Method for increasing content of residual manganese in molten steel at smelting end point of low-phosphorus steel converter
By controlling the smelting mode and injecting materials in the low-phosphorus steel converter smelting, optimizing the oxygen lance design, the residual manganese content of the final molten steel is increased, solving the problem of low end-point manganese content in the production of low-phosphorus steel, reducing costs and improving efficiency. Steel quality.
Patent Information
- Application Number
- CN202410800588.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-15
AI Technical Summary
The residual manganese content of the final molten steel during the converter smelting process of low phosphorus steel is low, resulting in high alloying costs. The existing technical solutions are not suitable for the production of low phosphorus steel.
By controlling the amount of slag left in the converter smelting, selecting the appropriate smelting mode (single slag method or double slag method), injecting lime powder and oxygen, optimizing the design of the oxygen lance nozzle, adjusting the oxygen blowing amount and oxygen supply intensity, and adding raw white clouds Stone and iron ore form a low melting point calcium ferrite phase, which promotes the dephosphorization reaction and inhibits the demanganization reaction, thereby increasing the residual manganese content of the final molten steel.
It significantly increases the residual manganese content at the end of low-phosphorus steel converter smelting, reduces the consumption of slagging materials and the degree of peroxidation of molten steel, reduces production costs, and improves the quality stability of steel.
Smart Images

Figure BDA0004903262860000091 
Figure BDA0004903262860000101 
Figure BDA0004903262860000102
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of converter smelting, and more particularly to a method for increasing the residual manganese content of molten steel at the end point of converter smelting of low-phosphorus steel. Background Art
[0002] Manganese is one of the main alloying elements of steel, which can significantly improve the mechanical properties of steel. In the converter steelmaking process, the molten iron entering the furnace usually contains 0.2-0.35% manganese. During oxygen blowing smelting, most of the manganese is oxidized into the slag. The degree of oxidation is affected by many factors such as the temperature of the molten steel, the amount of slag, and the oxidizability of the slag. When tapping the steel, manganese alloy is added to the molten steel for alloying according to the residual manganese content. Therefore, the residual manganese content has an important influence on the amount of manganese alloy added and the production cost.
[0003] Low-phosphorus steel is one of the high-quality and high-quality steels. In order to ensure that the phosphorus content meets the composition control requirements of the steel, the degree of peroxidation of the molten steel is high during the converter smelting process, and the residual manganese content of the molten steel is low, usually in the range of 0.05-0.08%, which causes the amount of manganese alloy added in the subsequent alloying process and high production costs. Therefore, in the production process of low-phosphorus steel, increasing the residual manganese content of the molten steel at the end of converter smelting is of great significance to reducing production costs.
[0004] After searching, Chinese patent document (I) CN113106190 discloses "a steelmaking method for obtaining high manganese and low phosphorus molten steel by converter smelting". This method mainly adds manganese ore after adding molten iron / semi-steel into the converter, and uses inert gas stirring and adding carbonaceous reducing agent to promote the reduction reaction of manganese in the molten steel. Since MnO and P2O5 in the slag will be reduced at the same time during the reduction process, it is very easy to cause the phosphorus content in the molten steel to exceed the standard.
[0005] Chinese patent document (II) CN109112249 discloses "a converter smelting method for increasing the residual manganese in terminal molten steel with medium-high manganese molten iron". This method is mainly for medium-high manganese molten iron with a manganese content of 0.75-1.10%. The residual manganese content in the terminal molten steel is increased by adopting slag retention operation, low-basicity BaCO3-based slag making process, less slag smelting, and steel-making slag washing. Since the use of less slag smelting will reduce the phosphorus holding capacity of the slag, which is not conducive to dephosphorization, and slag washing will cause phosphorus regeneration, both of which are not conducive to low-phosphorus steel production, this solution is not suitable for the production of low-phosphorus steel.
[0006] For another example, Chinese patent document (III) CN105483314 discloses "a control method for increasing the residual manganese content at the end of the converter". This method is mainly aimed at producing HRB400 steel bars. The residual manganese content is increased by controlling the smelting gun position, slag amount, final slag total iron content, and final composition and temperature. This method is only applicable to HRB400 steel and has strict requirements on the silicon content in the molten iron.
[0007] Chinese Patent Document (IV) CN106148629 discloses “a method for controlling the final manganese content of high manganese molten iron”. This method realizes targeted control of the smelting of low alloy steel and high alloy steel by optimizing the smelting process parameters according to the different requirements of the finished steel for the manganese content, but does not involve the problem of increasing the residual manganese in low-phosphorus steel.
[0008] The favorable thermodynamic conditions for converter dephosphorization are: low temperature, high basicity, high oxidation and large slag volume, while the favorable thermodynamic conditions for manganese retention are: high temperature, high basicity, low oxidation and small slag volume. Although there are many opposite thermodynamic conditions for dephosphorization and manganese retention, the removal reaction mechanisms of the two are different. The reactions of dephosphorization and demanganese removal during converter smelting are as follows:
[0009] 2[P]+5(FeO)+3(CaO)=(3CaO.P2O5)+5Fe
[0010] [Mn] + (FeO) = (MnO) + [Fe]
[0011] According to the dephosphorization and demanganese reactions, demanganese is mainly related to the oxidizability of the slag. Although dephosphorization is also affected by the oxidizability of the slag, it must be carried out before the lime is fully dissolved. If the lime is not fully dissolved, the FeO in the slag will consume a large amount of Mn in the molten iron. If the lime is fully dissolved, the demanganese reaction can be inhibited by dephosphorization. Summary of the invention
[0012] 1. Problem to be solved
[0013] Aiming at the problems of low residual manganese content and high alloying cost in converter smelting of low-phosphorus steel in the prior art, the present invention provides a method for increasing the residual manganese content of molten steel at the end point of converter smelting of low-phosphorus steel.
[0014] 2. Technical solution
[0015] In order to solve the above problems, the technical solution adopted by the present invention is as follows:
[0016] The present invention provides a method for increasing the residual manganese content of molten steel at the end point of low-phosphorus steel converter smelting, comprising the following steps:
[0017] a. Preparation before blowing: After the last furnace is finished tapping, slag is left, and the amount of slag left is controlled to be 20-50kg / t steel, and then slag is splashed to solidify the slag;
[0018] b. Early stage of blowing: add scrap steel and molten iron into the converter, and select the smelting mode according to the silicon content (mass content) in the molten iron:
[0019] When Si≤0.45wt%, single slag method is used for smelting;
[0020] When Si>0.45wt%, double slag method is used for smelting;
[0021] During the blowing process, oxygen and lime powder are blown into the converter through an oxygen lance, and the total injection amount of lime powder is controlled to be 15-35kg / t. Raw dolomite and iron ore are added into the converter, and the addition amount of raw dolomite is controlled to be 10-20kg / t, and the addition amount of iron ore is controlled to be 10-25kg / t.
[0022] c. Mid-blowing period: when the oxygen blowing amount is 0-40% of the total oxygen amount, the oxygen supply intensity is controlled to be 3.5-4.5m 3 / min / t, bottom blowing oxygen supply intensity is 0.02-0.05m 3 / min / t, the oxygen lance height is 1.5-2m above the molten pool surface, the lime powder injection amount is 50-70% of the total amount, the raw dolomite addition amount is 30-50% of the total amount, and the oxygen content in the slag is 1.5-3.0m 3 / t;
[0023] When the oxygen blowing volume is 40-90% of the total oxygen volume, the oxygen supply intensity is controlled to be 3.0-3.5m 3 / min / t, bottom blowing oxygen supply intensity is 0.02-0.05m 3 / min / t, the oxygen lance height is 1.0-2.5m above the molten pool surface, the lime powder injection amount is 30-50% of the total amount, the raw dolomite addition amount is 50-70% of the total amount, and the oxygen content in the slag is 1.5-2.0m 3 / t;
[0024] When the oxygen blowing volume is more than 90% of the total oxygen volume, the oxygen supply intensity is controlled to 2.0-2.8m 3 / min / t, bottom blowing oxygen supply intensity is 0.08-0.15m 3 / min / t, the oxygen lance height is 0.9-1.2m above the molten pool surface, and the oxygen content in the slag is 1.0-1.5m 3 / t;
[0025] d. Late stage of blowing: When the oxygen blowing amount of the converter reaches 100%, an auxiliary gun is used for measurement. When the end point of the converter is reached, steel is tapped and slag is retained.
[0026] In the above technical solution, the purpose of leaving slag in step a is to form dephosphorization slag early, promote dephosphorization and inhibit demanganese removal.
[0027] In step b, when the silicon content is high, the purpose of using the double slag method is to prevent the slag from being too large and diluting the MnO in the slag, which is not conducive to increasing the residual manganese content; the purpose of using an oxygen lance to spray oxygen and lime powder is twofold, one is to utilize the high temperature at the position of the oxygen lance nozzle to promote the rapid melting of the lime powder, and the other is to spray the molten lime powder into the molten pool to accelerate the dephosphorization reaction and inhibit the oxidation of manganese.
[0028] In step c, the basicity of the slag in the early stage is gradually increased and the FeO in the slag is gradually reduced by spraying lime powder and furnace gas analysis, so as to promote the precipitation of dicalcium silicate particles in the slag, promote the dephosphorization reaction, and inhibit the demanganese reaction; when the oxygen blowing amount is 0-40% of the total oxygen amount, the purpose of using a high gun position and high intensity is to accelerate the oxidation of Fe in the early stage, increase the slag FeO, and preferentially dephosphorize at low temperature; when the oxygen blowing amount is more than 90% of the total oxygen amount, the purpose of using a low oxygen supply intensity and strong stirring is to prevent excessive oxidation of Fe in molten steel, increase the terminal carbon content, and promote manganese recovery.
[0029] Preferably, the components of the molten iron and the mass fraction of each component are: C: 4.0-5.1wt%, Si: 0.1-1.0wt%, P: 0.05-0.15wt%, Mn: 0.2-0.4wt%; the rest are iron and other inevitable impurities.
[0030] Preferably, in step b, lime powder and oxygen are sprayed into the furnace together from the central tube of the oxygen lance.
[0031] Preferably, the oxygen lance nozzle has 4 holes, the oxygen lance nozzle Mach number is 2.1-2.3, and the oxygen lance nozzle angle is 9-10°.
[0032] In the prior art, the Mach number of the oxygen lance nozzle is usually around 2.0, which affects the impact speed and depth. However, the present application can effectively increase the oxygen jet rate by increasing the oxygen lance Mach number, and at the same time optimize the angle of the oxygen lance nozzle, thereby increasing the impact depth, spraying lime powder into the molten pool, and optimizing the dephosphorization kinetic conditions.
[0033] Preferably, the size of the lime powder is ≤100um.
[0034] Preferably, the content of CaO in the lime powder is ≥85wt%.
[0035] Preferably, in the step b, the raw dolomite and the iron ore are added simultaneously, and the mass ratio of the dolomite to the iron ore is 0.8-1.2.
[0036] The purpose of adopting the above technical solution and adding raw dolomite and ore in proportion at the same time is to fully mix the two to form a low-melting-point calcium ferrite phase and promote slag formation.
[0037] Preferably, the bottom blowing gas is an inert gas.
[0038] Preferably, the bottom blowing gas is Ar.
[0039] Preferably, when the double slag method is used for smelting, the slag discharge point is controlled as follows: the oxygen blowing amount is 50-60% of the total oxygen blowing amount; the slag composition is controlled as follows: binary basicity: 2.2-2.8, MgO: 4-6wt%, FeO: 10-20wt%; the temperature is controlled as 1500-1580°C; and the slag discharge amount is controlled as 40-50%.
[0040] By adopting the above technical scheme, by increasing the pouring point temperature and the basicity, the reduction of manganese is promoted while ensuring that phosphorus does not return, and the slag with high phosphorus content and low manganese content is poured out.
[0041] Preferably, in step c, the oxygen content in the slag is the sum of the oxygen contents of FeO, MnO and P2O5 in the slag, and the oxygen content in the slag is obtained by a flue gas analysis system, which is calculated as follows:
[0042] dO 渣 =Q O2 +Q FeO -1 / 2Q CO -Q CO2 +21 / 79*Q N2
[0043] O 渣 =(∫(dOs)dt-Q Si ) / Wst
[0044] Among them, dO 渣 Represents the increment of oxygen content in slag per unit time, m 3 / min; Q O2 is the top blowing oxygen flow rate, m 3 / min; Q FeO is the oxygen content in the ore, m 3 / min; Q CO , Q CO2 and Q N2 are the measured CO, CO2 and N2 flow rates, m 3 / min; O 渣 is the oxygen content in the slag, m 3 / t; ∫(dOs) represents dO 渣 The integral over time represents the total increase in oxygen content in the slag from the beginning to the end of smelting; Q Si is the oxygen consumption for Si oxidation in molten iron, m 3 / t; Wst is the amount of molten steel, t.
[0045] Preferably, the final temperature of the converter is controlled at 1620-1680° C., the final carbon content is controlled at 0.1-0.15%, the final slag binary basicity is 3.0-5.0, and the MgO content in the slag is 7-9%.
[0046] 3. Beneficial effects
[0047] Compared with the prior art, the present invention has the following beneficial effects:
[0048] (1) The present invention selects different smelting processes and slag-forming paths for dephosphorization and manganese retention according to different molten iron compositions, and increases the slag-forming rate by injecting lime powder and oxygen through an oxygen lance. While achieving low-phosphorus steel production, the residual manganese content at the end of converter smelting is significantly increased, and the consumption of slag-forming materials such as lime powder and dolomite and the degree of peroxidation of molten steel are reduced, which not only improves the quality stability of steel, but also greatly reduces the production cost.
[0049] (2) The present invention designs a special oxygen lance nozzle to improve the stirring capacity of the molten pool, further optimizes the smelting process, and can greatly increase the residual manganese content of the molten steel at the end of smelting while ensuring that the phosphorus content of the low-phosphorus steel meets the requirements in advance, so that the residual manganese content is increased from 0.05-0.08% to more than 0.11%, significantly reducing the alloying cost.
[0050] (3) The present invention significantly reduces the degree of overoxidation of the final molten steel by optimizing the smelting process and equipment structure, which not only reduces the consumption of deoxidation alloy, but also avoids the formation of a large number of non-metallic inclusions in the subsequent deoxidation alloying process, thereby improving the stability of product quality. DETAILED DESCRIPTION
[0051] It should be noted that when a component is referred to as being "mounted" on another component, it may be directly on the other component or the two components may be directly integrated; when an component is referred to as being "connected" to another component, it may be directly connected to the other component or the two components may be directly integrated. At the same time, the terms such as "upper", "lower", "left", "right", "middle" and the like cited in this specification are only for the convenience of description, and are not used to limit the scope of implementation. Changes or adjustments in their relative relationships shall also be regarded as the scope of implementation of the present invention without substantially changing the technical content.
[0052] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs; the term "and / or" used herein includes any and all combinations of one or more of the associated listed items.
[0053] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0054] As used herein, the term "about" is used to provide flexibility and imprecision associated with a given term, measurement or value. The degree of flexibility for a particular variable can be easily determined by one skilled in the art.
[0055] As used herein, "adjacent" refers to the proximity of two structures or elements. Specifically, elements identified as "adjacent" can be adjacent or connected. Such elements can also be close to or in proximity to each other without necessarily touching each other. In some cases, the precise degree of proximity can depend on the specific context.
[0056] As used herein, the term "at least one of" is intended to be synonymous with "one or more of." For example, "at least one of A, B, and C" expressly includes only A, only B, only C, and combinations of each thereof.
[0057] Concentration, amount and other numerical data can be presented in range format herein.It should be understood that such range format is only used for convenience and simplicity, and should be flexibly interpreted as not only including the numerical value clearly described as range limit, but also including all single numerical values or sub-ranges contained in the range, just as each numerical value and sub-range are clearly described.For example, the numerical range of about 1 to about 4.5 should be interpreted as not only including the limit value of 1 to about 4.5 clearly described, but also including single numerals (such as 2,3,4) and sub-ranges (such as 1 to 3,2 to 4, etc.).The same principle is applicable to the scope of only narrating a numerical value, such as "less than about 4.5", which should be interpreted as including all the above-mentioned values and ranges.In addition, no matter how the breadth of the described range or feature is, this explanation should be applicable.
[0058] Any steps described in any method or process claim (for example, steps S1, S2, S3... or steps (1), (2), (3)... or steps 1), 2), 3)...) may be performed in any order and are not limited to the order presented in the claims.
[0059] Method+function or step+function limitations shall only be adopted if all of the following conditions are present in a particular claim limitation: a) "a method for..." or "a step for..." are explicitly recited; b) the corresponding function is explicitly recited. The structure, material, or action that supports the method+function is explicitly recited in the description herein. Therefore, the scope of the present invention should be determined solely by the appended claims and their legal equivalents, rather than by the description and examples given herein.
[0060] The present invention is further described below in conjunction with specific embodiments.
[0061] Example 1
[0062] This embodiment provides a method for increasing the residual manganese content of molten steel at the end of converter smelting of low-phosphorus steel. The experiment was conducted on a 150t converter. During the experiment, the number of oxygen lance nozzle holes was 4, the Mach number was 2.2, and the oxygen lance nozzle angle was 9°. The method specifically includes the following steps:
[0063] (a) Preparation before blowing: After the last furnace is finished tapping, the slag is left, and the amount of slag left is controlled to be 42kg / t steel. Then nitrogen is blown to splash the slag to fully solidify the slag;
[0064] (b) Early stage of blowing: adding scrap steel and molten iron into the converter, and according to the silicon content of the molten iron being 0.24% in Table 1, single slag method is adopted for smelting; during the blowing process, oxygen and lime powder are blown into the converter by an oxygen lance, the size of the lime powder is ≤100um, the content of CaO in the lime powder is ≥85wt%, and the total injection amount of the lime powder is controlled to be 18kg / t, and raw dolomite and iron ore are added into the converter, the raw dolomite and iron ore are added simultaneously, and the amount of raw dolomite added is controlled to be 17kg / t. The specific addition materials are shown in Tables 2 and 3.
[0065] (c) Mid-blowing: When the oxygen blowing amount is 0-40% of the total oxygen, the oxygen supply intensity is controlled to 4.1m 3 / min / t, bottom blowing oxygen supply intensity is 0.02m 3 / min / t, the oxygen lance height is 2.0m above the molten pool surface, the lime powder injection amount is 56% of the total amount, the raw dolomite addition amount is 30% of the total amount, and the oxygen content in the slag is 2.8m 3 / t; when the oxygen blowing amount is 40-90% of the total oxygen amount, the oxygen supply intensity is controlled to 3.1m 3 / min / t, bottom blowing oxygen supply intensity is 0.02m 3 / min / t, the oxygen lance height is 1.5m above the molten pool surface, the amount of lime powder injected is 44% of the total amount, the amount of raw dolomite added is 70% of the total amount, and the oxygen content in the slag is 1.8m 3 / t; when the oxygen blowing volume is more than 90% of the total oxygen volume, the oxygen supply intensity is controlled to 2.5m 3 / min / t, bottom blowing oxygen supply intensity is 0.1m 3 / min / t, the oxygen lance height is 0.9m above the molten pool surface, and the oxygen content in the slag is 1.2m 3 / t, see Table 2 for specific parameters.
[0066] (d) Late stage of blowing: When the oxygen blowing rate of the converter reaches 100%, an auxiliary gun is used for measurement. When the converter reaches the end point, steel is tapped and slag is retained. The specific smelting indicators are shown in Table 3.
[0067] Compared with the existing low-phosphorus steel production process, the advantages of Example 1 are mainly reflected in that the residual manganese content at the end of converter smelting is significantly improved while achieving low-phosphorus steel production, and the consumption of slag-making materials such as lime powder and dolomite and the degree of peroxidation of molten steel are reduced, which not only improves the quality stability of steel, but also greatly reduces the production cost. Compared with Comparative Example 1, the residual manganese content at the end of converter in Example 1 is increased from 0.07% to 0.15%, the total amount of lime powder added is reduced from 35kg / t steel to 18kg / t steel, a decrease of 48.6%, the total amount of dolomite added is reduced from 27kg / t steel to 17kg / t steel, a decrease of 37.1%, and the end carbon content is increased from 0.05% to 0.12%.
[0068] Example 2
[0069] This embodiment provides a method for increasing the residual manganese content of molten steel at the end of converter smelting of low-phosphorus steel. The experiment was conducted on a 150t converter. During the experiment, the number of oxygen lance nozzle holes was 4, the Mach number of the oxygen lance nozzle was 2.3, and the angle of the oxygen lance nozzle was 10°. The method specifically includes the following steps:
[0070] (a) Preparation before blowing: After the last furnace is finished tapping, the remaining slag is controlled to 35kg / t steel, and then nitrogen is blown to splash the slag to fully solidify the slag;
[0071] (b) Early stage of blowing: adding scrap steel and molten iron into the converter, and according to the silicon content of the molten iron being 0.42% in Table 1, single slag method is adopted for smelting; during the blowing process, oxygen and lime powder are blown into the converter by an oxygen lance, the size of the lime powder is ≤100um, the content of CaO in the lime powder is ≥85wt%, and the total injection amount of the lime powder is controlled to be 30kg / t, and raw dolomite and iron ore are added into the converter, the raw dolomite and iron ore are added simultaneously, and the amount of raw dolomite added is controlled to be 18kg / t. The specific addition materials are shown in Tables 2 and 3.
[0072] (c) Mid-blowing: When the oxygen blowing amount is 0-40% of the total oxygen, the oxygen supply intensity is controlled at 3.5m 3 / min / t, bottom blowing oxygen supply intensity is 0.03m 3 / min / t, the oxygen lance height is 1.5m above the molten pool surface, the lime powder injection amount is 68% of the total amount, the raw dolomite addition amount is 40% of the total amount, and the oxygen content in the slag is 2.6m 3 / t; when the oxygen blowing amount is 40-90% of the total oxygen amount, the oxygen supply intensity is controlled to 3.0m 3 / min / t, bottom blowing oxygen supply intensity is 0.03m 3 / min / t, the oxygen lance height is 2.1m above the molten pool surface, the lime powder injection amount is 32% of the total amount, the raw dolomite addition amount is 60% of the total amount, and the oxygen content in the slag is 1.6m 3 / t; when the oxygen blowing volume is more than 90% of the total oxygen volume, the oxygen supply intensity is controlled to 2.2m 3 / min / t, bottom blowing oxygen supply intensity is 0.15m 3 / min / t, the oxygen lance height is 1.0m above the molten pool surface, and the oxygen content in the slag is 1.1m 3 / t, see Table 2 for specific parameters.
[0073] (d) Late stage of blowing: When the oxygen blowing rate of the converter reaches 100%, an auxiliary gun is used for measurement. When the converter reaches the end point, steel is tapped and slag is retained. The specific smelting indicators are shown in Table 3.
[0074] Compared with the existing low-phosphorus steel production process, the advantages of Example 2 are mainly reflected in that the residual manganese content at the end of converter smelting is significantly improved while achieving low-phosphorus steel production, and the consumption of slag-making materials such as lime powder and dolomite and the degree of peroxidation of molten steel are reduced, which not only improves the quality stability of steel, but also greatly reduces the production cost. Compared with Comparative Example 1, the residual manganese content at the end of converter in Example 2 is increased from 0.07% to 0.14%, the total amount of lime powder added is reduced from 35kg / t steel to 30kg / t steel, a decrease of 14.3%, the total amount of dolomite added is reduced from 27kg / t steel to 18kg / t steel, a decrease of 33.3%, and the end carbon content is increased from 0.05% to 0.11%.
[0075] Example 3
[0076] This embodiment provides a method for increasing the residual manganese content of molten steel at the end point of converter smelting of low-phosphorus steel. The experiment was conducted on a 150t converter. During the experiment, the number of oxygen lance nozzle holes was 4, the Mach number of the oxygen lance nozzle was 2.3, and the angle of the oxygen lance nozzle was 9°. The method specifically includes the following steps:
[0077] (a) Preparation before blowing: After the last furnace is finished tapping, the slag is left, and the amount of slag left is controlled to be 32kg / t steel. Then nitrogen is blown to splash the slag to fully solidify the slag;
[0078] (b) Early stage of blowing: adding scrap steel and molten iron into the converter, and according to the silicon content of the molten iron being 0.48% in Table 1, the double slag method is adopted for smelting; during the blowing process, oxygen and lime powder are blown into the converter by an oxygen lance, the size of the lime powder is ≤100um, the content of CaO in the lime powder is ≥85wt%, and the total injection amount of the lime powder is controlled to be 19kg / t, and raw dolomite and iron ore are added into the converter, the raw dolomite and iron ore are added simultaneously, and the amount of raw dolomite added is controlled to be 15kg / t. The specific addition materials are shown in Tables 2 and 3.
[0079] (c) Mid-blowing: When the oxygen blowing amount is 0-40% of the total oxygen, the oxygen supply intensity is controlled at 4.5m 3 / min / t, bottom blowing oxygen supply intensity is 0.05m 3 / min / t, the oxygen lance height is 1.8m above the molten pool surface, the lime powder injection amount is 62% of the total amount, the raw dolomite addition amount is 42% of the total amount, and the oxygen content in the slag is 3.0m 3 / t; when the oxygen blowing amount is 40-90% of the total oxygen amount, the oxygen supply intensity is controlled to 3.5m 3 / min / t, bottom blowing oxygen supply intensity is 0.05m 3 / min / t, the oxygen lance height is 1.8m above the molten pool surface, the amount of lime powder injected is 38% of the total amount, the amount of raw dolomite added is 58% of the total amount, and the oxygen content in the slag is 2.0m 3 / t; when the oxygen blowing volume is more than 90% of the total oxygen volume, the oxygen supply intensity is controlled to 2.8m 3 / min / t, bottom blowing oxygen supply intensity is 0.12m 3 / min / t, the oxygen lance height is 1.1m above the molten pool surface, and the oxygen content in the slag is 1.5m 3 / t, see Table 2 for specific parameters.
[0080] The blowing is carried out until the oxygen blowing amount is 55% of the total oxygen blowing amount, the slag composition is controlled to be: binary basicity: 2.5, MgO: 5%, FeO: 15%, the temperature is 1540°C, and the slag discharge amount is controlled to be 52%.
[0081] (d) Late stage of blowing: When the oxygen blowing rate of the converter reaches 100%, an auxiliary gun is used for measurement. When the converter reaches the end point, steel is tapped and slag is retained. The specific smelting indicators are shown in Table 3.
[0082] Compared with the existing low-phosphorus steel production process, the advantages of Example 3 are mainly reflected in that the residual manganese content at the end of converter smelting is significantly improved while achieving low-phosphorus steel production, and the consumption of slag-making materials such as lime powder and dolomite and the degree of peroxidation of molten steel are reduced, which not only improves the quality stability of steel, but also greatly reduces the production cost. Compared with Comparative Example 2, the residual manganese content at the end of converter in Example 3 is increased from 0.08% to 0.13%, the total amount of lime powder added is reduced from 42kg / t steel to 19kg / t steel, a decrease of 54.8%, the total amount of dolomite added is reduced from 26kg / t steel to 15kg / t steel, a decrease of 42.3%, and the end carbon content is increased from 0.04% to 0.14%.
[0083] Example 4
[0084] This embodiment provides a method for increasing the residual manganese content of molten steel at the end of converter smelting of low-phosphorus steel. The experiment was conducted on a 150t converter. During the experiment, the number of oxygen lance nozzle holes was 4, the Mach number of the oxygen lance nozzle was 2.3, and the angle of the oxygen lance nozzle was 10°. The method specifically includes the following steps:
[0085] (a) Preparation before blowing: After the last furnace is finished tapping, the remaining slag is controlled to 30kg / t steel, and then nitrogen is blown to splash the slag to fully solidify the slag;
[0086] (b) Early stage of blowing: adding scrap steel and molten iron into the converter, and according to the silicon content of the molten iron being 0.74% in Table 1, the double slag method is adopted for smelting; during the blowing process, oxygen and lime powder are blown into the converter by an oxygen lance, the size of the lime powder is ≤100um, the content of CaO in the lime powder is ≥85wt%, and the total injection amount of the lime powder is controlled to be 31kg / t, and raw dolomite and iron ore are added into the converter, the raw dolomite and iron ore are added simultaneously, and the amount of raw dolomite added is controlled to be 20kg / t. The specific addition materials are shown in Tables 2 and 3.
[0087] (c) Mid-blowing: When the oxygen blowing amount is 0-40% of the total oxygen, the oxygen supply intensity is controlled to 3.8m 3 / min / t, bottom blowing oxygen supply intensity is 0.03m 3 / min / t, the oxygen lance height is 1.7m above the molten pool surface, the lime powder injection amount is 50% of the total amount, the raw dolomite addition amount is 47% of the total amount, and the oxygen content in the slag is 1.8m 3 / t; when the oxygen blowing amount is 40-90% of the total oxygen amount, the oxygen supply intensity is controlled to 3.2m 3 / min / t, bottom blowing oxygen supply intensity is 0.03m 3 / min / t, the oxygen lance height is 1.9m above the molten pool surface, the lime powder injection amount is 50% of the total amount, the raw dolomite addition amount is 53% of the total amount, and the oxygen content in the slag is 1.5m 3 / t; when the oxygen blowing volume is more than 90% of the total oxygen volume, the oxygen supply intensity is controlled to 2.5m 3 / min / t, bottom blowing oxygen supply intensity is 0.08m 3 / min / t, the oxygen lance height is 1.0m above the molten pool surface, and the oxygen content in the slag is 1.2m 3 / t, see Table 2 for specific parameters.
[0088] The blowing is carried out until the oxygen blowing amount is 57% of the total oxygen blowing amount, the slag composition is controlled to be: binary basicity: 2.2, MgO: 4wt%, FeO: 13wt%, the temperature is 1551°C, and the slag discharge amount is controlled to be 57%.
[0089] (d) Late stage of blowing: When the oxygen blowing rate of the converter reaches 100%, an auxiliary gun is used for measurement. When the converter reaches the end point, steel is tapped and slag is retained. The specific smelting indicators are shown in Table 3.
[0090] Compared with the existing low-phosphorus steel production process, the advantages of Example 4 are mainly reflected in that the residual manganese content at the end of converter smelting is significantly improved while achieving low-phosphorus steel production, and the consumption of slag-making materials such as lime powder and dolomite and the degree of peroxidation of molten steel are reduced, which not only improves the quality stability of steel, but also greatly reduces the production cost. Compared with Comparative Example 2, the residual manganese content at the end of converter in Example 4 is increased from 0.08wt% to 0.12wt%, the total amount of lime powder added is reduced from 42kg / t steel to 31kg / t steel, a decrease of 26.2%, the total amount of dolomite added is reduced from 26kg / t steel to 20kg / t steel, a decrease of 23.1%, and the end carbon content is increased from 0.04wt% to 0.10wt%.
[0091] Comparative Example 1
[0092] This comparative example provides a method for improving the converter smelting of low-phosphorus steel. After the last furnace is tapped, slag is left, and the amount of slag left is controlled to be 40kg / t steel. Then nitrogen is blown to splash the slag to fully solidify the slag. Scrap steel is added to the converter and molten iron is added. During the blowing process, the top blowing oxygen supply intensity is controlled to be 3.0m 3 / min / t, bottom blowing intensity is 0.05m 3 / min / t. When the oxygen blowing amount is 0-40% of the total oxygen, all lime is added, the amount of raw dolomite added is 65% of the total amount, and lime, ore and dolomite are added together; when the oxygen blowing amount is 40-90% of the total oxygen, the amount of raw dolomite added is 18% of the total amount; when the oxygen blowing amount is more than 90% of the total oxygen, the amount of raw dolomite added is 17% of the total amount, and ore and dolomite are added together. The specific parameters are shown in Table 2. When the oxygen blowing amount of the converter reaches 100%, the auxiliary gun is used for measurement. When the converter reaches the end point, the steel is tapped and the slag is left. The specific smelting indicators are shown in Table 3.
[0093] Comparative Example 2
[0094] This comparative example provides a method for improving the converter smelting of low-phosphorus steel. After the last furnace is tapped, slag is left, and the amount of slag left is controlled to be 45kg / t steel. Then nitrogen is blown to splash the slag to fully solidify the slag. Scrap steel is added to the converter and molten iron is added. During the blowing process, the top blowing oxygen supply intensity is controlled to be 3.2m 3 / min / t, bottom blowing intensity is 0.08m 3 / min / t. When the oxygen blowing amount is 0-40% of the total oxygen amount, all the lime is added, the amount of raw dolomite added is 70% of the total amount, and the lime, ore and dolomite are added together; when the oxygen blowing amount is 40-90% of the total oxygen amount, the amount of raw dolomite added is 15% of the total amount, and the ore and dolomite are added together; when the oxygen blowing amount is more than 90% of the total oxygen amount, the amount of raw dolomite added is 15% of the total amount, and the ore and dolomite are added together. The specific parameters are shown in Table 2. When the oxygen blowing amount of the converter reaches 100%, the auxiliary gun is used for measurement. When the converter reaches the end point, the steel is tapped and the slag is retained. The specific smelting indicators are shown in Table 3.
[0095] Table 1 Metal material conditions and process of converter smelting
[0096]
[0097] Table 2 Process parameters of converter blowing process
[0098]
[0099] Table 3 Converter smelting index
[0100]
[0101]
[0102] The above content is a schematic description of the present invention and its implementation methods, which is not restrictive. What is shown in the embodiment is only one of the implementation methods of the present invention, and the actual implementation method is not limited thereto. Therefore, if a person of ordinary skill in the art is inspired by it and designs implementation methods and embodiments similar to the technical solution without creative design without departing from the purpose of the invention, they should all fall within the scope of protection of the present invention.
Claims
1. A method for increasing the residual manganese content in molten steel at the end of converter smelting of low-phosphorus steel, characterized in that: The following steps are involved: a. Preparation before blowing: After the last furnace is finished tapping, slag is left, and the amount of slag left is controlled to be 20-50kg / t steel, and then slag is splashed to solidify the slag; b. Early stage of blowing: add scrap steel and molten iron into the converter, and select the smelting mode according to the silicon content in the molten iron: When Si≤0.45wt%, single slag method is used for smelting; When Si>0.45wt%, double slag method is used for smelting; During the blowing process, oxygen and lime powder are blown into the converter through an oxygen lance, and the total injection amount of lime powder is controlled to be 15-35kg / t. Raw dolomite and iron ore are added into the converter, and the addition amount of raw dolomite is controlled to be 10-20kg / t, and the addition amount of iron ore is controlled to be 10-25kg / t. c. Mid-blowing period: when the oxygen blowing amount is 0-40% of the total oxygen amount, the oxygen supply intensity is controlled to be 3.5-4.5m3 / min / t, the bottom blowing oxygen supply intensity is 0.02-0.05m3 / min / t, the oxygen lance height is 1.5-2m above the molten pool liquid level, the lime powder injection amount is 50-70% of the total amount, the raw dolomite addition amount is 30-50% of the total amount, and the oxygen content in the slag is 1.5-3.0m 3 / t; When the oxygen blowing volume is 40-90% of the total oxygen volume, the oxygen supply intensity is controlled to be 3.0-3.5m 3 / min / t, bottom blowing oxygen supply intensity is 0.02-0.05m 3 / min / t, the oxygen lance height is 1.0-2.5m above the molten pool surface, the lime powder injection amount is 30-50% of the total amount, the raw dolomite addition amount is 50-70% of the total amount, and the oxygen content in the slag is 1.5-2.0m 3 / t; When the oxygen blowing volume is more than 90% of the total oxygen volume, the oxygen supply intensity is controlled to 2.0-2.8m 3 / min / t, bottom blowing oxygen supply intensity is 0.08-0.15m 3 / min / t, the oxygen lance height is 0.9-1.2m above the molten pool surface, and the oxygen content in the slag is 1.0-1.5m 3 / t; d. Late stage of blowing: When the oxygen blowing amount of the converter reaches 100%, an auxiliary gun is used for measurement. When the end point of the converter is reached, steel is tapped and slag is retained.
2. The method for increasing the residual manganese content in molten steel at the end point of low-phosphorus steel converter smelting according to claim 1, characterized in that: In the step b, the components of the molten iron and the mass fraction of each component are: C: 4.0-5.1wt%, Si: 0.1-1.0wt%, P: 0.05-0.15wt%, Mn: 0.2-0.4wt%; the rest are iron and other inevitable impurities.
3. The method for increasing the residual manganese content in molten steel at the end point of low-phosphorus steel converter smelting according to claim 2, characterized in that: The oxygen lance nozzle has 4 holes, the oxygen lance nozzle Mach number is 2.1-2.3, and the oxygen lance nozzle angle is 9-10°.
4. The method for increasing the residual manganese content in molten steel at the end point of low-phosphorus steel converter smelting according to claim 3, characterized in that: The size of the lime powder is ≤100um.
5. The method for increasing the residual manganese content in molten steel at the end point of converter smelting of low-phosphorus steel according to claim 4, characterized in that: The content of CaO in the lime powder is ≥85wt%.
6. The method for increasing the residual manganese content in molten steel at the end point of converter smelting of low-phosphorus steel according to claim 5, characterized in that: In the step b, the raw dolomite and the iron ore are added simultaneously, and the mass ratio of the dolomite to the iron ore is 0.8-1.
2.
7. The method for increasing the residual manganese content in molten steel at the end point of low-phosphorus steel converter smelting according to claim 6, characterized in that: The bottom blowing gas is an inert gas.
8. The method for increasing the residual manganese content in molten steel at the end point of converter smelting of low-phosphorus steel according to claim 7, characterized in that: When the double slag method is used for smelting, the slag discharge point is controlled as follows: the oxygen blowing amount is 50-60% of the total oxygen blowing amount; the slag composition is controlled as follows: binary basicity: 2.2-2.8, MgO: 4-6wt%, FeO: 10-20wt%; the temperature is controlled as 1500-1580°C; and the slag discharge amount is controlled as 40-60%.
9. The method for increasing the residual manganese content in molten steel at the end point of converter smelting of low-phosphorus steel according to any one of claims 1 to 8, characterized in that: In the step c, the oxygen content in the slag is the sum of the oxygen contents of FeO, MnO and P2O5 in the slag. The oxygen content in the slag is obtained by a flue gas analysis system and is calculated as follows: dO 渣 =Q O2 +Q FeO -1 / 2Q CO -Q CO2 +21 / 79*Q N2 ABOUT 渣 =(∫(dOs)dt-Q Si ) / In Among them, dO 渣 Represents the increment of oxygen content in slag per unit time, m 3 / min; Q O2 is the top blowing oxygen flow rate, m 3 / min; Q FeO is the oxygen content in the ore, m 3 / min; Q CO , Q CO2 and Q N2 are the measured CO, CO2 and N2 flow rates, m 3 / min; O 渣 is the oxygen content in the slag, m 3 / t; ∫(dOs) represents dO 渣 The integral over time represents the total increase in oxygen content in the slag from the beginning to the end of smelting; Q Si is the oxygen consumption for Si oxidation in molten iron, m 3 / t; Wst is the amount of molten steel, t.
10. The method for increasing the residual manganese content in molten steel at the end point of converter smelting of low-phosphorus steel according to claim 9, characterized in that: The final converter temperature is controlled at 1620-1680°C, the final carbon content is controlled at 0.1-0.15%, the final slag binary basicity is 3.0-5.0, and the MgO content in the slag is 7-9%.