, and then dropping the obtained solution into the ZnO QDs solution obtained in step (2), stirring for reaction, collecting the precipitate by centrifugation, and then washing and drying to obtain; In step (2), the stirring reaction temperature is 0-80°C.
2. The method for preparing water-dispersible zinc oxide quantum dots with adjustable fluorescent color according to claim 1, characterized in that: In step (2), the molar ratio of zinc acetate dihydrate to lithium hydroxide is 1:(1-4).
3. The method for preparing water-dispersible zinc oxide quantum dots with adjustable fluorescent color according to claim 1, characterized in that: In step (3), the centrifugal conditions are: 8000r / min, 5min.
4. The method for preparing water-dispersible zinc oxide quantum dots with adjustable fluorescent color according to claim 1, characterized in that: In step (3), the washing method uses anhydrous ethanol and the number of washing times is 3-5 times.
5. The method for preparing water-dispersible zinc oxide quantum dots with adjustable fluorescent color according to any one of claims 1 to 4, characterized in that: In step (3), the drying temperature is 50-60° C. and the drying time is 4-6 hours.
6. Water-dispersible zinc oxide quantum dots with adjustable fluorescence color prepared by the method according to any one of claims 1 to 5.
7. Use of water-dispersible zinc oxide quantum dots with adjustable fluorescent color prepared by the method according to any one of claims 1 to 5 in preparing fluorescent ink.
8. Application of water-dispersible zinc oxide quantum dots with adjustable fluorescence color prepared by the method according to any one of claims 1 to 5 in light-emitting diodes and cell imaging.
Citation Information
Patent Citations
Synthesis method of silanized zinc oxide quantum dots with uniform size
CN111994943A
Cited By
Zinc oxide quantum dot fluorescence sensor and application thereof in detection of kaempferol
CN119666801A
Application of zinc oxide quantum dot fluorescent sensor and detection of kaempferol
CN119666801B