Nano composite material based on AIE molecule-rare earth inorganic nanocrystals and application of nano composite material
Through the nanocomposite material of AIE molecules and rare earth inorganic nanocrystals, the fluorescence quenching effect is used to achieve efficient detection of Fe3+ ions, which solves the cumbersome and complex detection problems in the existing technology and achieves highly sensitive and selective detection effects.
Patent Information
- Application Number
- CN202310375161.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-15
AI Technical Summary
The existing Fe3+ ion detection technology involves cumbersome sample preparation processes, complex instruments and operations, making it difficult to achieve efficient and simple detection.
A nanocomposite material based on AIE molecules and rare earth inorganic nanocrystals is used to form NaEuF4@TCPP through coordination, and its fluorescence quenching effect is used to achieve specific recognition and detection of Fe3+ ions.
It achieves highly sensitive and selective detection of Fe3+ ions with simple operation and fast detection speed. It is suitable for ion monitoring in living organisms and is not interfered by other metal ions.
Smart Images

Figure CN118772883A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal ion detection, and in particular relates to a nanocomposite material based on AIE molecules-rare earth inorganic nanocrystals and a use thereof. Background Art
[0002] Iron ion (Fe 3+ ) is one of the important biological trace elements in the human body and plays a vital role in many important chemical and biological processes such as oxygen uptake and transport, oxidative metabolism, enzyme catalysis and electron transfer. 3+ Both deficiency and excess of Fe ions can lead to various biological disorders and diseases, such as anemia, hepatitis, kidney and liver damage, neurodegeneration, Alzheimer's disease and Parkinson's disease. 3+ An ion detection strategy is essential.
[0003] Although some sensing techniques, such as atomic spectroscopy, electrochemical analysis, and inductively coupled plasma mass spectrometry (ICP-MS), have been developed to achieve this goal, they have certain limitations, including tedious sample preparation processes, complex instruments, time-consuming and complicated operations. In contrast, photoluminescence-based sensing methods have the advantages of high sensitivity and selectivity, easy operation, simple sample pretreatment process, and visual detection, which are widely used for the detection of Fe 3+ Ions offer a more promising strategy. Summary of the invention
[0004] In order to achieve the above object, the present invention provides the following technical solutions:
[0005] A nanocomposite material comprises aggregation-induced emission (AIE) molecules and rare earth inorganic nanocrystals, wherein the AIE molecules are anchored on the surface of the rare earth inorganic nanocrystals.
[0006] According to an embodiment of the present invention, the aggregation-induced emission molecules and the rare earth inorganic nanocrystals form the nanocomposite material through coordination.
[0007] According to an embodiment of the present invention, the aggregation-induced emission molecule is 2,3,5,6-tetrakis(4-carboxyphenyl)pyrazine (TCPP).
[0008] According to an embodiment of the present invention, the rare earth inorganic nanocrystal is NaReF4, and Re is selected from at least one of Eu, Tb, and Y, preferably Eu. Exemplarily, the rare earth inorganic nanocrystal is NaEuF4.
[0009] According to an embodiment of the present invention, the molar ratio of the rare earth inorganic nanocrystals to the aggregation-induced emission molecules is 100:(1-15), preferably 100:(6-10).
[0010] According to an exemplary embodiment of the present invention, the nanocomposite material includes 2,3,5,6-tetrakis(4-carboxyphenyl)pyrazine (TCPP) and NaEuF4, which is denoted as NaEuF4@TCPP.
[0011] According to an embodiment of the present invention, the maximum excitation wavelength of the NaEuF4@TCPP is 365 nm, and the maximum emission wavelength is 615 nm.
[0012] According to an embodiment of the present invention, the NaEuF4@TCPP is a spherical nanoparticle with a size of 8-10 nm.
[0013] According to an embodiment of the present invention, the nanoparticles of NaEuF4@TCPP have substantially Figure 5 X-ray diffraction pattern shown.
[0014] According to an embodiment of the present invention, the nanoparticles of NaEuF4@TCPP have substantially Figure 2 SEM images shown.
[0015] According to an embodiment of the present invention, Fe 3+ The ions have a fluorescence quenching effect on the NaEuF4@TCPP.
[0016] The present invention also provides a method for preparing the above-mentioned nanocomposite material, the preparation method comprising:
[0017] (1) The solvent reacts with rare earth salt, sodium salt and fluoride to form rare earth inorganic nanocrystals;
[0018] (2) modifying the surface of the rare earth inorganic nanocrystals in step (1) with aggregation-induced emission molecules through a ligand exchange reaction to obtain a nanocomposite material.
[0019] According to an embodiment of the present invention, in step (1), the reaction is carried out under the protection of an inert gas.
[0020] According to an embodiment of the present invention, in step (1), the solvent comprises oleic acid (OA) and / or octadecene (ODE).
[0021] According to an embodiment of the present invention, in step (1), the rare earth salt is selected from rare earth acetate and rare earth trifluoroacetate.
[0022] According to an embodiment of the present invention, in step (1), the rare earth element in the rare earth salt is selected from at least one of Eu, Tb, and Y. Preferably, the rare earth element is Eu.
[0023] According to an embodiment of the present invention, in step (1), the sodium salt is selected from sodium acetate.
[0024] According to an embodiment of the present invention, in step (1), the fluoride is selected from NaHF2.
[0025] According to an exemplary embodiment of the present invention, in step (1), the rare earth salt is selected from the acetate of Eu, the sodium salt is selected from sodium acetate, and the fluoride is selected from NaHF2.
[0026] According to an exemplary embodiment of the present invention, in step (1), the rare earth inorganic nanocrystal is NaEuF4.
[0027] According to an embodiment of the present invention, in step (2), the molar ratio of the rare earth inorganic nanocrystals to the aggregation-induced emission molecules added is 100:(1-15), preferably 100:(6-10).
[0028] According to the embodiment of the present invention, in step (2), adding concentrated hydrochloric acid before the ligand exchange reaction can effectively remove the surface oleic acid ligands without destroying the rare earth inorganic nanocrystals themselves, which is conducive to the faster and more effective modification of AIE molecules on the surface of NaEuF4 rare earth inorganic nanocrystals. Preferably, those skilled in the art can reasonably adjust the amount of concentrated hydrochloric acid added according to the amount of rare earth inorganic nanocrystals used, for example, 100-400 μL.
[0029] According to an embodiment of the present invention, before the ligand exchange reaction, the rare earth inorganic nanocrystals are added to a solution of concentrated hydrochloric acid and anhydrous ethanol for ultrasonic treatment.
[0030] According to an embodiment of the present invention, in step (2), after obtaining the nanocomposite material, washing may be performed. Preferably, washing may be performed by methods known in the art, such as washing with cyclohexane and / or anhydrous ethanol.
[0031] According to an embodiment of the present invention, step (1) comprises the following steps:
[0032] (A1) adding the acetate and sodium salt of Eu into a solvent, stirring and heating to dissolve, to obtain a first solution;
[0033] (A2) After the first solution of step (A1) is cooled to room temperature, fluoride is added, and the reaction is carried out at a constant temperature under the protection of an inert gas, followed by cooling to room temperature, precipitation, and washing to obtain rare earth inorganic nanocrystals.
[0034] According to an embodiment of the present invention, in the step (A1), the heating and dissolving is carried out under inert gas protection conditions.
[0035] According to an embodiment of the present invention, in the step (A1), the temperature for heating and dissolving is 120-180°C.
[0036] According to an embodiment of the present invention, in the step (A2), the isothermal reaction specifically includes: stirring and heating to 250°C to carry out a first isothermal reaction, for example, reacting for 0.5 hours; after the first isothermal reaction is completed, stirring and rapidly heating to 300°C under the protection of an inert gas to carry out a second isothermal reaction, for example, reacting for 1 hour.
[0037] According to an embodiment of the present invention, in the step (A2), the precipitation is specifically: using anhydrous ethanol for precipitation, and then collecting the precipitate by centrifugation; then using cyclohexane as a dispersant for redispersion, and anhydrous ethanol as a precipitant for precipitation, and the two solvents are used alternately for washing.
[0038] According to an embodiment of the present invention, in step (A2), cyclohexane and / or anhydrous ethanol are used for washing.
[0039] According to an exemplary embodiment of the present invention, the preparation method of the nanocomposite material NaEuF4@TCPP comprises the following steps:
[0040] (S1) Weigh Eu(CH3COO)3·4H2O and CH3COONa, add them to a mixed solvent of oleic acid and octadecene, heat to 150°C under N2 protection, stir and dissolve, keep warm for 0.5 hour until Eu(CH3COO)3·4H2O and CH3COONa are fully dissolved, then cool to room temperature; add NaHF2, heat to 250°C under N2 protection, stir, keep warm for 0.5 hour to promote the decomposition of NaHF2; after the insulation is completed, quickly heat to 300°C, keep the temperature for 1 hour, precipitate and wash to obtain NaEuF4;
[0041] (S2) dispersing the NaEuF4 obtained in step (S1) in an anhydrous ethanol solution containing aggregation-induced emission molecules, stirring at room temperature for 6 hours, and washing by centrifugation with anhydrous ethanol to obtain NaEuF4@TCPP.
[0042] Preferably, in step (S1), precipitation refers to: cooling the solution after the reaction to room temperature, adding anhydrous ethanol and centrifuging to obtain a precipitate.
[0043] Preferably, in step (S1), washing means: washing the precipitate with cyclohexane and / or anhydrous ethanol. Further, washing can be performed by ultrasonic washing.
[0044] Preferably, in step (S2), before dispersion, NaEuF4 can also be washed with concentrated hydrochloric acid, for example, by ultrasonic washing in an anhydrous ethanol solution containing concentrated hydrochloric acid.
[0045] The present invention also provides a nanocomposite material obtained by the above preparation method, wherein the nanocomposite material has the meaning as described above.
[0046] The present invention also provides the use of the above nanocomposite material in ion detection, preferably for Fe 3+ Ion detection. Preferably, the nanocomposite material is used for Fe 3+ Detection of ions.
[0047] The present invention also provides a fluorescent probe, which comprises the nanocomposite material.
[0048] According to an exemplary embodiment of the present invention, the fluorescent probe is an aqueous solution of NaEuF4@TCPP, wherein the concentration of NaEuF4@TCPP is 30 mg / 10 mL.
[0049] The present invention also provides the use of the fluorescent probe in ion detection, preferably for Fe 3+ Ion detection. Preferably, the nanocomposite material is used for Fe 3+ Detection of ions.
[0050] The present invention also provides a Fe 3+ The ion detection method comprises: bringing the sample to be tested into contact with the above-mentioned nanocomposite material and / or fluorescent probe, and measuring the fluorescence value.
[0051] According to an embodiment of the present invention, the fluorescent probe is an aqueous solution of NaEuF4@TCPP, wherein the concentration of 30mgNaEuF4@TCPP is 30mg / 10mL. Preferably, the fluorescence relative value y of the fluorescent probe is 3+ The relationship curve of concentration x is, y = 1-0.012x, r 2 =0.998, x is 0-60μM; Fe 3+ The lowest detection limit of the ion was 340 nM.
[0052] According to an embodiment of the present invention, the sample to be tested is derived from a 3+ Preferably, the sample to be tested is derived from a sample containing Fe 3+ Preferably, the sample to be tested can be treated by a method known in the art before testing.
[0053] According to an embodiment of the present invention, the detection method specifically comprises: ultrasonically dispersing the nanocomposite material and / or fluorescent probe in a solution, and then dripping the sample to be tested in situ to perform fluorescence detection.
[0054] Beneficial Effects
[0055] Rare earth nanocrystals (NCs) are candidate materials for luminescent probes due to their narrowband emission, large Stokes shift, long luminescence lifetime, excellent light and chemical stability, and low biological toxicity; AIE molecules are promising for applications in chemical sensing, bioimaging, medical diagnosis, etc. Therefore, the present invention combines rare earth nanocrystals and AIE molecules to construct a nanocomposite material with advanced optical properties and stimulus-responsive behavior, wherein the AIE molecules are anchored on the rare earth nanocrystals, wherein the AIE molecules can be used as antenna molecules to activate the luminescence of the rare earth nanocrystals. The nanocomposite material of the present invention is very suitable for becoming a luminescent platform for ion detection, which is a promising material for the development of convenient, economical, and accurate Fe 3+ The detection method of ions provides a new idea.
[0056] (1) The present invention uses red fluorescent NaEuF4@TCPP to construct a colorful fluorescent probe, which improves the sensitivity of observing fluorescent color changes with the naked eye. The fluorescent probe provides a basis for the further development of portable fluorescent visualization sensing equipment.
[0057] (2) The NaEuF4@TCPP prepared by the present invention has excellent luminescence performance, which can 3+ ions to achieve specific recognition. 3+ ions, will not be affected by Zn 2+ ,Mg 2+ , Ca 2+ ,Cr 3+ , Al 3+ , Pb 2+ , Na + , K + , Cd 2+ and Fe 2+ ions, the material has no effect on Fe 3+ The detection of ions showed excellent selectivity.
[0058] (3) The present invention also provides a nanocomposite material for detecting Fe 3+ The detection method of the present invention is simple to operate and has good detection performance. 3+ It has strong ion selectivity, high detection sensitivity and fast detection speed. 3+ Compared with the technology of ions, the NaEuF4@TCPP of the present invention can be used to treat Fe 3+ Ion quenching detection is a method with high sensitivity and small sampling volume. It can be easily applied to direct detection, labeling and identification of biological systems. Therefore, it has important significance and prospects for ion monitoring in organisms. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] Figure 1The nanocomposite material and / or fluorescent probe of the present invention detects Fe 3+ Schematic diagram of the principle of ions.
[0060] Figure 2 This is a transmission electron microscopy image of NaEuF4@TCPP nanoparticles prepared in Example 1 of the present invention.
[0061] Figure 3 This is a particle size analysis diagram of NaEuF4@TCPP nanoparticles prepared in Example 1 of the present invention.
[0062] Figure 4 This is the X-ray diffraction pattern of the NaEuF4@TCPP nanoparticles prepared in Example 1 of the present invention.
[0063] Figure 5 This is the fluorescence spectrum of NaEuF4@TCPP nanoparticles prepared in Example 1 of the present invention.
[0064] Figure 6 Fe is the luminescence intensity of the NaEuF4@TCPP probe prepared in Example 1 3+ Plot of the ion concentration-dependent response curve.
[0065] Figure 7 The NaEuF4@TCPP nanoprobe prepared in Example 1 of the present invention measures Fe at different concentrations 3+ Spectrum of ions.
[0066] Figure 8 This is the experimental result of the selectivity of the NaEuF4@TCPP nanoprobe prepared in Example 1 of the present invention for other metal ion interferents. DETAILED DESCRIPTION
[0067] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention, and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0068] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0069] Instruments and equipment:
[0070] The powder diffraction characterization of the product of the embodiment of the present invention is performed using an instrument model of Rigaku Dmax-2500 manufactured by Rigaku, and the radiation wavelength of the copper target is λ=0.154187 nm.
[0071] The instrument model used for X-ray energy spectrum analysis of the product in the embodiment of the present invention is Zetasizer Nano ZSZEN3600, manufactured by Malvern.
[0072] The scanning electron microscope used for the product of the embodiment of the present invention is JSM-6700F, manufactured by Japan Electronics Corporation.
[0073] The instrument model used for the fluorescence emission spectrum characterization of the product in the embodiment of the present invention is FLS980, the manufacturer is Edinburgh, and the excitation light source is a xenon lamp.
[0074] The reagents used in the following embodiments of the present invention can be prepared as follows:
[0075] (a) Preparation of NaEuF4@TCPP probe (3 mg / mL): 30 mg of NaEuF4@TCPP nanoparticles were added to 10 mL of deionized water and sonicated for 20 min.
[0076] (b) 40 mM Fe 3+ Preparation of ion solution: Weigh 64.8 mg FeCl3, add it to 10 mL deionized water, and sonicate to fully dissolve it. + , Na + ,Mg 2+ , Ca 2+ , Al 3+ ,Cr 3+ , Cd 2+ , Zn 2+ , Pb 2+ , Fe 2+ The solution is prepared by taking the corresponding mass of chloride in the same way.
[0077] (c) 4 mM Fe 3+ Ionic solution preparation: Take the prepared 40mM Fe 3+ 1mL of ion solution was diluted 10 times.
[0078] Example 1
[0079] The preparation method of NaEuF4@TCPP nanocomposite material is as follows:
[0080] (1) Preparation of NaEuF4 rare earth nanocrystals: Weigh Eu(CH3COO)3·4H2O (1mmol) and CH3COONa (1.5mmol), put them into a two-necked flask, add oleic acid (8mL) and octadecene (12mL) and stir to mix. Then stir and heat to 160℃ in a nitrogen atmosphere and keep the temperature constant for 30min. Until Eu(CH3COO)3·4H2O and CH3COONa in the mixed solution are fully dissolved and become clear and transparent, cool to room temperature. Then weigh NaHF2 (2mmol), add it to the mixed solution, heat the mixed solution to 250℃ under nitrogen protection, keep the temperature for 30min, and allow NaHF2 to fully decompose. Then quickly heat to 300℃ and keep it at this temperature for 1h to allow the reactants in the two-necked flask to fully react to form rare earth nanocrystals. After the reaction was completed, the mixture was naturally cooled to room temperature, 15 mL of ethanol was added to a two-necked flask for precipitation, and the reaction product was collected by centrifugation. The mixture was washed several times with 2 mL of cyclohexane and 3 mL of ethanol. The final product was NaEuF4 rare earth nanocrystals.
[0081] (2) Preparation of nanocomposite materials: 30 mg of oil-soluble NaEuF4 was ultrasonically cleaned and evenly dispersed in 15 mL of ethanol; 200 μL of concentrated hydrochloric acid was added, and the surface of the exposed NaEuF4 was obtained by centrifugation after ultrasonic cleaning for 1 h; the surface of the exposed NaEuF4 was added to an ethanol solution containing TCPP (4 mg) and stirred for 6 h. After centrifugation, the solution was washed with ethanol for several times and finally dispersed in 10 mL of deionized water for later use, thereby obtaining TCPP-modified rare earth nanocrystals, which were recorded as the nanocomposite material NaEuF4@TCPP.
[0082] Scanning electron microscopy and particle size distribution ( Figure 2 and Figure 3 ) shows that the NaEuF4@TCPP nanoparticles have good dispersibility and uniform morphology, and the particle size is about 9.8nm; the X-ray powder diffraction pattern ( Figure 5 ) showed that the NaEuF4@TCPP nanoparticles had good crystallinity, and the position and relative intensity of the diffraction peaks were consistent with the NaEuF4 standard card (JCPDS: 049-1897); the aqueous solution of the nanoparticles appeared purple-red under 365nm ultraviolet light; the fluorescence emission spectrum under 365nm excitation ( Figure 6 ) showed that the nanoparticles had luminescence at 425nm and 615nm, with strong luminescence at 615nm.
[0083] Example 2
[0084] As a fluorescent probe, NaEuF4@TCPP has a luminescent intensity similar to Fe 3+ Determination of concentration relationship curve:
[0085] 30 mg of NaEuF4@TCPP prepared in Example 1 was dispersed in 10 mL of deionized water; 2 mL of NaEuF4@TCPP solution was transferred into a clean four-way quartz cuvette using a 5 mL pipette, and the fluorescence spectrum was measured after adjusting the relevant parameters of the FLS 980 fluorescence spectrometer; after the test, 5 μL of Fe 3+ The ion aqueous solution (4 mM) was added to a four-way quartz cuvette, mixed with a centrifuge tube for 1 min, and then the fluorescence spectrum test was performed. After the test, 5 μL of Fe 3+ Add the ion solution into a four-way quartz cuvette, stir for 1 min, and then perform spectrum test. Repeat the addition of Fe 3+ Ion aqueous solution until Fe 3+ ions is 80μM. During the whole test process, in addition to the continuous addition of Fe 3+ The other conditions of the ion aqueous solution were not changed. The obtained spectrum is the NaEuF4@TCPP solution (i.e., fluorescent probe) with an excitation wavelength of 365nm when different Fe 3+ Fluorescence spectrum after ion concentration ( Figure 7 ).
[0086] Test conditions: The excitation wavelength and emission wavelength are 365nm and 615nm respectively. The relative fluorescence intensity (Fe 3+ The luminescence intensity ratio of NaEuF4@TCPP at 615nm before and after the addition of Fe ions is taken as the ordinate, and the luminescence intensity ratio of NaEuF4@TCPP at 615nm is taken as the ordinate. 3+ The concentration of the ion solution is plotted as the horizontal axis to obtain the relative luminescence intensity y of the NaEuF4@TCPP probe and Fe 3+ The relationship curve of concentration x Figure 6 ), y = 1-0.012x, r 2 =0.998, x=0-60μM, where the lowest detection limit LOD is 340nM.
[0087] Depend on Figure 6 and Figure 7 It can be seen that Fe 3+ The ion solution has a quenching effect on the luminescence of the NaEuF4@TCPP probe. 3+ The higher the concentration of the ion solution, the more obvious the quenching effect is. 3+ The concentration of the ions is linearly related.
[0088] Example 3
[0089] The response of NaEuF4@TCPP to different metal ions is as follows:
[0090] (1) The NaEuF4@TCPP probe solution required in this example is consistent with that in Example 2.
[0091] (2) Prepare Fe according to the above method 3+ Ion solution, and other common metal ions were selected as interfering ions to prepare interfering ion solutions, and the response of the system to different metal ions was further studied. Other common metal ions were K + , Na + ,Mg 2+ , Ca 2+ , Al 3+ ,Cr 3+ , Cd 2+ , Zn 2+ , Pb 2+ , Fe 2+ .
[0092] (3) Prepare various metal ion solutions with a concentration of 40 mM using deionized water, add 2 mL of NaEuF4@TCPP probe (3 mg / mL) to a four-way quartz cuvette, and measure its luminescence spectrum on an FLS 980 fluorescence spectrometer. Then, use a 20 μL pipette to transfer 5 μL of different metal ion aqueous solutions to the four-way quartz cuvette, use a centrifuge tube to mix for 1 min, and then perform fluorescence spectrum testing. Then, add 5 μL of Fe 3+ Ionic solution (i.e., the solution in the cuvette contains both interfering ions and Fe 3+ ions), and then mixed them in a centrifuge tube for 1 min, and then the fluorescence spectrum test was performed to obtain Fe 3+ The relative intensity of luminescence quenching of ions.
[0093] During the test, except for replacing the clean four-way quartz cuvette, the FLS 980 fluorescence spectrometer was not modified until all comparative experiments were completed. Test conditions: excitation wavelength and emission wavelength were 365nm and 615nm respectively. The fluorescence intensity and luminescence quenching relative intensity values corresponding to different interfering ions are shown in Figure 8 .
[0094] Depend on Figure 8 The bar chart shows that only Fe 3+ The Fe ions have a quenching effect on the luminescence of the NaEuF4@TCPP nanoprobe, while the other metal ions have little effect on the luminescence quenching effect of the probe. 3+ The ion quenching of NaEuF4@TCPP nanoprobe is still obvious. 3+ The ions have good selective response.
[0095] The above is a description of the exemplary embodiments of the present invention. However, the protection scope of the present application is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A nanocomposite material, characterized in that: The nanocomposite material comprises aggregation-induced luminescence molecules and rare earth inorganic nanocrystals, wherein the aggregation-induced luminescence molecules are anchored on the surface of the rare earth inorganic nanocrystals; The aggregation-induced emission molecules and the rare earth inorganic nanocrystals form the nanocomposite material through coordination.
2. The nanocomposite material according to claim 1, characterized in that The aggregation-induced emission molecule is 2,3,5,6-tetrakis(4-carboxylphenyl)pyrazine. Preferably, the rare earth inorganic nanocrystal is NaReF4, and Re is selected from at least one of Eu, Tb and Y. Preferably, the molar ratio of the rare earth inorganic nanocrystals to the aggregation-induced emission molecules is 100:(1-15).
3. The nanocomposite material according to claim 1 or 2, characterized in that: The nanocomposite material includes 2,3,5,6-tetrakis(4-carboxyphenyl)pyrazine and NaEuF4, and is recorded as NaEuF4@TCPP.
4. The nanocomposite material according to any one of claims 1 to 3, characterized in that: The maximum excitation wavelength of the NaEuF4@TCPP is 365 nm, and the maximum emission wavelength is 615 nm. Preferably, the NaEuF4@TCPP is a spherical nanoparticle with a size of 8-10 nm. Preferably, Fe 3+ The ions have a fluorescence quenching effect on the NaEuF4@TCPP.
5. The method for preparing the nanocomposite material according to any one of claims 1 to 4, characterized in that: The preparation method comprises: (1) The solvent reacts with rare earth salt, sodium salt and fluoride to form rare earth inorganic nanocrystals; (2) modifying the surface of the rare earth inorganic nanocrystals in step (1) with aggregation-induced emission molecules through a ligand exchange reaction to obtain a nanocomposite material. Preferably, in step (1), the reaction is carried out under the protection of an inert gas. Preferably, in step (1), the solvent comprises oleic acid and / or octadecene. Preferably, in step (1), the rare earth salt is selected from rare earth acetate and rare earth trifluoroacetate. Preferably, in step (1), the rare earth element in the rare earth salt is selected from at least one of Eu, Tb and Y. Preferably, in step (1), the sodium salt is selected from sodium acetate. Preferably, in step (1), the fluoride is selected from NaHF2. Preferably, in step (2), the molar ratio of the rare earth inorganic nanocrystals to the aggregation-induced emission molecules is 100:(1-15).
6. The preparation method according to claim 5, characterized in that: Step (1) comprises the following steps: (A1) adding the acetate and sodium salt of Eu into a solvent, stirring and heating to dissolve, to obtain a first solution; (A2) After the first solution of step (A1) is cooled to room temperature, fluoride is added, and the reaction is carried out at a constant temperature under the protection of an inert gas, followed by cooling to room temperature, precipitation, and washing to obtain rare earth inorganic nanocrystals. Preferably, in the step (A1), the heating and dissolving is carried out under inert gas protection conditions. Preferably, in the step (A1), the temperature for heating and dissolving is 120-180°C. Preferably, in the step (A2), the isothermal reaction specifically comprises: stirring and heating to 250° C. to carry out a first isothermal reaction; after the first isothermal reaction is completed, stirring and rapidly heating to 300° C. under the protection of an inert gas to carry out a second isothermal reaction.
7. The preparation method according to claim 5 or 6, characterized in that: The preparation method of the nanocomposite material NaEuF4@TCPP comprises the following steps: (S1) Weigh Eu(CH3COO)3·4H2O and CH3COONa, add them to a mixed solvent of oleic acid and octadecene, heat to 150°C under N2 protection, stir and dissolve, keep warm for 0.5 hour until Eu(CH3COO)3·4H2O and CH3COONa are fully dissolved, then cool to room temperature; add NaHF2, heat to 250°C under N2 protection, stir, keep warm for 0.5 hour to promote the decomposition of NaHF2; after the insulation is completed, quickly heat to 300°C, keep the temperature for 1 hour, precipitate and wash to obtain NaEuF4; (S2) dispersing the NaEuF4 obtained in step (S1) in an anhydrous ethanol solution containing aggregation-induced emission molecules, stirring at room temperature for 6 hours, and washing by centrifugation with anhydrous ethanol to obtain NaEuF4@TCPP.
8. A fluorescent probe, characterized in that The fluorescent probe comprises the nanocomposite material according to any one of claims 1 to 4.
9. Use of the nanocomposite material according to any one of claims 1 to 4 and / or the fluorescent probe according to claim 8 in ion detection.
10. Fe 3+ An ion detection method, characterized in that The detection method comprises: contacting a sample to be tested with the nanocomposite material according to any one of claims 1 to 4 and / or the fluorescent probe according to claim 8, and measuring the fluorescence value.
Citation Information
Patent Citations
Internally and externally refined composite nano photosensitizer as well as preparation method and application thereof
CN109481680A