Method for controlling brittle and hard inclusions in 12Cr1MoVG steel and 12Cr1MoVG steel

By using low-alkalinity slag refining technology in the smelting process of 12Cr1MoVG steel to control the reactions of CaO, SiO2 and Al2O3, the problem of excessive brittle inclusions caused by high-alkalinity refining is solved, the proportion of plastic inclusions in the steel is improved, and the Steel quality and economic benefits.

CN118773392APending Publication Date: 2024-10-15LINGYUAN IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410900902.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

During the smelting process of 12Cr1MoVG steel, high alkalinity refining results in excessive content of Class B, Class D and Class Ds brittle inclusions, which affects the quality of the steel. The existing technology lacks effective control methods to increase the proportion of plastic inclusions in the steel.

Method used

Using low-basicity slag refining technology, refining is carried out in the RH process. By mixing the molten steel after the end of the converter with low-basicity reducing slagging materials, LF and RH refining are performed to form low-basicity slag and control CaO, SiO2 and Al2O3 reaction to form composite inclusions and increase the proportion of plastic inclusions in the steel.

Benefits of technology

It effectively controls the content of B, D, and Ds inclusions in 12Cr1MoVG steel, increases the proportion of plastic inclusions in the steel, significantly improves the quality of the steel, and achieves economic benefits for high alkalinity refining.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773392A_ABST
    Figure CN118773392A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of ferrous metallurgy, and discloses a method for controlling brittle and hard inclusions in 12Cr1MoVG steel and the 12Cr1MoVG steel. The method comprises the following steps: feeding a steelmaking raw material of 12Cr1MoVG steel into a converter, carrying out converter smelting until the converter end point is reached to obtain molten steel, tapping, enabling the molten steel to flow into a steel ladle, and carrying out deoxidation alloying to obtain outbound molten steel; mixing the outbound molten steel with a high-alkalinity slagging material, and carrying out LF high-alkalinity slag white slag refining to obtain LF refined molten steel; mixing the LF refined molten steel with a low-alkalinity reducing slagging material, and performing RH refining to obtain RH refined molten steel; and the RH refined molten steel is used for carrying out a continuous casting steelmaking process, and the 12Cr1MoVG steel is obtained. According to the method, low-alkalinity slag refining is carried out in the RH procedure, and the problem that B, D and Ds type inclusions in the 12Cr1MoVG steel exceed the standard, and the quality of the steel is affected is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron and steel metallurgy, and more specifically, relates to a method for controlling brittle and hard inclusions in 12Cr1MoVG steel and the 12Cr1MoVG steel. Background Art

[0002] 12Cr1MoVG steel is a kind of low alloy heat-resistant steel widely used in power station boilers and other fields. During the deoxidation and alloying process of 12Cr1MoVG steel, aluminum with strong deoxidation is used for deep deoxidation to reduce the dissolved oxygen content in the steel. However, in actual production operations, in order to ensure the low oxygen level, the amount of aluminum added is often seriously exceeded, and the whole process is high-basicity refining. A large amount of Class B inclusions (aluminum oxide) formed after aluminum deoxidation will have a serious impact on the mechanical properties of steel. When Class B inclusions react with CaO and SiO2 inclusions in steel, large-sized brittle calcium aluminate inclusions (D and Ds) will be formed, which are fatal to the quality of steel.

[0003] However, up to now, there are few reports on methods for controlling brittle and hard inclusions in 12Cr1MoVG steel. Therefore, it is urgent to propose a method for controlling brittle and hard inclusions in 12Cr1MoVG steel, increase the proportion of plastic inclusions in 12Cr1MoVG steel, solve the problem of excessive brittle inclusions of type B, type D and type Ds in 12Cr1MoVG steel in the existing full-process high-basicity refining, achieve a high proportion of plastic inclusions in 12Cr1MoVG steel, and significantly improve the quality of 12Cr1MoVG steel. Summary of the invention

[0004] The purpose of the present invention is to solve the problem that the B, D and Ds inclusions in 12Cr1MoVG steel exceed the standard and affect the quality of the steel by performing low-basicity slag refining in the RH process.

[0005] In order to achieve the above object, the present invention provides a method for controlling brittle and hard inclusions in 12Cr1MoVG steel, the method comprising the following steps:

[0006] S1: feeding the steelmaking raw material of 12Cr1MoVG steel into a converter, performing converter smelting, reaching the converter end point, obtaining molten steel and tapping, making the molten steel flow into a ladle and performing deoxidation and alloying to obtain outlet molten steel;

[0007] S2: mixing the outgoing molten steel with high basicity slag-making material and performing LF high basicity slag white slag refining to obtain LF refined molten steel;

[0008] S3: mixing the LF refined molten steel with a low-basicity reducing slag-making material and performing RH refining to obtain RH refined molten steel;

[0009] S4: Utilizing the RH refined molten steel to carry out continuous casting steelmaking process to obtain 12Cr1MoVG steel.

[0010] According to the present invention, preferably, at the end point of the converter, C in the molten steel is ≤ 0.06%.

[0011] According to the present invention, preferably, at the end point of the converter, the temperature of the molten steel is 1680°C-1730°C.

[0012] According to the present invention, preferably, the steel tapping adopts a double slag blocking method, using a slide plate to block the slag in the early stage of steel tapping, and using a slag blocking cone to block the slag in the later stage of steel tapping, and controlling the slag amount to ≤2kg / t molten steel.

[0013] According to the present invention, preferably, the deoxidizing agent for the deoxidation alloying is at least one of aluminum ingot, ferrosilicon, ferromanganese, ferrochrome and ferrovanadium.

[0014] According to the present invention, preferably, the temperature for performing the LF high basicity slag refining is 1545-1555° C. and the time is 35-45 min.

[0015] According to the present invention, preferably, the RH refining is performed at a temperature of 1570-1620° C. and a time of 20-30 min.

[0016] According to the present invention, preferably, the low-basicity reducing slag-making material is composed of the following raw materials in weight percentage: FeO+MnO≤1.0%, CaO is 30-45%, SiO2 is 20-30%, Al2O3 is 20-30%; MgO is 1-10%; 1.3≤R≤1.6, R=CaO% / SiO2%; the rest are MnO, P2O5, TiO2 and impurities.

[0017] According to the present invention, preferably, based on the total weight of all inclusions in the 12Cr1MoVG steel obtained in step S4, the proportion of plastic inclusions in the 12Cr1MoVG steel obtained in step S4 is greater than 70%.

[0018] Another aspect of the present invention provides 12Cr1MoVG steel obtained by the method for controlling brittle and hard inclusions in 12Cr1MoVG steel.

[0019] The beneficial effects of the technical solution of the present invention are as follows:

[0020] 1. The present invention performs low-basicity slag refining in the RH process, controls the contents of B, D and Ds inclusions in 12Cr1MoVG steel to a certain extent, and solves the problem that high-basicity refining is used to control the basicity of the refined slag in the smelting process of 12Cr1MoVG steel, resulting in excessive B, D and Ds inclusions in the steel, thereby affecting the quality of the steel.

[0021] 2. The implementation of the method of the present invention is an operation carried out between the LF and RH processes and will not cause difficulties for the continuity of on-site production.

[0022] 3. The present invention uses low-basicity refined slag for operation. [Ca], [Si], [Al] and [O] in the molten steel will react to form composite inclusions or CaO, SiO2 and Al2O3 will react. The reaction equation is as follows:

[0023] x[Ca]+2y[Al]+z[Si]+(x+3y+2z)[O]=xCaO·yAl2O3·zSiO2(1)

[0024] xCaO+yAl2O3+zSiO2=xCaO·yAl2O3·zSiO2(2)

[0025] like Figure 1 As shown, the composition area of ​​the plastic inclusions of the CaO-SiO2-Al2O3 ternary inclusions is in the peripheral low melting point area adjacent to calcium plagioclase (CaO·Al2O3·2SiO2) and pseudowollastonite (CaO·SiO2), with a melting point within 1400°C, wherein the CaO content is 8-53%, the SiO2 content is 32-70%, and the Al2O3 content is 5-37%.

[0026] 4. The present invention provides a new method for transforming B, D and Ds inclusions into plastic inclusions during the refining process of 12Cr1MoVG steel, which will bring greater economic benefits.

[0027] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention with reference to the accompanying drawings.

[0029] Figure 1 It is the phase diagram and melting point representation of the CaO-Al2O3-SiO2 system plastic inclusions of the present invention ("mass fraction", "projection", "fact sage" thermochemical calculation software).

[0030] Figure 2 2. The comparative phase diagram of CaO-Al2O3-SiO2 plastic inclusions obtained in Example 1 of the present invention and Comparative Example 1 ("0765 heat" is Example 1, and "0768 heat" is Comparative Example 1).

[0031] Figure 3 2 is a comparative phase diagram of CaO-Al2O3-SiO2 plastic inclusions obtained in Example 2 of the present invention and Comparative Example 1 ("0766 heat" is Example 2).

[0032] Figure 4 3 is a comparative phase diagram of CaO-Al2O3-SiO2 plastic inclusions obtained in Example 3 of the present invention and Comparative Example 1 ("0767 heat" is Example 3). DETAILED DESCRIPTION

[0033] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.

[0034] Example 1

[0035] This embodiment provides a method for controlling brittle and hard inclusions in 12Cr1MoVG steel, the method comprising the following steps:

[0036] S1: feeding the steelmaking raw material of 12Cr1MoVG steel into a converter, performing converter smelting, reaching the converter end point (C in the molten steel ≤ 0.06%, temperature 1640° C.), obtaining molten steel and tapping, making the molten steel flow into a ladle and performing deoxidation and alloying, and obtaining outlet molten steel;

[0037] in:

[0038] The steel tapping adopts a double slag blocking method, wherein a slide plate is used to block the slag in the early stage of steel tapping, and a slag blocking cone is used to block the slag in the late stage of steel tapping, and the slag amount is controlled to be ≤2kg / t molten steel;

[0039] The deoxidizing agent for the deoxidation alloying is an aluminum ingot;

[0040] S2: mixing the outgoing molten steel with high basicity slag-making material and performing LF high basicity slag white slag refining at a temperature of 1550° C. for 40 min to obtain LF refined molten steel;

[0041] S3: mixing the LF refined molten steel with a low-basicity reducing slag-making material (the composition is shown in Table 1) and performing RH refining at a temperature of 1570-1620° C. for 25 min to obtain RH refined molten steel;

[0042] S4: Utilizing the RH refined molten steel to carry out continuous casting steelmaking process to obtain 12Cr1MoVG steel.

[0043] Example 2-3

[0044] Example 2-3 provides a method for controlling brittle and hard inclusions in 12Cr1MoVG steel. The only difference between Example 2-3 and Example 1 is that the components of the low-basicity reducing slag-making material are different, as shown in Table 1.

[0045] Table 1 Composition of low basicity reducing slag making material

[0046]

[0047] Comparative Example 1

[0048] The difference between this comparative example and Example 1 is that step S3 is not performed, and the LF refined molten steel is subjected to a continuous casting steelmaking process to obtain 12Cr1MoVG steel.

[0049] The finished product composition of the 12Cr1MoVG steel of Examples 1-3 and Comparative Example 1 is shown in Table 2.

[0050] Table 2

[0051]

[0052] like Figure 2 As shown, it is the inclusion projection of 12Cr1MoVG steel of Example 1 and Comparative Example 1 in the CaO-Al2O3-SiO2 phase diagram. It can be seen that the proportion of plastic inclusions in the 12Cr1MoVG steel of Example 1 is 75%; the proportion of plastic inclusions in the 12Cr1MoVG steel of Comparative Example 1 is 11%.

[0053] like Figure 3 As shown, it is the inclusion projection of 12Cr1MoVG steel of Example 2 and Comparative Example 1 in the CaO-Al2O3-SiO2 phase diagram. It can be seen that the proportion of plastic inclusions in the 12Cr1MoVG steel of Example 2 is 80%; the proportion of plastic inclusions in the 12Cr1MoVG steel of Comparative Example 1 is 11%.

[0054] like Figure 4As shown, it is the inclusion projection of 12Cr1MoVG steel of Example 3 and Comparative Example 1 in the CaO-Al2O3-SiO2 phase diagram. It can be seen that the proportion of plastic inclusions in the 12Cr1MoVG steel of Example 3 is 86%; the proportion of plastic inclusions in the 12Cr1MoVG steel of Comparative Example 1 is 11%.

[0055] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. A method for controlling brittle and hard inclusions in 12Cr1MoVG steel. It is characterized in that The method comprises the following steps: S1: feeding the steelmaking raw material of 12Cr1MoVG steel into a converter, performing converter smelting, reaching the converter end point, obtaining molten steel and tapping, making the molten steel flow into a ladle and performing deoxidation and alloying to obtain outlet molten steel; S2: mixing the outgoing molten steel with high basicity slag-making material and performing LF high basicity slag white slag refining to obtain LF refined molten steel; S3: mixing the LF refined molten steel with a low-basicity reducing slag-making material and performing RH refining to obtain RH refined molten steel; S4: Utilizing the RH refined molten steel to carry out continuous casting steelmaking process to obtain 12Cr1MoVG steel.

2. The method for controlling brittle and hard inclusions in 12Cr1MoVG steel according to claim 1, in, At the end point of the converter, C in the molten steel is ≤ 0.06%.

3. The method for controlling brittle and hard inclusions in 12Cr1MoVG steel according to claim 1 or 2, in, At the end of the converter, the temperature of the molten steel is 1680°C-1730°C.

4. The method for controlling brittle and hard inclusions in 12Cr1MoVG steel according to claim 1, in, The steel tapping adopts a double slag blocking method, wherein a slide plate is used to block the slag in the early stage of steel tapping, and a slag blocking cone is used to block the slag in the late stage of steel tapping, and the slag amount is controlled to be ≤2kg / t molten steel.

5. The method for controlling brittle and hard inclusions in 12Cr1MoVG steel according to claim 1, in, The deoxidizing agent used for the deoxidation alloying is at least one of aluminum ingot, ferrosilicon, ferromanganese, ferrochrome and ferrovanadium.

6. The method for controlling brittle and hard inclusions in 12Cr1MoVG steel according to claim 1, in, The temperature for refining the LF high basicity slag is 1545-1555° C. and the time is 35-45 minutes.

7. The method for controlling brittle and hard inclusions in 12Cr1MoVG steel according to claim 1, in, The RH refining is performed at a temperature of 1570-1620° C. and a time of 20-30 min.

8. The method for controlling brittle and hard inclusions in 12Cr1MoVG steel according to claim 1, in, The low basicity reducing slag-making material is composed of the following raw materials in weight percentage: FeO+MnO≤1.0%, CaO is 30-45%, SiO 2 20-30%, Al 2 O 3 20-30%; MgO is 1-10%; 1.3≤R≤1.6, R=CaO% / SiO 2 %; the rest is MnO, P 2 O 5 、TiO 2 and impurities.

9. The method for controlling brittle and hard inclusions in 12Cr1MoVG steel according to any one of claims 1 to 8, in, Based on the total weight of all inclusions in the 12Cr1MoVG steel obtained in step S4, the proportion of plastic inclusions in the 12Cr1MoVG steel obtained in step S4 is more than 70%.

10. 12Cr1MoVG steel obtained by the method for controlling brittle and hard inclusions in 12Cr1MoVG steel according to any one of claims 1 to 9.